Composite film, preparation method thereof and photovoltaic module

By using a composite film with a multi-layer functional structure in the photovoltaic module, including a barrier layer and a high-reflective layer, the problem of colorant migration and glue overflow in black photovoltaic modules under high temperature and humidity is solved, and the output power and service life of the photovoltaic module are improved. , while improving aesthetic appearance and reflectivity.

CN118744576AActive Publication Date: 2024-10-08SUZHOU FIRST PV MATERIAL CO LTD

Patent Information

Application Number
CN202410928388.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-08
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Under the influence of external factors such as high temperature and humidity, existing black photovoltaic modules can easily migrate colorant molecules, resulting in color differences and reduced power generation, and are prone to glue overflow problems during the lamination process.

Method used

A composite film with a multi-layer functional structure, including a barrier layer, a black high-reflective layer and a white high-reflective layer. The barrier layer is composed of a protective layer and a functional layer. The functional layer contains fluorocarbon resin, nanomaterials and curing agents. Through the nanomaterials Selection and particle size control improve barrier performance and stability, and an adhesive layer and UV absorber are provided during the lamination process to reduce the risk of glue spillage.

Benefits of technology

It effectively prevents the migration of colorant molecules, maintains the output power of photovoltaic modules, extends the service life of membrane materials, reduces the risk of glue overflow, and improves the reflectivity and aesthetic appearance of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744576A_ABST
    Figure CN118744576A_ABST
Patent Text Reader

Abstract

The invention relates to a composite film, a preparation method thereof and a photovoltaic module, and relates to the field of photovoltaic technology, the composite film comprises a barrier layer, a black high-reflection layer and a white high-reflection layer, and the water vapor transmittance of the barrier layer is less than 0.1 g / m < 2 >. Day. According to the composite film containing the multi-layer functional structure, the blocking layers with the excellent blocking effect are arranged on the black high-reflection layer and the white high-reflection layer, so that on one hand, coloring agent molecules in the black high-reflection layer can be prevented from migrating under the influence of external factors, namely, the coloring agent molecules are prevented from fading; therefore, sunlight is reflected to the upper battery piece layer, so that the photovoltaic assembly is ensured to have relatively good output power. On the other hand, the negative influence of water vapor on the lower-layer structure can be prevented, and the use environment of the black high-reflection layer and the white high-reflection layer is guaranteed, so that the stability of the black high-reflection layer and the white high-reflection layer is improved, and the effects of prolonging the service life of the membrane material and keeping the high-reflection performance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to a composite film and a preparation method thereof and a photovoltaic module. Background Art

[0002] With the development of the photovoltaic industry, various photovoltaic module products have gradually increased their requirements for product aesthetics on the basis of satisfying their high output power. In recent years, black photovoltaic modules, as a photovoltaic aesthetic component, have been widely used as packaging materials, mainly including black high-reflective adhesive films and black solar back panels, which are processed using titanium black and other organic dyes. Usually, black photovoltaic modules can absorb light above 400nm. In the process of power generation with the overall photovoltaic module, the temperature of the black photovoltaic module will increase, resulting in a 3-5% decrease in output power.

[0003] Under normal temperature and pressure, the backplane and film of the existing black photovoltaic modules can maintain a relatively stable state; however, after being laminated into photovoltaic modules, after PCT aging, water boiling aging or high temperature and humidity and UV aging, the colorant molecules in the high-reflective black film will migrate under the influence of external factors (high heat, high humidity, etc.), which will appear as color difference and fading on a macro scale. When the colorant molecules migrate to the surface of the battery or other components, it will not only affect the normal operation of other functional structures, but also greatly reduce the power generation of the overall photovoltaic module. In addition, the black high-reflective film in the black photovoltaic module is used as a packaging material, and it is also prone to glue overflow during the lamination production step. Summary of the invention

[0004] In order to solve the problem that the colorant molecules in the film may migrate under the influence of external factors and cause negative impact on photovoltaic modules, the present application provides a composite film and a preparation method thereof and a photovoltaic module.

[0005] The present application provides a composite film and a preparation method thereof and a photovoltaic module using the following technical solutions: A composite film comprising a barrier layer, a black high-reflection layer and a white high-reflection layer, wherein the water vapor transmission rate of the barrier layer is less than 0.1 g / m 2 day; The barrier layer comprises a protective layer and a functional layer, wherein the functional layer is attached to the protective layer, and the functional layer comprises, by weight, 130-150 parts of a first resin, 35-45 parts of a first nano material, and 10-20 parts of a curing agent.

[0006] By adopting the above-mentioned technical scheme, the composite film containing a multi-layer functional structure provided by the present application, by arranging a barrier layer with excellent barrier effect on the black high reflective layer and the white high reflective layer, on the one hand, it is possible to prevent the colorant molecules in the black high reflective layer from migrating under the influence of external factors, that is, to prevent the colorant molecules in the black high reflective layer from fading, thereby reflecting sunlight to the upper battery layer to ensure that the photovoltaic module as a whole has a better output power; on the other hand, the barrier layer can prevent water vapor from having a negative impact on the lower structure, that is, indirectly protect the use environment of the black high reflective layer and the white high reflective layer, thereby improving the stability of the black high reflective layer and the white high reflective layer, thereby achieving the effect of extending the service life of the film material and maintaining its high reflective performance.

[0007] In a specific embodiment, the first nanomaterial includes an organic nanomaterial and an inorganic nanomaterial, the organic nanomaterial includes modified polystyrene microspheres; the inorganic nanomaterial includes one or more of nano titanium dioxide, nano calcium carbonate, nano silicon dioxide, nano boron nitride, nano chromium oxide and nano graphene; the mass ratio of the organic nanomaterial to the inorganic nanomaterial is 1: (1.5-2.3); and / or the particle size of the first nanomaterial is 50-150nm; The first resin includes one or more of fluorocarbon resin, polyester resin, acrylic resin and epoxy resin; The curing agent includes one or more of a polyurethane curing agent, an isocyanate curing agent and an epoxy curing agent.

