Method for preparing adsorbent from sludge in wastewater of purification plant
Through pretreatment and carbonization of wastewater sludge in purification plants, combined with activator and magnetic zeolite microwave combined technology, an efficient carbon-based adsorbent was prepared, which solved the problems of high sludge treatment cost and insufficient removal capacity, and achieved low Cost-effective wastewater treatment and sludge resource utilization.
Patent Information
- Application Number
- CN202410895671.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-08
AI Technical Summary
Existing wastewater sludge treatment methods in purification plants are costly and easy to cause secondary pollution to the environment, and are difficult to effectively remove heavy metal ions and pigments.
By collecting the sludge in the wastewater of the purification plant for pretreatment, mixing diatomaceous earth and carbonizing it, and then mixing it with an activator for activation reaction to form a carbon-based adsorbent with high specific surface area and rich pore structure, using magnetic zeolite and microwave Combined treatment improves the dewatering performance of sludge.
The low-cost utilization of sludge resources is achieved, the wastewater treatment efficiency is improved, the preparation cost is low, and the obtained adsorbent has good industrial application prospects and efficient removal capabilities.
Smart Images

Figure CN118743979A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental protection and wastewater treatment, and relates to a method for preparing an adsorbent from sludge in wastewater from a purification plant. Background Art
[0002] With the acceleration of industrialization and urbanization, the problem of wastewater sludge treatment in water treatment plants has become increasingly prominent, causing serious impacts on the environment and human health. At present, the main methods for treating sludge include landfilling and incineration, which not only have high treatment costs, but also easily cause secondary pollution to the environment. In recent years, the method of preparing adsorbents using sludge has gradually attracted attention. This method can not only realize the resource utilization of sludge, but also can be used to remove heavy metal ions and pigments in wastewater, and has broad application prospects. Summary of the invention
[0003] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0004] Still another object of the present invention is to provide a method for preparing adsorbent from sludge in wastewater from a purification plant.
[0005] To this end, the technical solution provided by the present invention is:
[0006] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0007] Step 1: collecting sludge generated by a water treatment plant, pre-treating the sludge to obtain a dried sludge raw material, wherein the moisture content of the dried sludge raw material is less than 10%;
[0008] Step 2: crushing the sludge raw material into sludge particles with a particle size of 0.5 to 2 mm, then mixing the sludge particles with diatomaceous earth, and carbonizing them at a temperature of 600 to 700° C. for 20 to 70 minutes to form a porous carbon-based material, wherein the mass ratio of diatomaceous earth to the sludge particles is 1:10 to 20. During the carbonization, an inert gas is introduced at a flow rate of 0.5 to 1.0 L / min, and the temperature is gradually increased to 600 to 700° C. at a rate of 10 to 15° C. / min;
[0009] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:2 to 4, then put the mixed materials into an activation furnace, and perform an activation reaction at a temperature of 700-800° C. for 60-120 min;
[0010] Step 4: Wash and dry the activated material, and then grind and screen to obtain 200-250 mesh particles as an adsorbent.
[0011] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, in step 1, the method for pretreating the sludge in the wastewater comprises:
[0012] The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 6-8.
[0013] Then, magnetic zeolite is added thereto, mixed, and stirred and mixed again every 25 to 35 minutes. After adsorption for 8 to 10 hours, the magnetic zeolite is recovered, wherein the mass ratio of the magnetic zeolite to the sludge is 1:20 to 40.
[0014] Then, the sludge is irradiated with microwaves at a frequency of 2000 to 2500 MHZ and a power of 500 to 1000 W for 30 to 80 seconds.
[0015] Then dehydration is carried out to obtain dry sludge raw material.
[0016] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, in step 2, the sludge raw material is crushed and processed into sludge particles with a particle size of 0.5 to 2 mm, and then the sludge particles are mixed with diatomaceous earth and carbonized at a temperature of 650°C for 45 minutes to form a carbon-based material with a porous structure, and the mass ratio of diatomaceous earth to the sludge particles is 1:15. During the carbonization, an inert gas is introduced at a flow rate of 0.8 L / min, and the temperature is gradually increased to 650°C at a rate of 12°C / min.
