Bilateral high-density chemical bonding directional induction method for thermal connection interface of metal and thermoplastic composite material
By grafting high-density amino functional groups and coating functional block copolymers on the connection interface between metal and thermoplastic composite materials, high-density chemical bonds are formed, which solves the problems of low interface bonding density and weak binding force, and significantly improves the connection Strength, suitable for a variety of thermal joining processes.
Patent Information
- Application Number
- CN202410760203.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
The existing interface between metal and thermoplastic composite materials has low bond density and weak interface bonding force, making it difficult to achieve high-strength connections. Moreover, existing control methods have problems with processing time, difficulty in chemical bonding structure, and poor orientation.
By grafting high-density amino functional groups on the surface of thermoplastic composite materials, and coating functional block copolymers on the metal surface, chemical bonding reactions are used to form high-density Si-O-M and C-N covalent bonds, thus realizing the dual integration of metal and thermoplastic composite materials. Side-side high-density chemical bonding orientation induction.
It significantly improves the connection strength of the thermal connection interface between metal and thermoplastic composite materials, solves the problems of low bond density and weak bonding force at the interface, and is suitable for a variety of thermal connection processes. It has strong adaptability and is suitable for a variety of thermal connection processes.
Smart Images

Figure BDA0004890832270000021 
Figure BDA0004890832270000041 
Figure BDA0004890832270000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous material connection, and in particular relates to a double-sided high-density chemical bonding directional induction method for a thermal connection interface between a metal and a thermoplastic composite material. Background Art
[0002] Equipment lightweighting is an inevitable trend in the development of my country's industrial manufacturing. Multi-material composite structures that partially replace lightweight alloys with carbon fiber reinforced thermoplastic composites can achieve local weight reduction of 30-40%, becoming the main form of equipment lightweighting. It has broad application prospects in lightweight industries such as aerospace, rail transit, automobiles, and medical care.
[0003] Compared with the metallurgical bonding between homogeneous metal materials, the interface between metal and thermoplastic composites is limited by the huge difference in thermal physical properties. It is difficult to dissolve in each other to form a high-strength connection during the thermal connection process. The joint strength of two heterogeneous materials directly connected by thermal connection process is low. The direct high-strength connection between thermoplastic composites and metals, two very different lightweight materials, has become a research hotspot in the field of heterogeneous material connection.
[0004] The invention patent application with application number 202110626474.7, "A Thermoplastic Composite Material-Metal Laser Welding Method", improves the connection strength by prefabricating micro-textures on the metal surface and laying plastic powder to regulate the mechanical interlocking mechanism between the metal and the thermoplastic composite material. However, the micro-texture processing cycle introduced by this method is long, and the strength improvement effect is limited as the depth of the micro-texture increases. The pre-set powder does not adhere firmly to the parent material during the thermal connection process, and it is not suitable for connections between large-size structural parts, which restricts the industrial application of this technology.
[0005] The invention patent application with application number 202310008380.2, "A functional Schiff base polymer and its preparation method and application", synthesized a functional polymer structure to induce high-density secondary interactions at the interface based on the atomic and functional group composition of metal and thermoplastic composites, thereby achieving a significant improvement in the strength of the thermal connection joints between metal and thermoplastic composites. However, the secondary interactions induced by this method are weaker than chemical bonding connections, and the effect is not targeted.
[0006] It can be seen that the existing methods for regulating the interface between metal and thermoplastic composites still have disadvantages in processing aging, difficulty in chemical bonding, poor orientation and strengthening effect. The interface directional regulation technology for the composition differences of heterogeneous materials still needs to be developed urgently. Summary of the invention
[0007] In order to solve the problems of low bonding density and weak interface bonding force of existing metal and thermoplastic composite thermal connection interfaces, the present invention provides a double-sided high-density chemical bonding directional induction method for the thermal connection interface of metal and thermoplastic composite materials.
[0008] The technical solution of the present invention:
[0009] A method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material comprises the following steps:
[0010] Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials:
[0011] Step 2: Coating the functional block copolymer on the metal surface:
[0012] Step 3: Assemble the thermoplastic composite material with high-density amino functional groups grafted on the surface obtained in step 1 and the metal with functional block copolymer coating cured on the surface obtained in step 2 in an overlapping manner, complete chemical bonding during the thermal connection process, and obtain a thermal connection joint between the metal and the thermoplastic composite material.