[0008] By adopting the above technical scheme, by selecting different types of resins, such as fluorocarbon resin, polyester resin, acrylic resin and epoxy resin, and the combination of organic and inorganic nanomaterials, a comprehensive improvement of multiple properties can be achieved in the composite film, wherein fluorocarbon resin can improve chemical corrosion resistance, polyester resin can improve wear resistance, and epoxy resin can improve mechanical strength; The composite utilization of organic nanomaterials and inorganic nanomaterials. Organic and inorganic nanomaterials each have unique properties and can play their own advantages. Organic nanomaterials such as modified polystyrene microspheres may have good flexibility and toughness, and can absorb energy when the material is subjected to external impact or deformation, thereby improving the flexibility and tensile strength of the composite material. Inorganic nanomaterials, such as nano titanium dioxide, have excellent weather resistance and can resist the erosion of natural environmental factors such as ultraviolet rays, oxidation, and deliquescence, thereby extending the service life of the composite material. The composite utilization of organic and inorganic nanomaterials can construct a complex interface structure and improve the barrier properties of the composite material. Inorganic materials such as nano titanium dioxide can form a dense barrier on the surface of the material to prevent the penetration of gas or liquid, thereby improving the barrier properties of the composite material. The optimal balance of flexibility, weather resistance and barrier properties can be achieved by reasonably adjusting the mass ratio of organic and inorganic nanomaterials. Furthermore, by controlling the particle size of the first nanomaterial to be between 50 and 150 nm, its surface area is relatively large, and it can better interact with the matrix resin. Since the particle size of the nanomaterial is small, it has a higher specific surface area and a higher surface activity, which is conducive to full contact and interaction with the resin matrix, thereby achieving better dispersibility. This good dispersibility helps prevent the agglomeration or accumulation of the nanomaterial and ensures its uniform distribution in the composite material. Moreover, within the particle size range of 50 to 150 nm, the surface activity of the nanomaterial is high, which means that there are a large number of active functional groups or defect sites on the surface of the nanomaterial, which can undergo physical or chemical adsorption with the resin matrix, thereby promoting good bonding between the two. This good interfacial activity helps to improve the interfacial strength and durability of the composite material and reduce the possibility of interfacial shear stress and interfacial separation.

[0009] In a specific embodiment, the method for preparing the modified polystyrene microspheres comprises the following steps: (1) first copolymerizing styrene with a functional monomer to obtain a modified polystyrene precursor; the functional monomer includes a monomer containing an amino group, a sulfonic acid group, and a carboxyl group; (2) The modified polystyrene precursor of step (1) is subjected to suspension polymerization to obtain the modified polystyrene microspheres.

[0010] By adopting the above technical scheme, functional monomers containing amino, sulfonic acid, carboxyl and other functional groups are added for copolymerization, and these active functional groups can be introduced on the surface of modified polystyrene microspheres. These functional groups are chemically reactive, making it easier for the surface of the microspheres to react chemically with other materials, thereby enhancing the surface activity of the modified polystyrene microspheres, so that the modified polystyrene microspheres can better react chemically or physically with other materials or systems, thereby enhancing their application performance in composite materials and the like; the introduction of amino, sulfonic acid, carboxyl and other functional groups, because these functional groups can interact with other functional groups in the matrix through hydrogen bonds, electrostatic effects, etc., thereby improving the binding between the microspheres and the matrix and compatibility, so that the compatibility between the modified polystyrene microspheres and other matrices (such as resin matrices) is enhanced, and the dispersibility and bonding of the modified polystyrene microspheres in the composite materials are improved, thereby helping to improve the performance of the composite materials, such as strength, toughness and durability; and by selecting different functional monomers, the surface functional groups of the modified polystyrene microspheres can be regulated, thereby giving the modified polystyrene microspheres different chemical properties and functions. For example, the amino group can be used to react with other materials containing acidic functional groups, the sulfonic acid group can make the modified polystyrene microspheres hydrophilic, and the carboxyl group can be used to react with alkaline substances, thereby giving the modified polystyrene microspheres more application characteristics.

[0011] In a specific embodiment, the light transmittance of the barrier layer in the wavelength range of 400-1100 nm is greater than 90%.

[0012] In a specific embodiment, the black high reflective layer includes, by weight, 140-160 parts of the second resin, 10-20 parts of the colorant, 10-20 parts of the second nanomaterial, and 1-3 parts of the cross-linking agent.

[0013] In a specific embodiment, the colorant includes dye red, dye yellow and dye blue, and / or the mass percentage of the dye red, dye yellow and dye blue is (20-25%): (40-50%): (25-30%); The second resin includes one or more of ethylene copolymer resin, propylene copolymer resin, and vinyl acetate copolymer resin; The second nanomaterial includes one or more of nano silicon dioxide and nano titanium dioxide; The crosslinking agent includes one or more of tert-butyl peroxy-2-ethylhexanoate, dipentaerythritol hexaacrylate, and propoxylated trimethylolpropane triacrylate.

[0014] In a specific embodiment, the black high reflective layer also includes a surfactant, and the surfactant includes one or more of sodium dodecylbenzene sulfonate, alkyl glucoside, fatty acid glyceride, fatty acid sorbitan, polysorbate, and sodium glycocholate; and / or the mass ratio of the surfactant to the second nanomaterial is (0.1-0.2):1.

[0015] By adopting the above technical solution, by improving the various components in the black high reflective layer, the second nanomaterial and the surfactant are coordinated with each other, so that the second nanomaterial can be evenly dispersed in the resin system mixed with the colorant, thereby improving the adhesion and compatibility of the second nanomaterial and the colorant, and to a certain extent blocking the large and small colorant molecules decomposed by the black high reflective layer during use, further preventing the problem of color migration.

[0016] In a specific embodiment, the reflectivity of the black high reflective layer to light in the wavelength range of 280-1400nm is 10%-15%; the transmittance of the black high reflective layer to ultraviolet light in the wavelength range of 280-400nm is less than 0.5%, the transmittance of the black high reflective layer to visible light in the wavelength range of 400-700nm is less than 0.5%, and the transmittance of the black high reflective layer to infrared light in the wavelength range of 760-1100nm is greater than 75%; The reflectivity of the white high-reflection layer to light in the wavelength range of 400-1200nm is greater than 95%.

[0017] In a specific embodiment, the cross-linking degree between the black high-reflection layer and the white high-reflection layer is 20%-50%.