[0017] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, in step 4, the method for washing the activated material is: repeatedly washing the activated material with a hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4-5.
[0018] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, in step 4, the method for drying the activated material is: drying the cleaned material at 103-105° C. to constant weight.
[0019] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, in step three, the activator is ZnCl2 or KOH or a composite solution of zinc chloride and sulfuric acid in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are both 5 mol / L.
[0020] Preferably, in the method for preparing an adsorbent from sludge in wastewater from a purification plant, the inert gas is nitrogen or a rare gas.
[0021] The present invention has at least the following beneficial effects:
[0022] In the present invention, sludge particles are mixed with diatomite, and carbonization treatment is carried out at a temperature of 600-700°C for 20-70 minutes, and the first pyrolysis is carried out to form a carbon-based material with a porous structure. Diatomite can not only absorb water, but also, because of its special porous structure, it acts as a carrier of sludge particles to improve the porosity of the formed carbon-based material. After that, the activator and the carbon-based material are evenly mixed in a mass ratio of 1:2-4, and then the mixed material is placed in an activation furnace, and an activation reaction is carried out at a temperature of 700-800°C, and the activation time is 60-120 minutes. The second pyrolysis is carried out, and the activator and the carbon-based material react chemically to form a richer pore structure.
[0023] Through the preparation method of the present invention, a high specific surface area (> 2000m 2 / g), and an adsorbent with rich pore structure. The present invention makes full use of biomass resources in sludge, reduces the cost of adsorbent, improves wastewater treatment efficiency, has low preparation cost, simple operation, and good industrial application prospects.
[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is a flow chart of a method for preparing an adsorbent from sludge in wastewater from a water treatment plant. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0027] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0028] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.
[0029] like Figure 1 As shown, the present invention provides a method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0030] Step 1: collecting sludge generated by a water treatment plant, pre-treating the sludge to obtain a dried sludge raw material, wherein the moisture content of the dried sludge raw material is less than 10%;
[0031] Step 2: crushing the sludge raw material into sludge particles with a particle size of 0.5 to 2 mm, then mixing the sludge particles with diatomaceous earth, and carbonizing them at a temperature of 600 to 700° C. for 20 to 70 minutes to form a porous carbon-based material, wherein the mass ratio of diatomaceous earth to the sludge particles is 1:10 to 20. During the carbonization, an inert gas is introduced at a flow rate of 0.5 to 1.0 L / min, and the temperature is gradually increased to 600 to 700° C. at a rate of 10 to 15° C. / min;
[0032] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:2 to 4, then put the mixed materials into an activation furnace, and perform an activation reaction at a temperature of 700-800° C. for 60-120 min;
[0033] Step 4: Wash and dry the activated material, and then grind and screen to obtain 200-250 mesh particles as an adsorbent.
[0034] In the present invention, sludge particles are mixed with diatomaceous earth, and carbonization treatment is carried out at a temperature of 600-700°C for 20-70 minutes, and the first pyrolysis is carried out to form a porous carbon-based material. Diatomaceous earth can not only absorb water, but also because of its special porous structure, it acts as a carrier of sludge particles to improve the porosity of the formed carbon-based material. After that, the activator and the carbon-based material are evenly mixed in a mass ratio of 1:2-4, and then the mixed material is placed in an activation furnace, and an activation reaction is carried out at a temperature of 700-800°C, and the activation time is 60-120 minutes. The second pyrolysis is carried out, and the activator and the carbonaceous material react chemically to form a richer pore structure.
[0035] Through the preparation method of the present invention, a high specific surface area (> 2000m 2 / g), and an adsorbent with rich pore structure. The present invention makes full use of biomass resources in sludge, reduces the cost of adsorbent, improves wastewater treatment efficiency, has low preparation cost, simple operation, and good industrial application prospects.
[0036] In one embodiment of the present invention, preferably, in step 1, the method for pre-treating sludge in wastewater comprises:
[0037] The crushed biomass material is added into the sludge after preliminary treatment and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 6-8. The biomass material is preferably wheat or corn straw.
