Pt-loaded nanofiber aerogel material and preparation method thereof

Through electrospinning technology and carbonization treatment, the problem of uneven dispersion of platinum elements in Pt catalysts is solved, achieving uniform dispersion and efficient inlaying of platinum elements, simplifying the preparation process and reducing costs.

CN118743989APending Publication Date: 2024-10-08新疆理工学院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410665215.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

During the preparation process of existing Pt catalysts, platinum elements are prone to clustering and aggregation, resulting in uneven dispersion and affecting the catalytic effect. The cost is high and the process is complex.

Method used

By using N,N-dimethylformamide solution to dissolve chloroplatinic acid hexahydrate, combined with electrospinning technology to control the voltage, the platinum ions are excited from the ionic state to the atomic state, forming a uniformly dispersed state, and are embedded in the carbonization process into nanofiber membranes.

Benefits of technology

It achieves uniform and firm dispersion of platinum elements, reduces the probability of clustering and aggregation, improves the dispersion effect and use effect of the catalyst, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743989A_ABST
    Figure CN118743989A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a Pt-loaded nanofiber aerogel material, and particularly relates to the field of catalyst materials.The preparation method comprises the following steps that chloroplatinic acid, polyacrylonitrile and an organic solvent are mixed, the organic solvent is used for dissolving the chloroplatinic acid to form uniform platinum ions, stirring is conducted, and a spinning solution is obtained; under electrostatic spinning of the spinning solution, platinum ions in the spinning solution are excited from an ionic state to an atomic state and form a uniformly dispersed state by controlling the voltage of electrostatic spinning, so that platinum atoms are uniformly distributed on the nanofiber membrane, and a nanofiber membrane material is obtained; the nanofiber membrane material is subjected to carbonization treatment, platinum atoms are embedded into a fiber net of a nanofiber membrane, and the Pt-loaded nanofiber aerogel material is obtained. According to the preparation method, clustering and aggregation of platinum elements in the preparation process can be effectively avoided, and then atomic state platinum elements are evenly distributed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalyst materials, and in particular to a nanofiber aerogel material loaded with a Pt metal element and a preparation method thereof. Background Art

[0002] Pt catalyst is a catalyst often used in petroleum, coal and other chemical industries. In addition to high catalytic activity, strong selectivity, wide application fields and long life, it can also be recycled for regeneration and activation. However, Pt catalysts are expensive and can only be used on a small scale. In order to solve these problems, various new catalyst carrier structures and Pt catalysts with different catalytic functions are constantly being developed. As the key active component of the catalyst, Pt metal element plays an extremely important role in petrochemical reactions and environmental protection industries.

[0003] At present, Pt catalysts mainly exist in the form of composite catalysts, and the main preparation methods include hydrothermal method, precipitation coprecipitation method, sol-gel method and atomic layer deposition method. However, in addition to the high cost and complex preparation process of the above preparation methods, platinum elements are prone to clustering and aggregation during the preparation process, which makes the platinum elements in the obtained Pt catalyst not evenly dispersed, seriously affecting the use effect of the Pt catalyst.

[0004] Therefore, it is necessary to provide a catalytic system that can uniformly disperse Pt. Summary of the invention

[0005] In order to solve the problem that platinum element is prone to clustering and aggregation during the preparation of Pt catalyst in the prior art, resulting in uneven dispersion of platinum element, the present invention provides a nanofiber aerogel material loaded with Pt metal element and a preparation method thereof.

[0006] The present invention utilizes N,N-dimethylformamide solution to dissolve chloroplatinic acid hexahydrate to form uniform platinum ions. During the electrostatic spinning process, the voltage of the electrostatic spinning is controlled to excite the platinum ions from an ionic state to an atomic state and form a uniformly dispersed state, thereby reducing the probability of platinum elements generating clusters and aggregation during the preparation process, so that the obtained platinum atoms can be uniformly and firmly embedded in the nanofiber membrane network. Under carbonization treatment, the dispersion effect of the platinum atoms is further improved.

[0007] To achieve the above purpose, the specific technical scheme of the present invention is as follows.