[0018] By adopting the above technical scheme, the crosslinking degree of the black high reflective layer and the white high reflective layer is 20%-50%, which can reduce the abnormality of glue overflow in the lamination process of the composite film; the pre-crosslinking treatment of the black high reflective layer and the white high reflective layer can increase the stability and solvent resistance of the material, and the pre-crosslinking treatment helps to improve the thermal stability of the material, so that it can maintain structural stability and performance unchanged at high temperature, and reduce the glue overflow caused by thermal pressure during the lamination process. By adjusting the crosslinking degree of the black high reflective layer and the white high reflective layer between 20% and 50%, a good balance can be achieved, which not only maintains sufficient flexibility, but also improves the stability during the lamination process, thereby reducing the risk of glue overflow; the pre-crosslinking treatment can also improve the mechanical strength and wear resistance of the black high reflective layer and the white high reflective layer, thereby increasing the durability and service life of the composite film; and the pre-crosslinking treatment can also make the surface of the black high reflective layer and the white high reflective layer smoother and more uniform, improve its bonding strength with the substrate, thereby optimizing the lamination process and reducing the scrap rate in the production process.

[0019] In a specific embodiment, an adhesive layer is provided between the barrier layer and the black high-reflection layer or between the barrier layer and the white high-reflection layer, and the adhesive layer includes an ultraviolet absorber; The ultraviolet absorber includes one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, triazines, and hindered amines.

[0020] By adopting the above technical solution, by setting an adhesive layer with excellent bonding performance, the displacement of the materials on both sides of the adhesive bonding can be reduced during the lamination process, and the risk of adhesive overflow can be reduced to a certain extent; and because the protective layer of the barrier layer can be selected from PET material, the simple bonding between the adhesive film and PET is easy to be detached after conventional wet heat aging, so the barrier layer and the adhesive film must be bonded by an adhesive, and this adhesive layer can meet its use requirements. At the same time, mixing a certain amount of ultraviolet absorber into the adhesive layer can meet the actual needs of composite films with different interlayer bonding structures. On the one hand, it improves the bonding effect between the upper and lower layers; on the other hand, it can reduce the risk of ultraviolet aging of the lower film layer.

[0021] In a specific embodiment, the absorption rate of the ultraviolet cut-off layer to ultraviolet light in the wavelength range of 280-380 nm is greater than 90%; The transmittance of the adhesive layer to ultraviolet light in the wavelength range of 280-380nm is less than 5%, and the transmittance of the adhesive layer to light in the wavelength range of 400-1100nm is greater than 90%.

[0022] By adopting the above technical solution, the UV cutoff layer can effectively absorb ultraviolet rays while maintaining transparency. The UV cutoff layer can be applied to the production of objects made of photosensitive materials to prevent ultraviolet rays from damaging the objects made of photosensitive materials, thereby improving the quality and service life of the objects made of photosensitive materials.

[0023] A photovoltaic module comprises photovoltaic glass, an encapsulation film, a battery cell and a photovoltaic backboard. The photovoltaic module has the composite film as described above, and the composite film is arranged between the battery cell and the photovoltaic backboard.

[0024] By adopting the above-mentioned technical scheme, the photovoltaic module of the present application connects the battery cell and the photovoltaic backplane through a composite film, which can improve the problem of color difference in the appearance of the photovoltaic module, meet the aesthetic appearance requirements of the photovoltaic module, and can block substances such as oxygen and water vapor from "invading" the battery cell, thereby improving the overall output power of the photovoltaic module, and can improve the overall reflectivity, improve the utilization rate of the photovoltaic module for sunlight, and reduce the temperature of the photovoltaic module when generating electricity, thereby extending the service life of the photovoltaic module.

[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. The composite film with a multi-layer functional structure provided in the present application has a barrier layer with excellent barrier effect arranged on the black high-reflection layer and the white high-reflection layer. On the one hand, it can prevent the colorant molecules in the black high-reflection layer from migrating under the influence of external factors, that is, prevent the black high-reflection layer from fading, thereby reflecting the sunlight to the upper battery layer to ensure that the photovoltaic module has a good output power as a whole; on the other hand, the barrier layer can prevent water vapor from having a negative impact on the lower structure, that is, indirectly protect the use environment of the black high-reflection layer and the white high-reflection layer, thereby improving the stability of the black high-reflection layer and the white high-reflection layer, thereby achieving the effect of extending the service life of the film material and maintaining its high reflective performance; 2. The composite film of the present application can be suitable for the application of photovoltaic modules. By connecting the battery cell and the photovoltaic backplane through the composite film, the problem of color difference in the appearance of the photovoltaic module can be improved, which meets the aesthetic appearance requirements of the photovoltaic module. It can also block substances such as oxygen and water vapor from "invading" the battery cell, thereby improving the overall output power of the photovoltaic module, and can improve the overall reflectivity, improve the utilization rate of the photovoltaic module for sunlight, and reduce the temperature of the photovoltaic module when generating electricity, thereby extending the service life of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the structure of the composite membrane in Example 1 of the present application.

[0027] Explanation of the accompanying drawings: 1. barrier layer; 11. protective layer; 12. functional layer; 2. black high reflective layer; 3. white high reflective layer; 4. ultraviolet cutoff layer; 5. adhesive layer. DETAILED DESCRIPTION

[0028] The following is combined with Figure 1 This application is described in further detail.

[0029] Reference Figure 1 The present application discloses a composite film, which includes but is not limited to being applied to the encapsulation of photovoltaic modules. As an optional embodiment, the composite film includes an ultraviolet cutoff layer 4, a barrier layer 1, a black high-reflection layer 2 and a white high-reflection layer 3 arranged in order from top to bottom; the water vapor transmission rate of the barrier layer 1 is less than 0.1g / m 2 day; The composite film containing a multi-layer functional structure provided in the present application is provided with a barrier layer 1 with excellent barrier effect on the upper layer of the black high reflective layer 2 and the white high reflective layer 3. On the one hand, it can prevent the colorant molecules in the black high reflective layer 2 from migrating under the influence of external factors, that is, prevent itself from fading, and at the same time prevent negative impact on the performance of other layers, that is, prevent itself from fading, thereby preventing negative impact on photovoltaic modules, thereby ensuring that the performance and quality of the entire composite film are effectively maintained and the performance is improved; on the other hand, the barrier layer 1 can prevent water vapor from having a negative impact on the underlying structure, that is, indirectly protect the use environment of the black high reflective layer 2 and the white high reflective layer 3, thereby improving the physical stability of the black high reflective layer 2 and the white high reflective layer 3, thereby achieving the effect of extending the service life of the film material and maintaining its high reflective performance.