[0038] Then add magnetic zeolite, mix well, stir and mix again every 25-35 minutes, and after adsorption for 8-10 hours, recover the magnetic zeolite, wherein the mass ratio of the magnetic zeolite to the sludge is 1:20-40. After the adsorption is completed, the magnetic zeolite that adsorbs pollutants can be quickly separated from the environment by applying an external magnetic field, so that it can be recycled.
[0039] The sludge is then irradiated with microwaves at a frequency of 2000-2500 MHZ and a power of 500-1000 W for 30-80 seconds.
[0040] Then dehydration is carried out to obtain dry sludge raw material.
[0041] The present invention can destroy the aggregation state of sludge and adsorb harmful substances therein by adding magnetic zeolite and using microwaves in combination, so that the moisture in the sludge is easy to remove, the dehydration performance of the sludge is improved, and the later carbonization and activation treatment are convenient.
[0042] In one embodiment of the present invention, preferably, in step 2, the sludge raw material is crushed and processed into sludge particles with a particle size of 0.5 to 2 mm, and then the sludge particles are mixed with diatomaceous earth and carbonized at a temperature of 650°C for 45 minutes to form a porous carbon-based material, and the mass ratio of diatomaceous earth to the sludge particles is 1:15. During the carbonization, an inert gas is introduced at a flow rate of 0.8 L / min, and the temperature is gradually increased to 650°C at a rate of 12 / min.
[0043] In one embodiment of the present invention, preferably, in step 4, the method for cleaning the activated material is: repeatedly washing the activated material with hydrochloric acid solution and deionized water at a temperature of 70° C. until the pH value of the tail water reaches 4-5.
[0044] In one embodiment of the present invention, preferably, in step 4, the method for drying the activated material is: drying the cleaned material at 103-105° C. to constant weight.
[0045] In one embodiment of the present invention, preferably, in step three, the activator is ZnCl2 or KOH or a composite solution of zinc chloride and sulfuric acid in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are both 5mol / L. Potassium hydroxide plays a role of swelling when activating sludge, which helps the sludge to form more pore structures during the pyrolysis process. The activated sludge carbon has a larger specific surface area after its activation, which significantly improves the adsorption performance of the sludge. Zinc chloride not only helps the swelling of sludge, but also helps the sludge to remove the side chains and oxygen-containing functional groups of the structural units through polycondensation reaction or cross-linking reaction during the pyrolysis process, further increasing the specific surface area. The sludge activated carbon activated by zinc chloride performs well in removing hydrogen sulfide gas, and its adsorption effect exceeds that of traditional activated carbon. The strong acidity of sulfuric acid can promote the decomposition of organic matter in sludge, thereby forming more pores during the pyrolysis process. It is low in cost and suitable for large-scale application. The synergistic effect of zinc chloride and sulfuric acid not only improves the adsorption performance of the adsorbent, but also reduces the cost.
[0046] In one embodiment of the present invention, preferably, the inert gas is nitrogen or a rare gas.
[0047] In order to enable those skilled in the art to better understand the technical solution of the present invention, the following embodiments are provided for illustration:
[0048] Example 1
[0049] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0050] Step 1: Collect sludge generated by a water treatment plant, pre-treat the sludge, and obtain a dry sludge raw material, wherein the moisture content of the dry sludge raw material is less than 10%; the method for pre-treating sludge in wastewater includes:
[0051] The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 7.
[0052] Then, magnetic zeolite is added thereto, mixed, and stirred and mixed again every 30 minutes. After adsorption for 9 hours, the magnetic zeolite is recovered, wherein the mass ratio of the magnetic zeolite to the sludge is 1:30.
[0053] The sludge was then irradiated with microwaves at a frequency of 2250 MHZ and a power of 750 W for 55 seconds.
[0054] Then dehydration is carried out to obtain dry sludge raw material.
[0055] Step 2: crush the sludge raw material into sludge particles with a particle size of 1 mm, then mix the sludge particles with diatomaceous earth, and carbonize them at a temperature of 650°C for 45 minutes to form a porous carbon-based material. The mass ratio of diatomaceous earth to the sludge particles is 1:15. During the carbonization, inert gas is introduced at a flow rate of 0.8 L / min, and the temperature is gradually increased to 650°C at a rate of 12°C / min.