[0008] The first aspect of the present invention provides a method for preparing a Pt-loaded nanofiber aerogel material, comprising the following steps:

[0009] Mixing chloroplatinic acid, polyacrylonitrile and an organic solvent, dissolving the chloroplatinic acid in the organic solvent to form uniform platinum ions, and stirring to obtain a spinning solution;

[0010] Under electrospinning, the platinum ions in the spinning solution are excited from the ionic state to the atomic state and form a uniformly dispersed state by controlling the electrospinning voltage. The platinum atoms are evenly distributed on the nanofiber membrane to obtain a nanofiber membrane material. The electrospinning voltage mainly plays two roles in the preparation of uniformly dispersed Pt atomic nanofiber membranes. One is to overcome the surface tension through the high voltage electric field to obtain a nanofiber material of uniform size, and the other is to provide electrons to excite the platinum ions from the ionic state to the atomic state.

[0011] The nanofiber membrane material is carbonized to embed platinum atoms into the fiber network of the nanofiber membrane to obtain a Pt-loaded nanofiber aerogel material.

[0012] In another preferred embodiment, the voltage of the electrospinning is 20-22 kV.

[0013] Under low voltage conditions, i.e., less than 20 kV, nanofiber materials are prone to breakage and lead to larger fiber diameters. Under 20-22 kV voltage conditions, nanofiber materials have thinner diameters, continuous fibers, and smooth surfaces, which are more conducive to the uniform distribution of atomic Pt elements. Excessive voltage, i.e., greater than 22 kV, will lead to faster spinning solution jets, uneven fiber jet splitting, the appearance of beaded nanofibers, and increased fiber diameter differences, which are more unfavorable for Pt ion excitation. Therefore, the present invention stabilizes the electrospinning voltage at 20-22 kV, which can not only obtain nanofiber materials with thinner diameters, continuous fibers, and smooth surfaces, but also is more conducive to the uniform distribution of atomic platinum elements.

[0014] In another preferred embodiment, the chloroplatinic acid is chloroplatinic acid hexahydrate, and the concentration of platinum ions in the chloroplatinic acid hexahydrate is 37.5-38.0 wt %.

[0015] The organic solvent is N,N-dimethylformamide, but the present invention is not limited to N,N-dimethylformamide organic solvent, and any organic solvent that can dissolve chloroplatinic acid and polyacrylonitrile reagents is included in the protection scope of the present invention.

[0016] In another preferred embodiment, the concentration of chloroplatinic acid in the spinning solution is 0.12-1.82 wt %.

[0017] In another preferred embodiment, the polyacrylonitrile accounts for 15.0-15.8 wt % of the organic solvent.

[0018] In another preferred embodiment, the specific process of the carbonization treatment is as follows:

[0019] Under protective atmosphere, heat up to 300-350°C at a heating rate of 2-5°C / min, and keep warm for 1-1.5h; then heat up to 900-950°C at a heating rate of 5-8°C / min, and keep warm for 1-1.5h.

[0020] In another preferred embodiment, the stirring time is 12 to 15 hours, and the rotation speed is 500 to 800 r / min.

[0021] In another preferred embodiment, the nanofiber membrane material further includes drying before the carbonization treatment, the drying temperature is 50-60° C., and the drying time is 3-5 hours.

[0022] In another preferred embodiment, the stirring time is 12 to 15 hours, and the rotation speed is 500 to 800 r / min.

[0023] The second aspect of the present invention provides a Pt-loaded nanofiber aerogel material, wherein the Pt-loaded nanofiber aerogel material is prepared by the preparation method provided by the first aspect of the present invention.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention controls the voltage of electrostatic spinning to excite the platinum ions in the spinning solution from the ionic state to the atomic state and form a uniformly dispersed state. At the same time, the obtained nanofiber material has a thinner diameter, continuous fibers and a thin surface, which is more conducive to the uniform distribution of atomic platinum elements, thereby effectively avoiding the problem in the prior art that platinum elements are prone to clustering and aggregation during the preparation of Pt catalysts, and the platinum elements in the obtained Pt catalysts are not uniformly dispersed. The dispersion effect of the platinum element is further improved under carbonization treatment, so that the obtained platinum atoms can be evenly and firmly embedded in the nanofiber membrane network.

[0026] (2) The N,N-dimethylformamide in the present invention can dissolve chloroplatinic acid to form uniform platinum ions, and the preparation method in the present application can disperse the platinum element to the maximum extent and embed it into the fiber network of the nanofiber membrane, making it difficult for the platinum element to be separated. After carbonization treatment, a highly dispersed polyacrylonitrile nanofiber aerogel material containing the Pt element can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A schematic flow chart of a method for preparing a polyacrylonitrile activated carbon nanofiber aerogel material loaded with Pt metal element provided in Example 1 of the present invention.

[0028] Figure 2 This is a product picture of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 1 of the present application.

[0029] Figure 3 This is a product picture of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Examples 1 to 10 of the present application.