[0030] The absorption rate of the ultraviolet cutoff layer 4 to ultraviolet light in the wavelength range of 280-380nm is greater than 90%, the transmittance of the ultraviolet cutoff layer 4 to ultraviolet light in the wavelength range of 280-380nm is less than 5%, and the transmittance of the ultraviolet cutoff layer 4 to light in the wavelength range of 400-1100nm is greater than 90%; the ultraviolet cutoff layer 4 is a film layer with high cutoff of ultraviolet light, and the thickness of the ultraviolet cutoff layer 4 is 200-400μm.

[0031] The material of the ultraviolet cutoff layer 4 includes but is not limited to using a polymer as a base material, for example, the polymer includes polyimide, polyester, and polypropylene, and the additive with ultraviolet cutoff function includes but is not limited to being made of one of organic materials or silicon-based materials. Specifically, organic materials such as benzimidazole, dihydropyran and other compounds have good ultraviolet absorption performance and can be used to prepare the ultraviolet cutoff layer 4; silicon-based materials such as nanocrystalline silicon, silicon dioxide and other materials have strong ultraviolet absorption ability and can be used to prepare the ultraviolet cutoff layer 4; The UV cutoff layer 4 can effectively absorb ultraviolet rays while maintaining transparency. Its main function is to prevent harmful, high-energy ultraviolet rays from entering the photosensitive material, thereby preventing the photosensitive material from rapidly aging. The UV cutoff layer 4 can be applied to the production of photosensitive material components to prevent ultraviolet rays from damaging components made of photosensitive materials, thereby improving the quality and service life of photovoltaic components.

[0032] The barrier layer 1 includes a protective layer 11 and a functional layer 12 attached to the protective layer 11, the light transmittance of the barrier layer 1 in the wavelength range of 400-1100nm is greater than 90%; the functional layer 12 is coated on the protective layer 11 with a coating thickness of 5-30μm, the protective layer 11 includes but is not limited to a PET layer, the functional layer 12 includes 130-150 parts of a first resin, 35-45 parts of a first nanomaterial and 10-20 parts of a curing agent, and the thickness of the barrier layer 1 is 10-20μm; The first resin includes one or more of fluorocarbon resin, polyester resin, acrylic resin and epoxy resin; by selecting different types of resins, such as fluorocarbon resin, polyester resin, acrylic resin and epoxy resin, and the combination of organic and inorganic nanomaterials, a comprehensive improvement of multiple properties can be achieved in the composite film, wherein fluorocarbon resin can improve chemical corrosion resistance, polyester resin can improve wear resistance, and epoxy resin can improve mechanical strength; The first nanomaterial includes organic nanomaterials and inorganic nanomaterials; Organic nanomaterials include modified polystyrene microspheres. The main skeleton of polystyrene microspheres is composed of benzene rings. Benzene rings have high chemical reactivity. Through appropriate reaction conditions, such as aromatization reaction, alkylation reaction, etc., different functional groups can be introduced on the benzene rings, thereby changing the properties and functions of polystyrene microspheres. The olefin double bond in polystyrene microspheres is also an active center for chemical reactions. Through the ring-opening reaction and addition reaction of the olefin double bond, various functional groups, such as carboxyl, amino, hydroxyl, etc., can be introduced, thereby changing the chemical properties and surface characteristics of polystyrene microspheres. The preparation method of modified polystyrene microspheres comprises the following steps: (1) firstly copolymerizing styrene with a functional monomer to obtain a modified polystyrene precursor; the functional monomer includes a monomer containing an amino group, a sulfonic acid group, and a carboxyl group; (2) The modified polystyrene precursor of step (1) is subjected to suspension polymerization to obtain modified polystyrene microspheres.

[0033] Functional monomers containing amino, sulfonic acid, carboxyl and other functional groups are added for copolymerization, and these active functional groups can be introduced on the surface of modified polystyrene microspheres. These functional groups are chemically reactive, making it easier for the surface of the microspheres to react chemically with other materials, thereby enhancing the surface activity of the modified polystyrene microspheres, allowing the modified polystyrene microspheres to better react chemically or physically with other materials or systems, thereby enhancing their application performance in composite materials and the like; The introduction of functional groups such as amino, sulfonic acid, and carboxyl groups can improve the binding and compatibility between the microspheres and the matrix because these functional groups can interact with other functional groups in the matrix through hydrogen bonds, electrostatic effects, etc., thereby enhancing the compatibility between the modified polystyrene microspheres and other matrices (such as resin matrices), improving the dispersibility and binding of the modified polystyrene microspheres in composite materials, and thus helping to improve the properties of the composite materials, such as strength, toughness, and durability. In addition, by selecting different functional monomers, the surface functional groups of the modified polystyrene microspheres can be regulated, thereby giving the modified polystyrene microspheres different chemical properties and functions. For example, amino groups can be used to react with other materials containing acidic functional groups, sulfonic acid groups can make the modified polystyrene microspheres hydrophilic, and carboxyl groups can be used to react with alkaline substances, thereby giving the modified polystyrene microspheres more application characteristics.

