Ablation-resistant / lightweight multilayer composite material and preparation method thereof

By using a multi-layer structure of a hard carbon fiber layer, a hard high-silica layer and a soft low-density layer in the composite material, the contradiction between ablation resistance and lightweight and low-cost in the existing technology is solved, and the problem is realized in the composite material. Effective thermal insulation and ablation resistance in high-temperature environments reduce the overall density and heat transfer of the material.

CN118744584APending Publication Date: 2024-10-08HUBEI FEILIHUA QUARTZ GLASS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410872185.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When improving the ablation resistance of existing composite materials, it is usually necessary to increase the thickness of the resin layer and carbon fiber layer, resulting in an increase in material weight and high production costs, making it difficult to use in large quantities.

Method used

Using a multi-layer composite material composed of a hard carbon fiber layer, a hard high-silica layer and a soft low-density layer, by optimizing the thickness ratio between layers and the ratio of raw materials, the overall density and cost of the material are reduced while maintaining excellent durability. Ablative and thermal insulation properties.

Benefits of technology

It can effectively reduce material weight and production costs while ensuring ablation resistance, and meet the use needs of composite materials in diverse environments. It improves the overall performance through the co-solidification molding of the hard carbon fiber layer and the hard high-silica layer. The strong, soft, low-density layer of airgel material significantly reduces overall density and heat transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744584A_ABST
    Figure CN118744584A_ABST
Patent Text Reader

Abstract

The invention relates to a composite material and a preparation method thereof, in particular to an ablation-resistant / lightweight multilayer composite material and a preparation method thereof. The composite material is prepared from a hard carbon fiber layer, a hard high silica layer and a soft low-density layer, the hard carbon fiber layer comprises phenolic resin, a functional filler, short carbon fibers and a solvent; the hard high-silica layer comprises phenolic resin, chopped high-silica fibers and a solvent; and the soft low-density layer is made of an aerogel material. The composite material is excellent in ablation resistance; the hard high silica layer can effectively reduce the cost; the soft low-density layer can realize light weight and improve heat insulation performance. The problems that an existing composite material is large in weight and high in production cost under the condition of the same ablation resistance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite material and a preparation method thereof, and in particular to an ablation-resistant / lightweight multilayer composite material and a preparation method thereof. Background Art

[0002] With the continuous development of aerospace technology, the preparation and research of thermal protection materials such as nozzles are becoming more and more important. Patent application CN116535811A introduces a low-density ablation-resistant phenolic resin-based carbon fiber composite material and its preparation method. First, an organic-inorganic hybrid zirconium silicate sol coating is coated on the surface of the carbon fiber cloth, and then impregnated with phenolic resin, and then cured and formed into the composite material; wherein, the presence of the organic-inorganic hybrid zirconium silicate sol effectively improves the compatibility between the carbon fiber and the phenolic resin, optimizes the interface problem, and improves the mechanical properties of the composite material. At the same time, the ceramic layer formed by the decomposition of the organic-inorganic hybrid zirconium silicate sol in a high-temperature ablation environment can effectively block the entry of oxygen and heat flow, thereby improving the anti-oxidation and ablation performance of the composite material. The composite material described in the present invention has good interface bonding performance and anti-oxidation and ablation performance, can meet the ablation thermal protection requirements under high-temperature and high-speed combustion service conditions, and the preparation method is simple, low cost, and has good application prospects.

[0003] Patent application CN110938281A introduces a modified carbon fiber reinforced phenolic resin-based composite material and a preparation method thereof, wherein the modified phenolic resin is used as a substrate, an ablation-resistant filler improves ablation resistance, and a high-strength carbon fiber is used as a reinforcing fiber, and the composite material is molded. The phenolic resin-based carbon fiber composite material is prepared from modified phenolic resin, ablation-resistant filler and carbon fiber; the modified phenolic resin is prepared from boric acid phenol ester, aldehydes and cardanol; the boric acid phenol ester is prepared from phenols, boric acid, a water-carrying agent and a catalyst. The invention also discloses a preparation method of the low-density ablation-resistant phenolic resin-based carbon fiber composite material. The invention has low specific gravity, good mechanical properties (shear strength can reach more than 190Mpa, tensile strength is more than 100Mpa), and excellent linear ablation rate (below 0.1mm / s).