[0013] Furthermore, the thermoplastic composite material in step 1 is a polyetheretherketone-based thermoplastic composite material, specifically one of polyetheretherketone monomer, carbon fiber reinforced polyetheretherketone or glass fiber reinforced polyetheretherketone.
[0014] Furthermore, the specific method of grafting in step 1 is: placing the thermoplastic composite material in a toluene solution containing azobisisobutyronitrile, stirring at 80°C for 1 hour, dropping methyl acrylate into the obtained mixed system and continuously stirring to obtain a thermoplastic composite material with surface grafted polymethyl acrylate, placing the obtained thermoplastic composite material with surface grafted polymethyl acrylate in an ethanol solution and dropping a certain amount of ethylenediamine, stirring at 50°C for 24 hours to obtain a thermoplastic composite material with uniformly distributed polymerized high-density amino functional groups grafted on the surface.
[0015] Furthermore, the mass volume ratio of the azobisisobutyronitrile to the toluene solution is 0.2 g:100 mL to 2 g:100 mL, the molar volume ratio of the methyl acrylate to the toluene solution in the mixed system is 0.05 mol:100 mL to 2 mol:100 mL, and the molar volume ratio of the ethylenediamine to the ethanol solution is 0.05 mol:100 mL to 2 mol:100 mL.
[0016] Furthermore, the chemical structural formula of the functional block copolymer in step 2 is:
[0017]
[0018] In the chemical structural formula, n=10-1000, and m=n×(5-50%).
[0019] Furthermore, the specific method of coating the functional block copolymer on the metal surface in step 2 is: dissolving the functional block copolymer and the catalyst in an organic solvent to obtain a functional block copolymer modified solution, spraying the functional block copolymer modified solution onto the metal surface to be connected, and drying at room temperature for 24 hours to obtain a metal with a block copolymer coating cured on the surface.
[0020] Furthermore, the catalyst is one of dibutyltin dilaurate or stannous octoate, and the organic solvent is one of dichloromethane, tetrahydrofuran, toluene or chloroform.
[0021] Furthermore, the concentration of the functional block copolymer in the functional block copolymer modification solution is 0.001 to 0.1 mol / mL, and the concentration of the catalyst in the functional block copolymer modification solution is 0.001 to 0.1 g / ml.
[0022] Furthermore, the metal to be connected is one of titanium alloy, stainless steel, aluminum alloy or magnesium alloy, and the thickness of the block copolymer coating cured on the metal surface is 50 to 1000 nm.
[0023] Furthermore, the thermal connection in step three is one of laser connection, stir friction connection, hot pressing connection, resistance welding or induction connection.
[0024] Beneficial effects of the present invention:
[0025] The present invention uses directional induction of double-sided chemical bonding at the thermal connection interface to graft uniformly distributed polymerized high-density amino functional (-NH2) groups on the surface of the thermoplastic composite material, and forms a functional block copolymer coating on the metal surface through dealcoholization reaction between the functional block copolymer and the hydroxyl (-OH) adsorbed on the metal surface to form high-density Si-OM (metal atom) covalent bonds. During the thermal connection process, the epoxy groups in the functional block copolymer cured on the metal surface react with the amino groups on the surface of the thermoplastic composite material to form CN covalent bonds, thereby realizing a bridge-type connection with double-sided high-density chemical bonding, which significantly improves the connection strength of the thermal connection interface between the metal and the thermoplastic composite material.