[0034] The inorganic nanomaterial includes one or more of nano titanium dioxide, nano calcium carbonate, nano silicon dioxide, nano boron nitride, nano chromium oxide and nano graphene. Preferably, the inorganic nanomaterial is nano titanium dioxide; the mass ratio of the organic nanomaterial to the inorganic nanomaterial is 1:(1.5-2.3); and / or the particle size of the first nanomaterial is 50-150nm; The composite utilization of organic nanomaterials and inorganic nanomaterials. Organic and inorganic nanomaterials each have unique properties and can play their own advantages. Organic nanomaterials such as modified polystyrene microspheres may have good flexibility and toughness, and can absorb energy when the material is subjected to external impact or deformation, thereby improving the flexibility and tensile strength of the composite material. Inorganic nanomaterials, such as nano titanium dioxide, have excellent weather resistance and can resist the erosion of natural environmental factors such as ultraviolet rays, oxidation, and deliquescence, thereby extending the service life of the composite material. The composite utilization of organic and inorganic nanomaterials can construct a complex interface structure and improve the barrier properties of the composite material. Inorganic materials such as nano titanium dioxide can form a dense barrier on the surface of the material to prevent the penetration of gas or liquid, thereby improving the barrier properties of the composite material. The optimal balance of flexibility, weather resistance and barrier properties can be achieved by reasonably adjusting the mass ratio of organic and inorganic nanomaterials. Furthermore, by controlling the particle size of the first nanomaterial to be between 50 and 150 nm, its surface area is relatively large, and it can better interact with the matrix resin. Since the particle size of the nanomaterial is small, it has a higher specific surface area and a higher surface activity, which is conducive to full contact and interaction with the resin matrix, thereby achieving better dispersibility. This good dispersibility helps prevent the agglomeration or accumulation of the nanomaterial and ensures its uniform distribution in the composite material. Moreover, within the particle size range of 50 to 150 nm, the surface activity of the nanomaterial is high, which means that there are a large number of active functional groups or defect sites on the surface of the nanomaterial, which can undergo physical or chemical adsorption with the resin matrix, thereby promoting good bonding between the two. This good interfacial activity helps to improve the interfacial strength and durability of the composite material and reduce the possibility of interfacial shear stress and interfacial separation.

[0035] The thickness of the black high reflective layer 2 is 20-100 μm. The black high reflective layer 2 includes, by weight, 140-160 parts of a second resin, 10-20 parts of a colorant, 10-20 parts of a modified nanomaterial, and 1-3 parts of a crosslinking agent. The second resin includes but is not limited to ethylene-vinyl acetate copolymer, ethylene-α-olefin copolymer, ethylene-methyl methacrylate copolymer, ethylene-methacrylic acid ionomer, low-density polyethylene, polypropylene, polybutylene, polyvinyl butyral, and silicone material. The colorant includes dye red, dye yellow and dye blue, wherein the mass ratio of dye red: dye yellow: dye blue is (20-25%): (40-50%): (25-30%), and the color is adjusted to black according to the principle of three primary colors; The second nanomaterial includes nano silicon dioxide and nano titanium dioxide; The crosslinking agent includes one or more of tert-butyl peroxy-2-ethylhexanoate, dipentaerythritol hexaacrylate, and propoxylated trimethylolpropane triacrylate; The black high reflective layer 2 also includes a surfactant, which includes one or more of sodium dodecylbenzene sulfonate, alkyl glucoside, fatty acid glyceride, fatty acid sorbitan, polysorbate, and sodium glycocholate; the mass ratio of the surfactant to the second nanomaterial is (0.1-0.2): 1; By improving the various components in the black high reflective layer 2, the second nanomaterial and the surfactant are matched with each other, so that the second nanomaterial can be evenly dispersed in the resin system mixed with the colorant, thereby improving the adhesion and compatibility of the second nanomaterial and the colorant, and to a certain extent blocking the large and small colorant molecules decomposed by the black high reflective layer 2 during use, further preventing the problem of color migration.

[0036] The reflectivity of the black high reflective layer 2 to light in the wavelength range of 280-1400nm is 10%-15%; the transmittance of the black high reflective layer 2 to ultraviolet light in the wavelength range of 280-400nm is less than 0.5%, the transmittance of the black high reflective layer 2 to visible light in the wavelength range of 400-700nm is less than 0.5%, and the transmittance of the black high reflective layer 2 to infrared light in the wavelength range of 760-1100nm is greater than 75%; In order to improve the weather resistance and mechanical properties of the black high reflective layer 2 , including but not limited to adding plasticizers or antioxidants, plasticizers can improve the flexibility and toughness of the copolymer, and antioxidants can prevent material aging and degradation, thereby extending the service life of the black high reflective layer 2 .

[0037] The reflectivity of the white high-reflection layer 3 in the wavelength range of 400-1200 is greater than 95%; the thickness of the white high-reflection layer 3 is 50-250μm, and the white high-reflection layer 3 is made of inorganic filler titanium dioxide dispersed in ethylene-vinyl acetate copolymer. In order to ensure the reflectivity of the white high-reflection layer 3, the filler content of the inorganic filler titanium dioxide includes but is not limited to 10%-30%, which can improve the reflectivity of the white high-reflection layer 3 and ensure that the light transmittance of the film is still high enough; through the white high-reflection layer 3 made of the above material, the light has a higher reflectivity after passing through the black high-reflection layer 2 in the white high-reflection layer 3, further improving the reflectivity of the entire composite film.

[0038] The overall cross-linking degree of the black high reflective layer 2 and the white high reflective layer 3 is 20%-50%; the cross-linking degree of the black high reflective layer 2 and the white high reflective layer 3 is 20%-50%, which can reduce the abnormality of glue overflow during the lamination process of the composite film; the pre-cross-linking treatment of the black high reflective layer 2 and the white high reflective layer 3 can increase the stability and solvent resistance of the material. The pre-cross-linking treatment helps to improve the thermal stability of the material, so that it can maintain structural stability and performance unchanged at high temperatures, and reduce the glue overflow caused by thermal pressure during the lamination process. By regulating the black high reflective layer 2 and the white The degree of cross-linking of the high reflective layer 3 is between 20% and 50%, which can achieve a good balance, maintaining sufficient flexibility while improving stability during the lamination process, thereby reducing the risk of glue overflow; the pre-cross-linking treatment can also improve the mechanical strength and wear resistance of the black high reflective layer 2 and the white high reflective layer 3, thereby increasing the durability and service life of the composite film; and the pre-cross-linking treatment can also make the surface of the black high reflective layer 2 and the white high reflective layer 3 smoother and more uniform, and improve its bonding strength with the substrate, thereby optimizing the lamination process and reducing the scrap rate in the production process.