[0004] The above-mentioned composite materials have excellent ablation resistance and form a certain protective layer under high temperature conditions, which can effectively protect the profile. However, in order to cope with the high-temperature environment during work, the above-mentioned composite materials generally obtain ablation resistance through the thickness of the resin layer and the carbon fiber layer (or carbon fiber cloth layer). Although the composite material with a large thickness has improved ablation resistance, its weight will increase with the increase of thickness, and the large amount of resin and carbon fiber used leads to high cost, making it difficult to use in large batches. Therefore, it is necessary to develop an ablation-resistant / lightweight multilayer composite material and a preparation method thereof to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide an ablation-resistant / lightweight multilayer composite material and a preparation method thereof, which can effectively reduce weight and production cost while ensuring ablation resistance, in view of the shortcomings of the prior art. The multilayer composite material is composed of three layers: a hard carbon fiber layer, a hard high-silicon oxide layer, and a soft low-density layer. It has low overall cost, excellent ablation resistance, can effectively isolate heat transfer, and meet the requirements of the diversified use environment of the composite material.

[0006] The technical solution of the present invention is: An ablation-resistant / lightweight multilayer composite material, which is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2): (0.5-2): (0.5-2); characterized in that: the hard carbon fiber layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, functional filler: 5-50 parts, chopped carbon fiber: 30-100 parts, solvent: 50-150 parts; The hard high-silicon oxide layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, short-cut high-silica fiber: 30-100 parts, solvent: 20-150 parts; The soft low-density layer is aerogel material.

[0007] The phenolic resin is one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin and boronphenolic resin.

[0008] The chopped carbon fiber is one or more of viscose-based carbon fiber, polyacrylonitrile-based carbon fiber, and asphalt-based carbon fiber.

[0009] The functional filler is one or more of silicon carbide, silicon nitride, boron carbide, kaolin, silicon micropowder, and low-melting-point glass frit.

[0010] The solvent is one or more of ethanol, methanol and acetone.

[0011] A method for preparing an ablation-resistant / lightweight multilayer composite material, characterized in that the method comprises the following steps: 1) weighing the raw materials of the hard high-silica layer according to the ratio, mixing the phenolic resin and the solvent to obtain a phenolic resin solution; after the phenolic resin solution is evenly mixed, the phenolic resin solution and the short-cut high-silica fiber are evenly mixed to obtain a prefabricated liquid, and pre-curing and molding to obtain a hard high-silica layer; 2) weighing the raw materials of the hard carbon fiber layer according to the ratio, mixing the phenolic resin, the functional filler and the solvent to prepare a mixed liquid, uniformly mixing the mixed liquid and the chopped carbon fiber to prepare a prefabricated liquid, and co-curing the prefabricated liquid and the hard high-silica layer obtained by pre-curing to obtain a hard carbon fiber layer and a hard high-silica layer bonded together; 3) The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

[0012] The beneficial effects of the present invention are: The oxyacetylene linear ablation rate of the hard carbon fiber layer in the ablation-resistant / lightweight multilayer composite material is 0.003-0.011 mm / s, which can effectively resist the erosion of high-temperature flames through the hard carbon fiber layer, and has excellent anti-ablation performance; the linear ablation rate of the hard high-silicon oxide layer is 0.072-0.076 mm / s, and the thermal conductivity is 0.45-0.49 W / (mK), which can reduce the use of short-cut carbon fiber and functional fillers while ensuring the requirements of anti-ablation and thermal insulation performance, and can effectively reduce costs; the density of the soft low-density layer is 0.3 g / cm 3 , thermal conductivity 0.02W / (mK). Since the aerogel material itself has the characteristics of low density and strong thermal insulation, the addition of a soft low-density layer can significantly reduce the average density of the composite material as a whole, thereby effectively reducing the overall weight and achieving lightweight; and the extremely low thermal conductivity of the soft low-density layer can effectively weaken the heat transfer of the composite material as a whole and improve the thermal insulation performance. The hard carbon fiber layer and the hard high-silica layer are co-cured and molded in one piece. The co-curing molding can effectively reduce the problem of interface fusion, promote the fusion of the hard carbon fiber layer and the hard high-silica layer, and improve the overall strength. It can meet the diverse requirements of the environment according to the actual application requirements, and the design of multiple layers with different thicknesses can solve the problem of heavy weight and high production cost of existing composite materials with the same ablation resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram of the production process of the present invention.

[0014] In the figure: 1. Hard high-silica layer, 2. Hard carbon fiber layer, 3. Soft low-density layer. DETAILED DESCRIPTION Example 1

[0015] The ablation-resistant / lightweight multilayer composite material is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2):(0.5-2):(0.5-2).

[0016] The composition of the hard carbon fiber layer is as follows: 100 parts of phenolic resin, 5 parts of silicon carbide, 5 parts of low melting point glass, 50 parts of chopped carbon fiber, and 100 parts of solvent. The composition of the hard high silica layer is as follows: 100 parts of phenolic resin, 50 parts of chopped high silica fiber, and 30 parts of solvent. The soft low-density layer is aerogel material.