[0026] The method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite materials provided by the present invention solves the problems of difficulty in direct bonding, difficulty in directional introduction, unclear bonding, low bonding density and weak interface bonding force caused by existing interface control methods of chemical bonding at the connection interface of metal and thermoplastic composite materials. The control size can be adjusted according to the connection area, the control process is simple and convenient, and it is applicable to a variety of thermal connection processes with strong adaptability. It has good application prospects in the field of thermal connection interface control of metal and thermoplastic composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 a is a Fourier transform infrared spectrum of the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK plate before and after grafting high-density amino functional groups in step 1 of Example 1, and b is a local enlarged view of the typical functional group wavenumber region in a;
[0028] Figure 2 is a Fourier transform infrared spectrum of the surface of TC4 titanium alloy before and after curing the block copolymer in step 2 of Example 1, and b is a local enlarged view of the typical functional group wave number region in a;
[0029] Figure 3 This is an infrared spectrum of the thermal connection interface area of the TC4 titanium alloy plate and the carbon fiber reinforced polyetheretherketone CF-PEEK plate in Example 1;
[0030] Figure 4 It is a comparison diagram of the tensile curves of the thermal connection joints obtained in Example 1, Example 2 and the comparative example;
[0031] Figure 5 This is a connection mechanism diagram of the directional regulation of high-density chemical bonding on both sides of the thermal connection interface of the TC4 titanium alloy plate and the carbon fiber reinforced polyetheretherketone CF-PEEK plate in Example 1. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0033] Example 1
[0034] This embodiment provides a method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material.
[0035] In this embodiment, the thermoplastic composite material to be connected is a carbon fiber reinforced polyetheretherketone CF-PEEK plate, and the plate size is 50 mm long, 30 mm wide, and 2 mm thick. Before implementing the grafting regulation, the carbon fiber reinforced polyetheretherketone (CF-PEEK) is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the cleaned carbon fiber reinforced polyetheretherketone (CF-PEEK) plate is placed in an 80°C drying oven for 2 hours for standby use.
[0036] The chemical structural formula of the functional block copolymer in this embodiment is:
[0037]
[0038] In the chemical structure formula, n=40, m=10.
[0039] In this embodiment, the metal to be connected is a TC4 titanium alloy plate, and the plate size is 50 mm long, 30 mm wide, and 1.5 mm thick. Before implementing the coating control, the TC4 titanium alloy plate is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the TC4 titanium alloy plate is pickled in a mixed acid solution of 80% deionized water + 15% hydrochloric acid + 5% hydrofluoric acid for 1 minute and then blown dry for standby use.
[0040] The method for directional induction of high-density chemical bonding on both sides of the thermal connection interface between metal and thermoplastic composite material in this embodiment includes the following steps:
[0041] Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials:
[0042] The carbon fiber reinforced polyetheretherketone CF-PEEK sheet was placed in a 200ml toluene solution containing 0.4g azobisisobutyronitrile and stirred at 80°C for 1h to generate active points on the surface of the thermoplastic composite material. 0.2mol methyl acrylate was added dropwise to the obtained mixed system and stirred continuously to graft polymethyl acrylate onto the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK sheet. The carbon fiber reinforced polyetheretherketone CF-PEEK sheet with polymethyl acrylate grafted on the surface was taken out and placed in 200ml anhydrous ethanol and 0.2mol ethylenediamine was added dropwise. It was stirred at 50°C for 24h to cause aminolysis reaction to introduce amino groups, and a carbon fiber reinforced polyetheretherketone CF-PEEK sheet with uniformly distributed polymerized high-density amino functional groups grafted on the surface was obtained.
[0043] Step 2: Coating the functional block copolymer on the metal surface:
[0044] The functional block copolymer and the catalyst dibutyltin dilaurate are dissolved in tetrahydrofuran, and the mixture is fully mixed and stirred to obtain a functional block copolymer modified solution. The concentration of the functional block copolymer in the functional block copolymer modified solution is 0.01 mol / mL, and the concentration of the dibutyltin dilaurate is 0.005 g / ml.
[0045] The functional block copolymer modified solution was sprayed onto the surface of the TC4 titanium alloy plate, and after high-temperature drying at 80°C, a directional control coating with a thickness of 500 nm was obtained. After drying at room temperature for 24 hours, a TC4 titanium alloy plate with a block copolymer coating cured on the surface was obtained.
[0046] Step 3. Tightly overlap the carbon fiber reinforced polyetheretherketone CF-PEEK plate with high-density amino functional groups grafted on the surface obtained in step 1 and the TC4 titanium alloy plate with functional block copolymer coating cured on the surface obtained in step 2, with an overlap width of 20 mm. Perform laser connection under the following process parameters: laser power: 850 W, defocus: +6 mm, laser scanning speed: 0.8 m / min, welding length: 30 mm, interface clamping pressure: 0.3 MPa, laser scanning surface: TC4 titanium alloy surface; chemical bonding is completed during the laser connection process to obtain a thermal connection joint between TC4 titanium alloy and carbon fiber reinforced polyetheretherketone CF-PEEK.