[0056] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:3, then put the mixed materials into an activation furnace, and carry out an activation reaction at a temperature of 750°C for 90 minutes; the activator is a composite solution of zinc chloride and sulfuric acid in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are both 5 mol / L.
[0057] Step 4: Wash and dry the activated material, and then grind and screen to obtain 220 mesh particles as an adsorbent. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4.5. The method for drying the activated material is: dry the washed material at 104°C to constant weight.
[0058] Example 2
[0059] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0060] Step 1: Collect sludge generated by a water treatment plant, pre-treat the sludge, and obtain a dry sludge raw material, wherein the moisture content of the dry sludge raw material is less than 10%; the method for pre-treating sludge in wastewater includes:
[0061] The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 6.
[0062] Then, magnetic zeolite is added thereto, mixed, and stirred and mixed again every 25 minutes. After adsorption for 8 hours, the magnetic zeolite is recovered, wherein the mass ratio of the magnetic zeolite to the sludge is 1:20.
[0063] Then, the sludge is irradiated with microwaves at a frequency of 2000 MHZ and a power of 500 W for 80 seconds.
[0064] Then dehydration is carried out to obtain dry sludge raw material.
[0065] Step 2: crush the sludge raw material into sludge particles with a particle size of 0.5 mm, then mix the sludge particles with diatomaceous earth, and carbonize them at a temperature of 600°C for 70 minutes to form a porous carbon-based material, wherein the mass ratio of diatomaceous earth to the sludge particles is 1:10. During the carbonization, an inert gas is introduced at a flow rate of 0.5 L / min, and the temperature is gradually increased to 600°C at a rate of 10°C / min; crush the sludge raw material into sludge particles with a particle size of 0.5 mm, then mix the sludge particles with diatomaceous earth, and carbonize them at a temperature of 650°C for 45 minutes to form a porous carbon-based material, wherein the mass ratio of diatomaceous earth to the sludge particles is 1:15.
[0066] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:2, then put the mixed materials into an activation furnace, and perform an activation reaction at a temperature of 700° C. for 120 minutes; the activator is KOH.
[0067] Step 4: Wash and dry the activated material, and then grind and screen to obtain 200 mesh particles as an adsorbent. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4. The method for drying the activated material is: dry the washed material at 103°C to constant weight.
[0068] Example 3
[0069] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0070] Step 1: Collect sludge generated by a water treatment plant, pre-treat the sludge, and obtain a dry sludge raw material, wherein the moisture content of the dry sludge raw material is less than 10%; the method for pre-treating sludge in wastewater includes:
[0071] The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 8.
[0072] Then, magnetic zeolite was added thereto, mixed, and stirred again every 35 minutes. After adsorption for 10 hours, the magnetic zeolite was recovered, wherein the mass ratio of the magnetic zeolite to the sludge was 1:40.
[0073] Then, the sludge is irradiated with microwaves at a frequency of 2500 MHZ and a power of 1000 W for 30 seconds.
[0074] Then dehydration is carried out to obtain dry sludge raw material.
[0075] Step 2: crush the sludge raw material into sludge particles with a particle size of 2 mm, then mix the sludge particles with diatomaceous earth, and carbonize them at a temperature of 700°C for 20 minutes to form a porous carbon-based material, the mass ratio of diatomaceous earth to the sludge particles is 1:20, and during carbonization, an inert gas is introduced at a flow rate of 1.0L / min, and the temperature is gradually increased to 700°C at a rate of 15°C / min; crush the sludge raw material into sludge particles with a particle size of 2 mm, then mix the sludge particles with diatomaceous earth, and carbonize them at a temperature of 650°C for 45 minutes to form a porous carbon-based material, the mass ratio of diatomaceous earth to the sludge particles is 1:15. The inert gas is nitrogen.
[0076] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:4, then put the mixed materials into an activation furnace, and perform an activation reaction at a temperature of 780°C for 120 minutes; the activator is ZnCl2.