[0030] Figure 4 This is a product picture of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Examples 11 to 18 of the present application.

[0031] Figure 5 : is a scanning electron microscope image of the Pt-loaded nanofiber aerogel material in Example 1 of the present invention; a) is a SEM image of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 1 of the present invention; b) is a SEM image of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Example 1 of the present invention.

[0032] Figure 6 : is a scanning electron microscope image of the Pt-loaded nanofiber aerogel material in Example 2 of the present invention; a) is a SEM image of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 2 of the present invention; b) is a SEM image of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Example 2 of the present invention.

[0033] Figure 7 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 3 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 3 of the present invention.

[0034] Figure 8 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 4 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 4 of the present invention.

[0035] Fig. 9 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 5 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 5 of the present invention.

[0036] Fig.10 : a) is the SEM image of the Pt-loaded nanofiber aerogel material in Example 6 of the present invention; b) is the SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 6 of the present invention.

[0037] Fig.11 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 7 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 7 of the present invention.

[0038] Fig.12 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 8 of the present invention; a) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber membrane prepared in Example 8 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel prepared in Example 8 of the present invention.

[0039] Fig.13 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 9 of the present invention; a) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber membrane prepared in Example 9 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel prepared in Example 9 of the present invention.

[0040] Fig.14 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 10 of the present invention; a) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber membrane prepared in Example 10 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel prepared in Example 10 of the present invention.

[0041] Fig.15 : is a scanning electron microscope image of the Pt-loaded nanofiber aerogel material in Example 11 of the present invention; a) is a SEM image of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 11 of the present invention; b) is a SEM image of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Example 11 of the present invention.

[0042] Fig.16 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 12 of the present invention; a) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber membrane prepared in Example 12 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel prepared in Example 12 of the present invention.

[0043] Fig.17: a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 13 of the present invention; a) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber membrane prepared in Example 13 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel prepared in Example 13 of the present invention.

[0044] Fig.18 : a) is a SEM image of the Pt-loaded nanofiber aerogel material in Example 14 of the present invention; b) is a SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 14 of the present invention.

[0045] Fig.19 : a) is the SEM image of the Pt-loaded nanofiber aerogel material in Example 15 of the present invention; b) is the SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 15 of the present invention.

[0046] Fig. 20 : a) is the SEM image of the Pt-loaded nanofiber aerogel material in Example 16 of the present invention; b) is the SEM image of the Pt-loaded polyacrylonitrile nanofiber aerogel in Example 16 of the present invention.

[0047] Fig.21 This is a scanning electron microscope image of the Pt-loaded nanofiber aerogel material in Example 17 of the present invention; a) is a SEM image of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 17 of the present invention; b) is a SEM image of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Example 17 of the present invention.

[0048] Fig. 22 : is a scanning electron microscope image of the nanofiber aerogel material loaded with Pt in Example 18 of the present invention; a) is a SEM image of the polyacrylonitrile nanofiber membrane loaded with Pt element prepared in Example 1 of the present invention; b) is a SEM image of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Example 18 of the present invention.

[0049] Fig.23 This is the XRD diagram of the polyacrylonitrile nanofiber aerogel in Example 1 of the present invention. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0051] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0052] Currently, Pt catalysts mainly exist in the form of composite catalysts, and the main preparation methods include hydrothermal method, precipitation co-precipitation method, sol-gel method and atomic layer deposition method. The above preparation methods have the problems of high cost, complex preparation process and uneven dispersion of platinum elements.

[0053] Activated carbon nanofiber aerogel is an excellent carrier widely used in the field of catalysis. It uses organic fiber as a precursor and is made into a new functional aerogel material through various methods. Activated carbon nanofiber aerogel materials are widely used in environmental issues, battery fields, energy fields, etc. The preparation of activated carbon nanofiber aerogel-loaded Pt catalyst is based on the high specific surface area and high porosity of activated carbon nanofiber aerogel, and the preparation method and process conditions of aerogel-loaded Pt catalyst are studied. The polyacrylonitrile nanofiber aerogel prepared by electrospinning has a large specific surface area, high conductivity, extremely high aspect ratio and high porosity, and has broad application prospects in the fields of medicine, chemical industry, new materials, environmental protection, pesticides, pigments, dyes, etc. Polyacrylonitrile nanofibers make up for the shortcomings of small specific surface area of ​​traditional catalyst carriers, and are expected to reduce the amount of Pt element without changing the catalytic activity of the catalyst, and even make the catalyst more active.