[0047] Figure 1 : This is the Fourier transform infrared spectrum of the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK plate before and after grafting high-density amino functional groups in step 1 of Example 1, and b is a local enlarged view of the wavenumber area of the typical functional group in a; compared with the Fourier transform infrared spectrum of the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK plate before regulation, the Fourier transform infrared spectrum of the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK plate after grafting high-density amino functional groups is 3359cm -1 and 3379cm -1 A typical diffraction peak of amino group (-NH2) appears at the position of the carbon fiber reinforced polyetheretherketone (CF-PEEK) sheet. This indicates that Example 1 successfully introduces high-density amino group (-NH2) functional groups in a polymerized state on the surface of the carbon fiber reinforced polyetheretherketone (CF-PEEK) sheet.
[0048] Figure 2 : The Fourier transform infrared spectra of the TC4 titanium alloy surface before and after curing the block copolymer in step 2 of Example 1; b is a local enlarged view of the typical functional group wavenumber region in a; compared with the Fourier transform infrared spectrum of the uncured TC4 surface, the functional block copolymer on the surface of the TC4 titanium alloy after curing has a wavelength of 1676 cm -1 The Si-OC bond disappears at the interface, while the -1The Si-O-Ti bond appears at 908 cm-1, indicating that the Si-OC bond reacts with the hydroxyl groups adsorbed on the surface of TC4 to form a covalent bond. -1 The epoxy groups appeared, indicating that the epoxy functional groups were also successfully cured on the surface of TC4 titanium alloy.
[0049] Figure 3 This is the infrared spectrum of the thermal connection interface area of the TC4 titanium alloy plate and the carbon fiber reinforced polyetheretherketone CF-PEEK plate in Example 1; by comparison Figure 1 and Figure 2 It can be seen that the block copolymer formed after curing the surface of TC4 titanium alloy in step 2 is located at 940cm -1 The Si-O-Ti bond is retained on the TC4 side of the interface, while the wave number of the high-density amino functional groups introduced by grafting the surface of the polyetheretherketone CF-PEEK sheet in step 1 is 3359 cm -1 and 3379cm -1 The wave number introduced by the amino group (-NH2) and the block copolymer cured on the surface of TC4 titanium alloy in step 2 is 908cm -1 The epoxy group disappears at a wave number of 1249 cm -1 The typical peak of CN bond appears at , indicating that during the thermal connection process, the high-density chemical structure introduced on the surface of metal and thermoplastic composite materials by the method of directional induction of double-sided high-density chemical bonding at the thermal connection interface can react at the interface and form a chemical bonding bridge structure, thereby realizing directional induction of double-sided high-density chemical bonding at the thermal connection interface.
[0050] Example 2
[0051] This embodiment provides a method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material.
[0052] In this embodiment, the thermoplastic composite material to be connected is a carbon fiber reinforced polyetheretherketone CF-PEEK plate, and the plate size is 50 mm long, 30 mm wide, and 2 mm thick. Before implementing the grafting regulation, the carbon fiber reinforced polyetheretherketone (CF-PEEK) is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the cleaned carbon fiber reinforced polyetheretherketone (CF-PEEK) plate is placed in an 80°C drying oven for 2 hours for standby use.
[0053] The chemical structural formula of the functional block copolymer in this embodiment is:
[0054]
[0055] In the chemical structure formula, n=40, m=10.
[0056] In this embodiment, the metal to be connected is a TC4 titanium alloy plate, and the plate size is 50 mm long, 30 mm wide, and 1.5 mm thick. Before implementing the coating control, the TC4 titanium alloy plate is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the TC4 titanium alloy plate is pickled in a mixed acid solution of 80% deionized water + 15% hydrochloric acid + 5% hydrofluoric acid for 1 minute and then blown dry for standby use.