[0039] The barrier layer 1 is provided with an adhesive layer 5 on one side close to the ultraviolet cut-off layer 4 and the black high-reflection layer 2, and the adhesive layer 5 includes an ultraviolet absorber; the adhesive resin used in the adhesive layer 5 can be selected from one of polyolefin resins and polyester resins, or a combination of the two; The ultraviolet absorber includes one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, triazines, and hindered amines; The adhesive layer 5 does not require a drying oven to remove the solvent, is energy-saving and environmentally friendly, has high production efficiency, and can be laminated on both sides at the same time; and has good bonding performance, can reduce the displacement of materials on both sides of the adhesive during the lamination process, and reduce the risk of adhesive overflow to a certain extent; and because the protective layer 11 of the barrier layer 1 can be made of PET material, the simple bonding between the adhesive film and PET is easy to detach after conventional wet and hot aging, so the barrier layer 1 and the adhesive film must be bonded by an adhesive, and this adhesive layer 5 can meet its use requirements.

[0040] The composite film containing a multi-layer functional structure provided in the present application is provided with a barrier layer 1 with excellent barrier effect on the black high-reflection layer 2 and the white high-reflection layer 3. On the one hand, it can prevent the colorant molecules in the black high-reflection layer 2 from migrating under the influence of external factors, that is, prevent itself from fading, thereby reflecting sunlight to the upper battery layer to ensure that the photovoltaic module as a whole has a good output power; on the other hand, the barrier layer 1 can prevent water vapor from having a negative impact on the lower structure, that is, indirectly protect the use environment of the black high-reflection layer 2 and the white high-reflection layer 3, thereby improving the stability of the black high-reflection layer 2 and the white high-reflection layer 3, thereby achieving the effect of extending the service life of the film material and maintaining its high reflective performance.

[0041] The present application provides a method for preparing a composite film, which adopts the following technical solution: S1: S10, the raw materials required for preparing the black high reflective layer 2 are melt co-extruded to form a film, so as to prepare the black high reflective layer 2; the raw materials required for preparing the white high reflective layer 3 are melt co-extruded to form a film, so as to prepare the white high reflective layer 3; the prepared black high reflective layer 2 and the prepared white high reflective layer 3 are then bonded together and formed, and subjected to radiation cross-linking treatment; specifically, including but not limited to adding fillers in the co-extrusion process, for the black high reflective layer 2, adding an organic dye dispersed in ethylene-vinyl acetate copolymer in an extruder, and for the white high reflective layer 3, adding an inorganic filler titanium dioxide dispersed in ethylene-vinyl acetate copolymer in an extruder, and the extruder melts the above-mentioned multiple materials; By realizing the black high reflective layer 2 and the white high reflective layer 3 on the same film, in the co-extrusion process, by controlling the material combination and thickness of different layers, specifically, controlling the thickness of the black high reflective layer 2 to 20-100 μm, and controlling the thickness of the white high reflective layer 3 to 50-250 μm, the desired black and white reflective characteristics can be achieved.

[0042] S20. The integrally formed black high reflective layer 2 and the white high reflective layer 3 are subjected to radiation cross-linking treatment to improve their thermal stability, mechanical properties and chemical stability, so that the overall cross-linking degree of the black high reflective layer 2 and the white high reflective layer 3 is between 20-50%; the radiation cross-linking of the black high reflective layer 2 and the white high reflective layer 3 includes but is not limited to the use of electron beam irradiation or gamma ray irradiation equipment, and the radiation dose applied during the irradiation of the black high reflective layer 2 and the white high reflective layer 3 includes but is not limited to 10-50 kGy. In actual operation, experiments can be conducted to determine the appropriate irradiation dose and treatment conditions.

[0043] S2, preparing a coating liquid for the functional layer 12, and then coating or evaporating the coating liquid onto the surface of the protective layer 11 to obtain the barrier layer 1; The specific steps of the coating method include: a. preparing 130-150 parts of the first resin, 35-45 parts of the first nanomaterial and 10-20 parts of the curing agent as raw materials for preparing the coating liquid, mixing and stirring to ensure that the components are fully and evenly mixed together to prepare the functional layer 12 coating liquid; b. coating: placing the PET protective layer 11 on a flat surface, and using a coating process to evenly coat the functional layer 12 coating liquid on the surface of the PET protective layer 11, including but not limited to coating by dipping, scraping or spraying; c. drying and curing: drying the coated PET protective layer 11 so that the barrier material forms a dense film structure, including but not limited to curing by natural drying, oven drying or heat treatment to form a barrier layer 1.

[0044] The specific steps of the evaporation method include: a. preparing 130-150 parts of the first resin, 35-45 parts of the first nanomaterial and 10-20 parts of the curing agent as raw materials for preparing the coating liquid, mixing and stirring to ensure that the components are fully and evenly mixed together to prepare the functional layer 12 evaporation liquid; b. evaporation: placing the PET protective layer 11 in a vacuum evaporation equipment, heating it to a certain temperature and generating sufficient vacuum, and then heating the functional layer 12 evaporation liquid to the evaporation temperature, so that it evaporates and deposits on the surface of the PET protective layer 11 to form a barrier layer 1, thereby making a barrier layer 1.

[0045] S3, preparing adhesive solution for adhesive layer 5, and using adhesive layer 5 to respectively bond the UV cutoff layer 4 and the black surface of the integrally formed black high reflective layer 2 and the white high reflective layer 3 to both sides of the barrier layer 1 in a solvent-free composite production line, and pressing and forming; The specific steps include: a. cleaning treatment, cleaning the surfaces of the UV cutoff layer 4 and the integrated black high reflective layer 2 and the white high reflective layer 3 to be bonded, ensuring that they are free of dust, oil and other impurities; b. adhesive coating, coating the adhesive layer 5 on both sides of the barrier layer 1, including but not limited to spraying, rolling or brushing; c. bonding the black surfaces of the UV cutoff layer 4 and the integrated black high reflective layer 2 and the white high reflective layer 3 to both sides of the barrier layer 1 coated with the adhesive, ensuring accurate positioning during bonding to avoid problems such as bubbles or misalignment; d. pressing and molding, placing the bonded materials in a pressing device and pressing and molding them, during which appropriate parameters such as temperature, pressure and time are set according to specific requirements and material properties.