[0054] The present invention is different from the existing Pt composite catalyst preparation method in that, by combining the electrostatic spinning technology and controlling the voltage of the electrostatic spinning, Pt is excited from the ion state of the spinning solution to the atomic state by a high-voltage electrostatic method, thereby reducing the probability of clustering and aggregation in the preparation process of the Pt composite catalyst in the existing preparation method, and greatly improving the uniformity of Pt atomic dispersion. The method of the present invention can directly prepare a highly dispersed Pt-containing nanofiber aerogel material, the method is simple, and the preparation industrial process is simplified.

[0055] The present invention utilizes N,N-dimethylformamide solution to dissolve chloroplatinic acid hexahydrate to form uniform platinum ions, and then uses electrostatic spinning to excite the platinum ions from an ionic state to an atomic state to form a uniformly dispersed state, and the obtained platinum atoms are uniformly and firmly embedded in the nanofiber membrane network. Under carbonization treatment, the dispersion effect of the platinum element can be further improved.

[0056] The molecular weight of polyacrylonitrile in the following examples is 5×104 ~15×10 4 Preferably, the molecular weight of the polyacrylonitrile is 5×10 4 , 8.5×10 4 , 15×10 4 The embodiment of the present invention can use polyacrylonitrile reagents with different molecular weights to prepare Pt nanofiber aerogel materials, and mainly gives priority to three commonly used molecular weight polyacrylonitrile widely used in the market.

[0057] The following is a detailed description of a method for preparing a nanofiber aerogel material loaded with Pt metal element.

[0058] Example 1

[0059] A method for preparing a Pt-loaded nanofiber aerogel material, such as Figure 1 As shown, the following steps are included:

[0060] S1. Measure 6 portions of 10 mL of N,N-dimethylformamide solution into a 50 mL beaker, weigh 0.11 wt% of chloroplatinic acid hexahydrate, add chloroplatinic acid hexahydrate into the N,N-dimethylformamide solution in sequence, and stir at 650 r / min for 40 min to dissolve, to prepare a mixed solution A.

[0061] S2, weighing 1.5 g of polyacrylonitrile powder with a molecular weight of 50,000, adding the polyacrylonitrile powder to the mixed solution A under stirring, and continuing to stir at a speed of 650 r / min for 12 h to allow the polyacrylonitrile to fully dissolve, to prepare a spinning solution B;

[0062] S3, select a 10mL syringe to absorb the electrospinning solution, use a micro-injection pump device at a temperature of 25°C and a voltage of 20kV, the electrospinning liquid supply rate is 1.25mL / h, the distance between the electrospinning needle and the negative electrode plate is 10cm, the electrospinning is 7h, and the polyacrylonitrile nanofiber membrane material is obtained by drying in a constant temperature drying oven at 50°C for 3h;

[0063] S4. Compress the polyacrylonitrile nanofiber membrane material and prepare it into a cylindrical shape. Under nitrogen protection, transfer the prepared polyacrylonitrile nanofiber membrane material to a tubular furnace, heat it to 300°C at a heating rate of 2°C / min, and keep it at this temperature for 1 hour for pre-oxidation treatment, and then heat it to 900°C at a heating rate of 5°C / min and keep it at this temperature for 1 hour for carbonization to obtain a Pt-loaded nanofiber aerogel material.

[0064] Example 2

[0065] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.18 wt % which is different from Example 1, the remaining steps are the same as those of Example 1.

[0066] Example 3

[0067] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.46wt% which is different from Example 1, the remaining steps are the same as those of Example 1.

[0068] Example 4

[0069] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.93wt% which is different from Example 1, the remaining steps are the same as those of Example 1.

[0070] Example 5

[0071] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.36wt% which is different from Example 1, the remaining steps are the same as those of Example 1.

[0072] Example 6

[0073] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.86wt% which is different from Example 1, the remaining steps are the same as those of Example 1.