[0057] The method for directional induction of high-density chemical bonding on both sides of the thermal connection interface between metal and thermoplastic composite material in this embodiment includes the following steps:
[0058] Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials:
[0059] The carbon fiber reinforced polyetheretherketone CF-PEEK sheet was placed in a 200ml toluene solution containing 0.8g azobisisobutyronitrile and stirred at 80°C for 1h to generate active points on the surface of the thermoplastic composite material. 0.4mol methyl acrylate was added dropwise to the obtained mixed system and stirred continuously to graft polymethyl acrylate onto the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK sheet. The carbon fiber reinforced polyetheretherketone CF-PEEK sheet with polymethyl acrylate grafted on the surface was taken out and placed in 200ml anhydrous ethanol and 0.4mol ethylenediamine was added dropwise. It was stirred at 50°C for 24h to cause aminolysis reaction to introduce amino groups, and a carbon fiber reinforced polyetheretherketone CF-PEEK sheet with uniformly distributed polymerized high-density amino functional groups grafted on the surface was obtained.
[0060] Step 2: Coating the functional block copolymer on the metal surface:
[0061] The functional block copolymer and the catalyst dibutyltin dilaurate are dissolved in tetrahydrofuran, and the mixture is fully mixed and stirred to obtain a functional block copolymer modified solution. The concentration of the functional block copolymer in the functional block copolymer modified solution is 0.01 mol / mL, and the concentration of the dibutyltin dilaurate is 0.005 g / ml.
[0062] The functional block copolymer modified solution was sprayed onto the surface of the TC4 titanium alloy plate, and after high-temperature drying at 80°C, a directional control coating with a thickness of 500 nm was obtained. After drying at room temperature for 24 hours, a TC4 titanium alloy plate with a block copolymer coating cured on the surface was obtained.
[0063] Step 3. Tightly overlap the carbon fiber reinforced polyetheretherketone CF-PEEK plate with high-density amino functional groups grafted on the surface obtained in step 1 and the TC4 titanium alloy plate with functional block copolymer coating cured on the surface obtained in step 2, with an overlap width of 20 mm. Perform laser connection under the following process parameters: laser power: 850 W, defocus: +6 mm, laser scanning speed: 0.8 m / min, welding length: 30 mm, interface clamping pressure: 0.3 MPa, laser scanning surface: TC4 titanium alloy surface; chemical bonding is completed during the laser connection process to obtain a thermal connection joint between TC4 titanium alloy and carbon fiber reinforced polyetheretherketone CF-PEEK.
[0064] Example 3
[0065] This embodiment provides a method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material.
[0066] In this embodiment, the thermoplastic composite material to be connected is a carbon fiber reinforced polyetheretherketone CF-PEEK plate, and the plate size is 50 mm long, 30 mm wide, and 2 mm thick. Before implementing the grafting regulation, the carbon fiber reinforced polyetheretherketone (CF-PEEK) is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the cleaned carbon fiber reinforced polyetheretherketone (CF-PEEK) plate is placed in an 80°C drying oven for 2 hours for standby use.
[0067] The chemical structural formula of the functional block copolymer in this embodiment is:
[0068]
[0069] In the chemical structure formula, n=40, m=10.
[0070] In this embodiment, the metal to be connected is a 6061 aluminum alloy plate, and the plate size is 50 mm long, 30 mm wide, and 1.5 mm thick. Before implementing the coating control, the 6061 aluminum alloy plate is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the 6061 aluminum alloy plate is pickled in a mixed acid solution of 80% deionized water + 15% hydrochloric acid + 5% hydrofluoric acid for 1 minute and then blown dry for standby use.
[0071] The method for directional induction of high-density chemical bonding on both sides of the thermal connection interface between metal and thermoplastic composite material in this embodiment includes the following steps:
[0072] Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials:
[0073] The carbon fiber reinforced polyetheretherketone CF-PEEK sheet was placed in a 200ml toluene solution containing 0.4g azobisisobutyronitrile and stirred at 80°C for 1h to generate active points on the surface of the thermoplastic composite material. 0.2mol methyl acrylate was added dropwise to the obtained mixed system and stirred continuously to graft polymethyl acrylate onto the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK sheet. The carbon fiber reinforced polyetheretherketone CF-PEEK sheet with polymethyl acrylate grafted on the surface was taken out and placed in 200ml anhydrous ethanol and 0.2mol ethylenediamine was added dropwise. It was stirred at 50°C for 24h to cause aminolysis reaction to introduce amino groups, and a carbon fiber reinforced polyetheretherketone CF-PEEK sheet with uniformly distributed polymerized high-density amino functional groups grafted on the surface was obtained.