[0046] S4, placing the multi-layered film layer pressed in S3 into a curing room at 20-35° C. for 20-30 hours to allow the adhesive to react completely, and a composite film is obtained after the curing is completed; The specific steps include: a. Prepare the curing room and ensure that the temperature in the curing room is controlled within the range of 20-35℃. A constant temperature box or other temperature control equipment can be used to maintain the required temperature; b. Place the film layer and put the pressed film layer into the curing room. Be careful not to stack or press the film layer to avoid affecting the curing effect; c. Set the curing time to 20-30 hours based on experience and actual conditions, and regularly check the temperature and humidity in the curing room during the curing process to ensure the stability of the curing conditions; d. After waiting for the curing time to end, take the film layer out of the curing room. At this time, the adhesive has fully reacted to form a composite film.

[0047] In the above preparation process, the order of S1, S2, S3, and S4 can be interchanged.

[0048] The present application also provides a photovoltaic module, the photovoltaic module having the above-mentioned composite film; the photovoltaic module comprises photovoltaic glass, an encapsulation film, a battery cell and a photovoltaic backplane, and the composite film is arranged between the battery cell and the photovoltaic backplane; The photovoltaic module of the present application connects the battery cell and the photovoltaic backplane through a composite film, which can improve the problem of color difference in the appearance of the photovoltaic module, meet the aesthetic appearance requirements of the photovoltaic module, and can block substances such as oxygen and water vapor from "invading" the battery cell, thereby improving the overall output power of the photovoltaic module, and can improve the overall reflectivity, improve the utilization rate of the photovoltaic module for sunlight, and reduce the temperature of the photovoltaic module when generating electricity, thereby extending the service life of the photovoltaic module.

[0049] Example The present application provides a composite membrane, such as Figure 1 As shown, from top to bottom, an ultraviolet cutoff layer 4, an (upper layer) adhesive layer 2, a protective layer 11, a functional layer 12, a (lower layer) adhesive layer 2, a black high reflective layer 2 and a white high reflective layer 3 are sequentially arranged, wherein the raw materials for preparing each layer are shown in Table 1 below.

[0050] A detailed description of the components used in Examples 1-10 is as follows: Functional layer: (A) First resin (A1) polyester resin (Nanya Plastics Industries, NPSN resin), (A2) acrylic resin (Zhejiang Lihuo New Materials Technology Co., Ltd., LHC1011 resin).

[0051] (B) The first nanomaterial (B1) Organic nanomaterials: modified polystyrene microspheres.

[0052] (B2) Inorganic nanomaterials: (B21) Nano-titanium dioxide (Zhejiang Zhitai Nano-Micro New Materials Co., Ltd., ZT-T60), (B22) Nano-calcium carbonate (Zhejiang Changshan Jinxiong Co., Ltd., CCR nano-calcium carbonate), (B23) Nano-silicon dioxide (Zhejiang Zhitai Nano-Micro New Materials Co., Ltd., ZT-SP30T).

[0053] (C) Curing agent (C1) Polyurethane curing agent (Asahi Kasei, TPA-90SB curing agent), (C2) Isocyanate curing agent (Covestro Polymers Co., Ltd., N3400 curing agent), (C3) Epoxy curing agent (Wanhua Chemical, WH-602).

[0054] Black High Reflective Layer: (D) Second resin (D1) Ethylene copolymer resin (Total 282PV photovoltaic EVA resin from South Korea), (D2) Vinyl acetate copolymer resin (Lianhong UL00428 from Shandong Province).

[0055] (E) Colorant (E1) Dye red (Clariant D3G70), (E2) Dye yellow (Clariant H3G), (E3) Dye blue (Clariant A2R).

[0056] (F) Second nanomaterial (F1) Nano-silicon dioxide (Zhejiang Zhitai Nano-Micro New Materials Co., Ltd., ZT-SP30T), (F2) Nano-titanium dioxide (Zhejiang Zhitai Nano-Micro New Materials Co., Ltd., ZT-T60).

[0057] (G) Cross-linking agent (G1) tert-butyl peroxy-2-ethylhexanoate, (G2) dipentaerythritol hexaacrylate.

[0058] (H) Surfactant (H1) Sodium dodecylbenzene sulfonate, (H2) Fatty acid glycerides.

[0059] Table 1 Comparative Example Comparative Example 1 This comparative example provides a composite film, which is different from Example 1 in that no organic nanomaterial is added to the first nanomaterial of the functional layer; Comparative Example 2 This comparative example provides a composite film, which is different from Example 1 in that the mass ratio of the organic nanomaterial to the inorganic nanomaterial in the first nanomaterial of the functional layer is 3:1; Comparative Example 3 This comparative example provides a composite film, which is different from Example 1 in that the mass ratio of the surfactant to the second nanomaterial in the black high reflective layer is 1:1; Comparative Example 4 This comparative example provides a composite film, which is different from Example 1 in that, in the preparation method, in step S1, no radiation cross-linking treatment is performed between the black high-reflection layer and the white high-reflection layer.

[0060] Performance testing The following performance tests were performed on the composite films prepared in Examples 1-10 and Comparative Examples 1-4. The test results are shown in Table 2 below.

[0061] Test method: 1. Water vapor transmission rate: The barrier layers in each embodiment and comparative example were tested according to ASTM-F1249 "Standard Test Method for Water Vapor Transmission Rate of Plastic Film and Sheet"; 2. Reflectivity test: Tested in accordance with ASTM-17 "Test Method for Solar Energy Transmission and Reflection of Thin Sheet Materials"; 3. Photovoltaic module appearance test: The test was conducted in accordance with IEC 61215 "Identification and finalization of terrestrial crystalline silicon photovoltaic modules". The test conditions were: 85°C, 85% humidity, 2000h. The appearance of the photovoltaic modules was monitored before and after the damp heat aging test. The composite film layer was visually inspected for pigment agglomeration and precipitation. 4. Test of peel strength between conventional backsheet and composite film of the present application: According to the GB / T2790 adhesive 180° peel strength test method, the flexible material is tested on the rigid material; The peel strength between the back sheet and the composite film of the present application was tested at 85°C, 85% humidity, and 2000 hours, and the black high reflective layer of the composite film layer was visually inspected to see if it faded or had color migration.