[0077] Step 4: Wash and dry the activated material, and then grind and screen to obtain 250 mesh particles as an adsorbent. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4-5. The method for drying the activated material is: dry the washed material at 105°C to constant weight.
[0078] Comparative Example 1
[0079] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0080] Step 1: Collect the sludge generated by the water treatment plant, pre-treat the sludge to obtain dry sludge raw material; dehydrate it through a centrifuge, and then dry it in a drying oven at 60°C to obtain dry sludge; the water content of the dry sludge is about 15%.
[0081] Step 2: crush the sludge raw material into sludge particles with a particle size of 1 mm, and then carbonize the sludge particles at a temperature of 650° C. for 45 minutes to form a carbon-based material.
[0082] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:3, then put the mixed materials into an activation furnace, and carry out an activation reaction at a temperature of 750°C for 90 minutes; the activator is a composite solution of zinc chloride solution and sulfuric acid solution in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are 5 mol / L respectively.
[0083] Step 4: Wash and dry the activated material, and then grind and screen to obtain 220 mesh particles as an adsorbent. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4.5. The method for drying the activated material is: dry the washed material at 104°C to constant weight.
[0084] Comparative Example 2
[0085] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0086] Step 1: Collect the sludge generated by the water treatment plant, pre-treat the sludge, dehydrate it through a centrifuge, and then dry it in a drying oven at 60°C to obtain dry sludge; the water content in the dry sludge is about 15%.
[0087] Step 2: crush the sludge raw material into sludge particles with a particle size of 1 mm, and then carbonize the sludge particles at a temperature of 650° C. for 45 minutes to form a carbon-based material.
[0088] Step 3: reacting the carbon-based material at a temperature of 750° C. for 90 minutes.
[0089] Step 4: Wash and dry the activated material, and then grind and screen to obtain 220 mesh particles as an adsorbent. The activator is a 5 mol / L sulfuric acid solution. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4.5. The method for drying the activated material is: dry the washed material at 104°C to constant weight.
[0090] Comparative Example 3
[0091] A method for preparing an adsorbent from sludge in wastewater from a purification plant, comprising:
[0092] Step 1: Collect sludge generated by a water treatment plant, pre-treat the sludge, and obtain a dry sludge raw material, wherein the moisture content of the dry sludge raw material is less than 10%; the method for pre-treating sludge in wastewater includes:
[0093] The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 7.
[0094] Then, magnetic zeolite is added thereto, mixed, and stirred and mixed again every 30 minutes. After adsorption for 9 hours, the magnetic zeolite is recovered, wherein the mass ratio of the magnetic zeolite to the sludge is 1:30.
[0095] The sludge was then irradiated with microwaves at a frequency of 2250 MHZ and a power of 750 W for 55 seconds.
[0096] Then dehydration is carried out to obtain dry sludge raw material.
[0097] Step 2: crush the sludge raw material into sludge particles with a particle size of 1 mm, and then carbonize the sludge particles at a temperature of 650° C. for 45 minutes to form a carbon-based material.
[0098] Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:3, then put the mixed materials into an activation furnace, and carry out an activation reaction at a temperature of 750°C for 90 minutes; the activator is a composite solution of zinc chloride and sulfuric acid in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are both 5 mol / L.
[0099] Step 4: Wash and dry the activated material, and then grind and screen to obtain 220 mesh particles as an adsorbent. The method for washing the activated material is: repeatedly wash the activated material with hydrochloric acid solution and deionized water at a temperature of 70°C until the pH value of the tail water reaches 4.5. The method for drying the activated material is: dry the washed material at 104°C to constant weight.