[0074] Step 2: Coating the functional block copolymer on the metal surface:
[0075] The functional block copolymer and the catalyst dibutyltin dilaurate are dissolved in tetrahydrofuran, and the mixture is fully mixed and stirred to obtain a functional block copolymer modified solution. The concentration of the functional block copolymer in the functional block copolymer modified solution is 0.01 mol / mL, and the concentration of the dibutyltin dilaurate is 0.005 g / ml.
[0076] The functional block copolymer modified solution was sprayed onto the surface of the 6061 aluminum alloy plate, and after high-temperature drying at 80°C, a directional control coating with a thickness of 500 nm was obtained. After drying at room temperature for 24 hours, a 6061 aluminum alloy plate with a block copolymer coating cured on the surface was obtained.
[0077] Step 3. Tightly overlap the carbon fiber reinforced polyetheretherketone CF-PEEK sheet with high-density amino functional groups grafted on the surface obtained in step 1 and the 6061 aluminum alloy sheet with functional block copolymer coating cured on the surface obtained in step 2, with an overlap width of 20 mm. Perform laser connection under the following process parameters: laser power: 850 W, defocus: +6 mm, laser scanning speed: 0.8 m / min, welding length: 30 mm, interface clamping pressure: 0.3 MPa, laser scanning surface: 6061 aluminum alloy surface; chemical bonding is completed during the laser connection process to obtain a thermal connection joint between 6061 aluminum alloy and carbon fiber reinforced polyetheretherketone CF-PEEK.
[0078] Example 4
[0079] This embodiment provides a method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material.
[0080] In this embodiment, the thermoplastic composite material to be connected is a carbon fiber reinforced polyetheretherketone CF-PEEK plate, and the plate size is 50 mm long, 30 mm wide, and 2 mm thick. Before implementing the grafting regulation, the carbon fiber reinforced polyetheretherketone (CF-PEEK) is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the cleaned carbon fiber reinforced polyetheretherketone (CF-PEEK) plate is placed in an 80°C drying oven for 2 hours for standby use.
[0081] The chemical structural formula of the functional block copolymer in this embodiment is:
[0082]
[0083] In the chemical structure formula, n=40, m=10.
[0084] In this embodiment, the metal to be connected is an AZ31B magnesium alloy plate, and the plate size is 50 mm long, 30 mm wide, and 1.5 mm thick. Before implementing the coating control, the AZ31B magnesium alloy plate is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the AZ31B magnesium alloy plate is pickled in a mixed acid solution of 80% deionized water + 15% hydrochloric acid + 5% hydrofluoric acid for 1 minute and then blown dry for standby use.
[0085] The method for directional induction of high-density chemical bonding on both sides of the thermal connection interface between metal and thermoplastic composite material in this embodiment includes the following steps:
[0086] Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials:
[0087] The carbon fiber reinforced polyetheretherketone CF-PEEK sheet was placed in a 200ml toluene solution containing 0.4g azobisisobutyronitrile and stirred at 80°C for 1h to generate active points on the surface of the thermoplastic composite material. 0.2mol methyl acrylate was added dropwise to the obtained mixed system and stirred continuously to graft polymethyl acrylate onto the surface of the carbon fiber reinforced polyetheretherketone CF-PEEK sheet. The carbon fiber reinforced polyetheretherketone CF-PEEK sheet with polymethyl acrylate grafted on the surface was taken out and placed in 200ml anhydrous ethanol and 0.2mol ethylenediamine was added dropwise. It was stirred at 50°C for 24h to cause aminolysis reaction to introduce amino groups, and a carbon fiber reinforced polyetheretherketone CF-PEEK sheet with uniformly distributed polymerized high-density amino functional groups grafted on the surface was obtained.