[0074] Example 7

[0075] A method for preparing a Pt-loaded nanofiber aerogel material comprises the following steps:

[0076] S1. Measure 6 portions of 10 mL of N,N-dimethylformamide solution into a 50 mL beaker, weigh 0.10 wt% chloroplatinic acid hexahydrate, add the chloroplatinic acid hexahydrate reagent into the N,N-dimethylformamide solution in sequence, and stir and dissolve at a speed of 650 r / min for 40 min to prepare a mixed solution A;

[0077] S2, weighing 1.5 g of polyacrylonitrile powder with a molecular weight of 85,000, adding the polyacrylonitrile powder to the mixed solution A under stirring, and continuing to stir at a speed of 650 r / min for 12 h to allow the polyacrylonitrile to fully dissolve, to prepare a spinning solution B;

[0078] S3, select a 10mL syringe to absorb the electrospinning solution, use a micro-injection pump device at a temperature of 25°C and a voltage of 20kV, the electrospinning liquid supply rate is 2.0mL / h, the distance between the electrospinning needle and the negative electrode plate is 20cm, the electrospinning is 7h, and it is dried in a constant temperature drying oven at 50°C for 3h to obtain a polyacrylonitrile nanofiber membrane material;

[0079] S4. Compress the polyacrylonitrile activated carbon nanofiber membrane and prepare it into a cylindrical shape. Under nitrogen protection, transfer the prepared polyacrylonitrile nanofiber membrane material to a tubular furnace, heat it to 300°C at a heating rate of 2°C / min, and keep it at this temperature for 1 hour for pre-oxidation treatment, and then heat it to 900°C at a heating rate of 5°C / min and keep it at this temperature for 1 hour for carbonization to obtain a Pt-loaded nanofiber aerogel material.

[0080] Example 8

[0081] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.20wt% which is different from Example 7, the remaining steps are the same as those of Example 7.

[0082] Example 9

[0083] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.47 wt % which is different from Example 7, the remaining steps are the same as those of Example 7.

[0084] Example 10

[0085] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.13 wt % which is different from Example 7, the remaining steps are the same as those of Example 7.

[0086] Embodiment 11

[0087] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.40wt% which is different from Example 7, the remaining steps are the same as those of Example 7.

[0088] Example 12

[0089] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.86wt% which is different from Example 7, the remaining steps are the same as those of Example 7.

[0090] Example 13

[0091] A method for preparing a Pt-loaded nanofiber aerogel material comprises the following steps:

[0092] S1. Measure 6 portions of 10 mL of N,N-dimethylformamide solution into a 50 mL beaker, weigh 0.12 wt% of chloroplatinic acid hexahydrate, add the chloroplatinic acid hexahydrate reagent to the N,N-dimethylformamide solution in sequence, and stir and dissolve at a speed of 650 r / min for 40 min to prepare a mixed solution A;

[0093] S2, weighing 1.5 g of polyacrylonitrile powder with a molecular weight of 150,000, adding the polyacrylonitrile powder to the mixed solution A under stirring, and continuing to stir at a speed of 650 r / min for 12 h to allow the polyacrylonitrile to fully dissolve, to prepare a spinning solution B;

[0094] S3, select a 10mL syringe to absorb the electrospinning solution, use a micro-injection pump device at a temperature of 25°C and a voltage of 20kV, the electrospinning liquid supply rate is 2.0mL / h, the distance between the electrospinning needle and the negative electrode plate is 20cm, the electrospinning is 7h, and it is dried in a constant temperature drying oven at 50°C for 3h to obtain a polyacrylonitrile nanofiber membrane material product;

[0095] S4. Compress the polyacrylonitrile activated carbon nanofiber membrane and prepare it into a cylindrical shape. Under nitrogen protection, transfer the prepared polyacrylonitrile nanofiber membrane material to a tubular furnace, heat it to 300°C at a heating rate of 2°C / min, and keep it at this temperature for 1 hour for pre-oxidation treatment, and then heat it to 900°C at a heating rate of 5°C / min and keep it at this temperature for 1 hour for carbonization to obtain a Pt-loaded nanofiber aerogel material.

[0096] Embodiment 14

[0097] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.18wt% which is different from Example 13, the remaining steps are the same as Example 13.

[0098] Embodiment 15

[0099] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 0.45wt% which is different from Example 13, the remaining steps are the same as Example 13.

[0100] Example 16

[0101] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.13wt% which is different from Example 13, the remaining steps are the same as Example 13.

[0102] Embodiment 17

[0103] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.35wt% which is different from Example 13, the remaining steps are the same as Example 13.

[0104] Embodiment 18

[0105] A method for preparing a Pt-loaded nanofiber aerogel material, except that the concentration of chloroplatinic acid hexahydrate is 1.82wt% which is different from Example 13, the remaining steps are the same as Example 13.

[0106] In order to further illustrate that platinum elements are uniformly dispersed in the Pt-loaded nanofiber aerogel materials prepared in Examples 1 to 18 of the present invention, we conducted the following experiments.