[0062] Table 2 Combined with the above Tables 1 and 2, the composite films of Examples 1-10 all have good water-blocking properties, and the color of the black high-reflection layer does not change after the aging test at 85°C, 85% humidity, and 2000h, indicating that the composite film is added with the above-mentioned nanomaterials and combined with a certain degree of crosslinking of the composite film, which effectively avoids the migration of pigments and meets the requirements for the use of photovoltaic modules. For Comparative Examples 1-3, the water-blocking properties are slightly poor, which will cause the migration of pigments. For Comparative Example 4, during the lamination process of the composite film without pre-crosslinking, the black high-reflection layer and the white high-reflection layer will invade each other, resulting in abnormal appearance. After 85°C, 85% humidity, and 2000h, the migration of pigments will also greatly affect the peel strength between the conventional backplane and the composite film.

[0063] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A composite film, characterized in that: The invention comprises a barrier layer (1), a black high-reflection layer (2) and a white high-reflection layer (3), wherein the water vapor transmission rate of the barrier layer (1) is less than 0.1 g / m 2 day; The barrier layer (1) comprises a protective layer (11) and a functional layer (12), wherein the functional layer (12) is attached to the protective layer (11), and the functional layer (12) comprises, by weight, 130-150 parts of a first resin, 35-45 parts of a first nanomaterial, and 10-20 parts of a curing agent.

2. The composite membrane according to claim 1, characterized in that: The first nanomaterial includes an organic nanomaterial and an inorganic nanomaterial, wherein the organic nanomaterial includes modified polystyrene microspheres; the inorganic nanomaterial includes one or more of nano titanium dioxide, nano calcium carbonate, nano silicon dioxide, nano boron nitride, nano chromium oxide and nano graphene; the mass ratio of the organic nanomaterial to the inorganic nanomaterial is 1:(1.5-2.3); and / or the particle size of the first nanomaterial is 50-150nm; Preferably, the first resin comprises one or more of fluorocarbon resin, polyester resin, acrylic resin and epoxy resin; Preferably, the curing agent includes one or more of a polyurethane curing agent, an isocyanate curing agent and an epoxy curing agent.

3. The composite membrane according to claim 2, characterized in that: The preparation method of the modified polystyrene microspheres comprises the following steps: (1) first copolymerizing styrene with a functional monomer to obtain a modified polystyrene precursor; the functional monomer includes a monomer containing an amino group, a sulfonic acid group, and a carboxyl group; (2) The modified polystyrene precursor of step (1) is subjected to suspension polymerization to obtain the modified polystyrene microspheres.

4. The composite membrane according to claim 1, characterized in that: The light transmittance of the barrier layer (1) in the wavelength range of 400-1100 nm is greater than 90%.

5. The composite membrane according to claim 1, characterized in that: The black high-reflective layer (2) comprises, by weight, 140-160 parts of a second resin, 10-20 parts of a colorant, 10-20 parts of a second nanomaterial, and 1-3 parts of a cross-linking agent.

6. The composite membrane according to claim 5, characterized in that: The colorant includes dye red, dye yellow and dye blue, and / or the mass percentage of the dye red, dye yellow and dye blue is (20-25%): (40-50%): (25-30%); Preferably, the second resin includes one or more of ethylene copolymer resin, propylene copolymer resin, and vinyl acetate copolymer resin; Preferably, the second nanomaterial includes one or more of nano silicon dioxide and nano titanium dioxide; Preferably, the crosslinking agent includes one or more of tert-butyl peroxy-2-ethylhexanoate, dipentaerythritol hexaacrylate and propoxylated trimethylolpropane triacrylate.

7. The composite membrane according to claim 5, characterized in that: The black high reflective layer (2) further comprises a surfactant, wherein the surfactant comprises one or more of sodium dodecylbenzene sulfonate, alkyl glucoside, fatty acid glyceride, fatty acid sorbitan, polysorbate, and sodium glycocholate; and / or the mass ratio of the surfactant to the second nanomaterial is (0.1-0.2):

1.

8. The composite membrane according to claim 1, characterized in that: The reflectivity of the black high reflective layer (2) to light in the wavelength range of 280-1400nm is between 10% and 15%; the transmittance of the black high reflective layer (2) to ultraviolet light in the wavelength range of 280-400nm is less than 0.5%, the transmittance of the black high reflective layer (2) to visible light in the wavelength range of 400-700nm is less than 0.5%, and the transmittance of the black high reflective layer (2) to infrared light in the wavelength range of 760-1100nm is greater than 75%; The reflectivity of the white high-reflection layer (3) to light in the wavelength range of 400-1200 nm is greater than 95%.

9. The composite membrane according to claim 1, characterized in that: The degree of cross-linking between the black high-reflection layer (2) and the white high-reflection layer (3) is 20%-50%.

10. The composite membrane according to claim 1, characterized in that: An adhesive layer (5) is provided between the barrier layer (1) and the black high-reflection layer (2) or between the barrier layer (1) and the white high-reflection layer (3); Preferably, the adhesive layer (5) includes an ultraviolet absorber; The ultraviolet absorber includes one or more of salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, triazines, and hindered amines.

11. The composite membrane according to claim 1, characterized in that: It also includes an ultraviolet cutoff layer (4), wherein the ultraviolet cutoff layer (4) is located on the light-facing side of the composite film; Preferably, the absorption rate of the ultraviolet cutoff layer (4) to ultraviolet light in the wavelength range of 280-380 nm is greater than 90%; Preferably, the transmittance of the adhesive layer (5) to ultraviolet light in the wavelength range of 280-380 nm is less than 5%, and the transmittance of the adhesive layer (5) to light in the wavelength range of 400-1100 nm is greater than 90%.

12. A photovoltaic module, comprising photovoltaic glass, an encapsulation film, a battery cell and a photovoltaic backplane, characterized in that: The photovoltaic module has the composite film according to any one of claims 1 to 11, and the composite film is arranged between the battery cell and the photovoltaic backsheet.

Citation Information

Patent Citations

  • Composite membrane, preparation method thereof and solar cell assembly

    CN104992995A

  • High-reflection black adhesive film as well as preparation method and application thereof

    CN114149769A

  • Photovoltaic backboard and photovoltaic module

    CN115714147A

  • High-infrared-reflection black barrier packaging adhesive film, preparation method thereof and photovoltaic module

    CN116494620A

  • Solar cell backboard with good anti-aging performance

    CN209561436U

Cited By

  • Anti-aging nano calcium carbonate surface treatment method for photovoltaic sealant and photovoltaic sealant

    CN119799034A