[0088] Step 2: Coating the functional block copolymer on the metal surface:
[0089] The functional block copolymer and the catalyst dibutyltin dilaurate are dissolved in tetrahydrofuran, and the mixture is fully mixed and stirred to obtain a functional block copolymer modified solution. The concentration of the functional block copolymer in the functional block copolymer modified solution is 0.01 mol / mL, and the concentration of the dibutyltin dilaurate is 0.005 g / ml.
[0090] The functional block copolymer modified solution was sprayed onto the surface of the AZ31B magnesium alloy sheet, and after high-temperature drying at 80°C, a directional control coating with a thickness of 500 nm was obtained. The AZ31B magnesium alloy sheet with the block copolymer coating cured on the surface was obtained by drying at room temperature for 24 hours.
[0091] Step 3. Tightly overlap the carbon fiber reinforced polyetheretherketone CF-PEEK sheet with high-density amino functional groups grafted on the surface obtained in step 1 and the AZ31B magnesium alloy sheet with functional block copolymer coating cured on the surface obtained in step 2, with an overlap width of 20 mm. Perform laser connection under the following process parameters: laser power: 850 W, defocus: +6 mm, laser scanning speed: 0.8 m / min, welding length: 30 mm, interface clamping pressure: 0.3 MPa, laser scanning surface: AZ31B magnesium alloy surface; chemical bonding is completed during the laser connection process to obtain a thermal connection joint between AZ31B magnesium alloy and carbon fiber reinforced polyetheretherketone CF-PEEK.
[0092] Comparative Example
[0093] In this comparative example, TC4 titanium alloy and carbon fiber reinforced polyetheretherketone (CF-PEEK) sheet are directly connected by laser.
[0094] The thermoplastic composite material to be connected in this comparative example is a carbon fiber reinforced polyetheretherketone CF-PEEK plate, and the plate size is 50 mm long, 30 mm wide, and 2 mm thick. Before implementing the grafting regulation, the carbon fiber reinforced polyetheretherketone (CF-PEEK) is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the cleaned carbon fiber reinforced polyetheretherketone (CF-PEEK) plate is placed in an 80°C drying oven for 2 hours for standby use.
[0095] The metal to be connected in this comparative example is a TC4 titanium alloy plate, and the plate size is 50 mm long, 30 mm wide, and 1.5 mm thick. Before implementing the coating regulation, the TC4 titanium alloy plate is cleaned in a mixed solution of acetone and alcohol for 60 seconds to remove surface oil stains, and then the TC4 titanium alloy plate is pickled in a mixed acid solution of 80% deionized water + 15% hydrochloric acid + 5% hydrofluoric acid for 1 minute and then blown dry for standby use.
[0096] The TC4 titanium alloy and carbon fiber reinforced polyetheretherketone CF-PEEK plates are tightly overlapped with an overlap width of 20 mm; laser connection is performed under the following process parameters: laser power: 850 W, defocus: +6 mm, laser scanning speed: 0.8 m / min, welding length: 30 mm, interface clamping pressure: 0.3 MPa, laser scanning surface: TC4 titanium alloy surface; a thermal connection joint between TC4 titanium alloy and carbon fiber reinforced polyetheretherketone (CF-PEEK) is obtained through the laser connection process.
[0097] The tensile shear strength of the thermal connection joints obtained in Example 1, Example 2 and the comparative example was tested, and the results are as follows: Figure 4 And as shown in Table 1.
[0098] Table 1
[0099] Control plan Joint shear strength (N) Comparative Example 1024 Example 1 2551 Example 2 3003 Example 3 1875 Example 4 2076
[0100] pass Figure 4 It can be seen that compared with the 1024N shear strength of the TC4 / CF-PPEK joint in the untreated state in the comparative example, after the thermal connection interface is regulated by the double-sided high-density chemical bonding directional induction method of the metal and thermoplastic composite thermal connection interface provided in Example 1, the joint shear strength is increased by 149% to 2551N. This shows that the chemically bonded bridge structure formed by the CN bond formed by the reaction of the epoxy group and the amino group (-NH2) introduced on the surface of CF-PPEK and TC4, the Si-O-Ti bond, and the thermal connection process of the interface realizes the directional induction of the double-sided chemical bonding of the interface, and the high-density characteristics of the polymer structure make the joint strength significantly improved. By comparing the tensile strength of the TC4 / CF-PPEK joint regulated in Example 1, the tensile strength of the TC4 / CF-PPEK joint regulated in Example 2 is increased to 3003N, which is 193% higher than the joint strength obtained in the comparative example. This shows that with the increase of the initiating active points, the bonding density of the interface increases, the bonding probability per unit area increases, the interface bonding strength increases, and the interface regulation effect is significantly improved.