[0107] Figure 2 This is a product picture of the Pt-loaded nanofiber aerogel material prepared in Example 1 of the present application. Figure 2 It can be seen that by using the electrospinning technology, the spinning solution is spun into a uniform fiber material under the conditions of a high voltage power supply and a micro-propulsion pump; the polyacrylonitrile nanofiber membrane material can be covered on the tin foil layer by layer to form a fiber membrane material with a certain thickness. Under the vertical spinning method, the polyacrylonitrile nanofiber material forms a relatively standardized circular shape.

[0108] from Figure 3 and Figure 4 The product pictures of the polyacrylonitrile nanofiber aerogel loaded with Pt element prepared in Examples 1 to 18 are shown in FIG. Figure 3 and Figure 4 It can be seen that the aerogel material is obtained by plasticizing and then carbonizing the polyacrylonitrile nanofiber material, and the aerogel material has a sheet-like structure.

[0109] from Figures 5 to 22 As shown, the scanning electron microscopy analysis of the polyacrylonitrile nanofiber materials loaded with Pt elements prepared in Examples 1 to 18 shows that the aerogel materials have obvious fiber structures, and the platinum elements cover the surface of the aerogel fibers during the electrospinning and aerogel carbonization processes.

[0110] Due to the addition of platinum, compared with the simple polypropylene nanofiber aerogel material, Fig.23 The XRD diffraction peak of the aerogel material containing platinum has a more obvious diffraction peak at the 40° position, which indirectly proves the presence of platinum in the aerogel material.

[0111] It can be seen from the above experimental results that the present invention controls the voltage of electrostatic spinning to excite the platinum ions in the spinning solution from the ionic state to the atomic state and form a uniformly dispersed state. At the same time, the obtained nanofiber material has a thinner diameter, continuous fibers and a surface, which is more conducive to the uniform distribution of atomic platinum elements, thereby effectively avoiding the problem in the prior art that platinum elements are prone to clustering and aggregation during the preparation of Pt catalysts, and the platinum elements in the obtained Pt catalysts are not uniformly dispersed. The dispersion effect of the platinum element is further improved under carbonization treatment, so that the obtained platinum atoms can be evenly and firmly embedded in the nanofiber membrane network.

[0112] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalent technologies, the present invention is also intended to include these changes and variations. The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and their protection scope is not limited thereto. Equivalent substitutions or changes made by those skilled in the art on the basis of the present invention are all within the protection scope of the present invention, and the protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a Pt-loaded nanofiber aerogel material, characterized in that: The following steps are involved: Mixing chloroplatinic acid, polyacrylonitrile and an organic solvent, dissolving the chloroplatinic acid in the organic solvent to form uniform platinum ions, and stirring to obtain a spinning solution; Under electrostatic spinning, the platinum ions in the spinning solution are excited from the ionic state to the atomic state and form a uniformly dispersed state by controlling the voltage of the electrostatic spinning, so that the platinum atoms are evenly distributed on the nanofiber membrane to obtain a nanofiber membrane material; The nanofiber membrane material is carbonized to embed platinum atoms into the fiber network of the nanofiber membrane to obtain a Pt-loaded nanofiber aerogel material.

2. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The voltage of the electrostatic spinning is 20-22 kV.

3. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The chloroplatinic acid is chloroplatinic acid hexahydrate, and the concentration of platinum ions in the chloroplatinic acid hexahydrate is 37.5-38.0wt%; The organic solvent is N,N-dimethylformamide.

4. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The concentration of chloroplatinic acid in the spinning solution is 0.12-1.82 wt %.

5. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The polyacrylonitrile accounts for 15.0-15.8 wt % of the organic solvent.

6. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The specific process of the carbonization treatment is as follows: Under protective atmosphere, heat up to 300-350°C at a heating rate of 2-5°C / min, and keep warm for 1-1.5h; then heat up to 900-950°C at a heating rate of 5-8°C / min, and keep warm for 1-1.5h.

7. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The stirring time is 12 to 15 hours, and the rotation speed is 500 to 800 r / min.

8. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The conditions of the electrospinning are: The temperature is 25-30° C., the extrusion speed of the spinning solution is 1.25-2.0 mL / h, and the distance between the electrospinning needle and the negative electrode plate is 10-20 cm.

9. The method for preparing a Pt-loaded nanofiber aerogel material according to claim 1, characterized in that: The nanofiber membrane material is further dried before the carbonization treatment, the drying temperature is 50-60° C., and the drying time is 3-5 hours.

10. A Pt-loaded nanofiber aerogel material prepared by the preparation method according to any one of claims 1 to 9.