[0100] Effect and verification
[0101] The specific surface areas of the adsorbents prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were measured, as shown in Table 1 below:
[0102] Table 1 Specific surface area of adsorbent
[0103] Group <![CDATA[Specific surface area (m 2 / g)]]> Example 1 2603 Example 2 2557 Example 3 2580 Comparative Example 1 997 Comparative Example 2 837 Comparative Example 3 1368
[0104] It can be seen that the addition of diatomite has a great influence on the specific surface area of the finally prepared adsorbent. The specific surface area of the adsorbent prepared in Comparative Example 3 without the addition of diatomite is much lower than that in Example 1. It can also be seen from Comparative Examples 1 and 3 that the dehydration treatment of sewage cement and the treatment of the dehydration degree also have a great influence on the specific surface area of the adsorbent. It can also be seen from Comparative Example 2 that the addition of the compound activator is more conducive to the formation of abundant voids and a larger specific surface area in the adsorbent.
[0105] The number of modules and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention are obvious to those skilled in the art.
[0106] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing an adsorbent from sludge in wastewater from a purification plant, characterized in that: include: Step 1: collecting sludge generated by a water treatment plant, pre-treating the sludge to obtain a dried sludge raw material, wherein the moisture content of the dried sludge raw material is less than 10%; Step 2: crushing the sludge raw material into sludge particles with a particle size of 0.5 to 2 mm, then mixing the sludge particles with diatomaceous earth, and carbonizing them at a temperature of 600 to 700° C. for 20 to 70 minutes to form a porous carbon-based material, wherein the mass ratio of diatomaceous earth to the sludge particles is 1:10 to 20. During the carbonization, an inert gas is introduced at a flow rate of 0.5 to 1.0 L / min, and the temperature is gradually increased to 600 to 700° C. at a rate of 10 to 15° C. / min; Step 3: Evenly mix the activator and the carbon-based material in a mass ratio of 1:2 to 4, then put the mixed materials into an activation furnace, and perform an activation reaction at a temperature of 700-800° C. for 60-120 min; Step 4: Wash and dry the activated material, and then grind and screen to obtain 200-250 mesh particles as an adsorbent.
2. The method for preparing an adsorbent from sludge in wastewater from a purification plant according to claim 1, characterized in that: In step 1, the method for pre-treating the sludge in the wastewater includes: The crushed biomass material is added to the preliminarily treated sludge and mixed, the mass ratio of the biomass material to the sludge is 1:2, and the pH of the sludge is adjusted to 6-8. Then, magnetic zeolite is added thereto, mixed, and stirred and mixed again every 25 to 35 minutes. After adsorption for 8 to 10 hours, the magnetic zeolite is recovered, wherein the mass ratio of the magnetic zeolite to the sludge is 1:20 to 40. Then, the sludge is irradiated with microwaves at a frequency of 2000 to 2500 MHZ and a power of 500 to 1000 W for 30 to 80 seconds. Then dehydration is carried out to obtain dry sludge raw material.
3. The method for preparing an adsorbent from sludge in wastewater from a purification plant according to claim 1, characterized in that: In step 2, the sludge raw material is crushed and processed into sludge particles with a particle size of 0.5 to 2 mm. The sludge particles are then mixed with diatomaceous earth and carbonized at 650°C for 45 minutes to form a porous carbon-based material. The mass ratio of diatomaceous earth to the sludge particles is 1:
15. During the carbonization, an inert gas is introduced at a flow rate of 0.8 L / min, and the temperature is gradually increased to 650°C at a rate of 12°C / min.
4. The method for preparing an adsorbent from sludge in wastewater from a purification plant according to claim 1, characterized in that: In step 4, the method for washing the activated material is: repeatedly washing the activated material with hydrochloric acid solution and deionized water at a temperature of 70° C. until the pH value of the tail water reaches 4-5.
5. The method for preparing an adsorbent from sludge in wastewater from a purification plant according to claim 1, characterized in that: In step 4, the method for drying the activated material is: drying the cleaned material at 103-105° C. to constant weight.
6. The method for preparing an adsorbent from sludge in wastewater from a purification plant according to claim 1, characterized in that: In step 3, the activator is ZnCl2 or KOH or a composite solution of zinc chloride and sulfuric acid in a volume ratio of 1:1, and the concentrations of zinc chloride and sulfuric acid are both 5 mol / L.
7. The method for preparing an adsorbent from sludge in wastewater from a purification plant as claimed in claim 1, characterized in that: The inert gas is nitrogen or a rare gas.