Claims
1. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite materials, characterized in that: The steps include: Step 1: Grafting high-density amino functional groups on the surface of thermoplastic composite materials: Step 2: Coating the functional block copolymer on the metal surface: Step 3: Assemble the thermoplastic composite material with high-density amino functional groups grafted on the surface obtained in step 1 and the metal with functional block copolymer coating cured on the surface obtained in step 2 in an overlapping manner, complete chemical bonding during the thermal connection process, and obtain a thermal connection joint between the metal and the thermoplastic composite material.
2. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 1, characterized in that: The thermoplastic composite material in step 1 is a polyetheretherketone-based thermoplastic composite material, specifically one of polyetheretherketone monomer, carbon fiber reinforced polyetheretherketone or glass fiber reinforced polyetheretherketone.
3. A method for directional induction of double-sided high-density chemical bonding at a thermal connection interface between a metal and a thermoplastic composite material according to claim 1 or 2, characterized in that: The specific method of grafting in step 1 is as follows: placing the thermoplastic composite material in a toluene solution containing azobisisobutyronitrile, stirring at 80°C for 1 hour, dropping methyl acrylate into the obtained mixed system and continuously stirring to obtain a thermoplastic composite material with surface grafted polymethyl acrylate, placing the obtained thermoplastic composite material with surface grafted polymethyl acrylate in anhydrous ethanol and dropping a certain amount of ethylenediamine, stirring at 50°C for 24 hours to obtain a thermoplastic composite material with uniformly distributed polymerized high-density amino functional groups grafted on the surface.
4. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 3, characterized in that: The mass volume ratio of the azobisisobutyronitrile to the toluene solution is 0.2g:100mL-2g:100mL, the molar volume ratio of the methyl acrylate to the toluene solution in the mixed system is 0.05mol:100mL-2mol:100mL, and the molar volume ratio of the ethylenediamine to the ethanol solution is 0.05mol:100mL-2mol:100mL.
5. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 4, characterized in that: The chemical structural formula of the functional block copolymer in step 2 is: In the chemical structural formula, n=10-1000, and m=n×(5-50%).
6. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 5, characterized in that: The specific method of coating the functional block copolymer on the metal surface in step 2 is: dissolving the functional block copolymer and the catalyst in an organic solvent to obtain a functional block copolymer modified solution, spraying the functional block copolymer modified solution onto the metal surface to be connected, and drying at room temperature for 24 hours to obtain a metal with a block copolymer coating cured on the surface.
7. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 6, characterized in that: The catalyst is one of dibutyltin dilaurate or stannous octoate, and the organic solvent is one of dichloromethane, tetrahydrofuran, toluene or chloroform.
8. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 7, characterized in that: The concentration of the functional block copolymer in the functional block copolymer modification solution is 0.001-0.1 mol / mL, and the concentration of the catalyst in the functional block copolymer modification solution is 0.001-0.1 g / ml.
9. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 8, characterized in that: The metal to be connected is one of titanium alloy, stainless steel, aluminum alloy or magnesium alloy, and the thickness of the block copolymer coating cured on the metal surface is 50 to 1000 nm.
10. A method for directional induction of double-sided high-density chemical bonding at the thermal connection interface of metal and thermoplastic composite material according to claim 9, characterized in that: The thermal connection in step 3 is one of laser connection, friction stir connection, hot pressing connection, resistance welding or induction connection.
Citation Information
Cited By
Preparation and regulation method of chemical regulation block copolymer applied to thermal connection interface of metal and thermoplastic composite material
CN117402305A
Preparation of a chemical-regulating block copolymer applied to the thermal connection interface of metal and thermoplastic composite material and regulating method thereof
CN117402305B
Connecting material, preparation method thereof, bolt and application
CN119859800A
A connecting material, its preparation method, a bolt and applications
CN119859800B
Metal surface high bonding strength polymer additive manufacturing method
CN121178868A