[0017] The specific steps of the preparation method of the ablation-resistant / lightweight multilayer composite material are as follows: The raw material ratio of the hard high-silica layer is weighed, phenolic resin and solvent are mixed to obtain a phenolic resin solution, the phenolic resin solution and short-cut high-silica fibers are evenly mixed, and pre-cured to obtain a hard high-silica layer.

[0018] The raw material ratio of the above-mentioned hard carbon fiber layer is weighed, the phenolic resin, functional filler and solvent are mixed to obtain a phenolic resin solution, and then the phenolic resin solution and the chopped carbon fiber are evenly mixed, and co-cured with the hard high-silica layer obtained by pre-curing to obtain a hard carbon fiber layer and a hard high-silica layer.

[0019] The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

[0020] The oxyacetylene line ablation rate of the hard carbon fiber layer in the multilayer composite material is 0.011mm / s, which can effectively resist the erosion of high-temperature flames and has excellent anti-ablation performance; the line ablation rate of the hard high-silicon oxide layer is 0.073mm / s, and the thermal conductivity is 0.47W / (mK), which can reduce costs while ensuring the requirements of anti-ablation and thermal insulation performance. The density of the soft low-density layer is 0.3g / cm 3 , thermal conductivity is 0.02W / (mK), which can significantly reduce the overall average density of the material and weaken the heat transfer. Example 2

[0021] The ablation-resistant / lightweight multilayer composite material is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2):(0.5-2):(0.5-2).

[0022] The composition of the hard carbon fiber layer is as follows: 100 parts of phenolic resin, 7 parts of silicon carbide, 3 parts of low melting point glass, 45 parts of chopped carbon fiber, and 100 parts of solvent. The composition of the hard high silica layer is as follows: 100 parts of phenolic resin, 45 parts of chopped high silica fiber, and 30 parts of solvent. The soft low-density layer is aerogel material.

[0023] The specific steps of the preparation method of the ablation-resistant / lightweight multilayer composite material are as follows: The raw material ratio of the hard high-silica layer is weighed, phenolic resin and solvent are mixed to obtain a phenolic resin solution, the phenolic resin solution and short-cut high-silica fibers are evenly mixed, and pre-cured to obtain a hard high-silica layer.

[0024] The raw material ratio of the above-mentioned hard carbon fiber layer is weighed, the phenolic resin, functional filler and solvent are mixed to obtain a phenolic resin solution, and then the phenolic resin solution and the chopped carbon fiber are evenly mixed, and co-cured with the hard high-silica layer obtained by pre-curing to obtain a hard carbon fiber layer and a hard high-silica layer.

[0025] The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

[0026] The oxyacetylene linear ablation rate of the hard carbon fiber layer in the multi-layer composite material is 0.005 mm / s, which can effectively withstand the erosion of high-temperature flames and has excellent anti-ablation performance; the linear ablation rate of the hard high-silicon oxide layer is 0.076 mm / s, and the thermal conductivity is 0.45 W / (mK), which can reduce costs while ensuring the requirements of anti-ablation and thermal insulation performance. The density of the soft low-density layer is 0.3 g / cm3, and the thermal conductivity is 0.02 W / (mK), which can significantly reduce the overall average density of the material and weaken the heat transfer. Example 3

[0027] The ablation-resistant / lightweight multilayer composite material is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2):(0.5-2):(0.5-2).

[0028] The composition of the hard carbon fiber layer is as follows: 100 parts of phenolic resin, 10 parts of silicon carbide, 5 parts of low melting point glass, 50 parts of chopped carbon fiber, and 100 parts of solvent. The composition of the hard high silica layer is as follows: 100 parts of phenolic resin, 55 parts of chopped high silica fiber, and 30 parts of solvent. The soft low-density layer is aerogel material.

[0029] The specific steps of the preparation method of the ablation-resistant / lightweight multilayer composite material are as follows: The raw material ratio of the hard high-silica layer is weighed, phenolic resin and solvent are mixed to obtain a phenolic resin solution, the phenolic resin solution and short-cut high-silica fibers are evenly mixed, and pre-cured to obtain a hard high-silica layer.

[0030] The raw material ratio of the above-mentioned hard carbon fiber layer is weighed, the phenolic resin, functional filler and solvent are mixed to obtain a phenolic resin solution, and then the phenolic resin solution and the chopped carbon fiber are evenly mixed, and co-cured with the hard high-silica layer obtained by pre-curing to obtain a hard carbon fiber layer and a hard high-silica layer.

[0031] The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

[0032] The oxyacetylene linear ablation rate of the hard carbon fiber layer in the multi-layer composite material is 0.003 mm / s, which can effectively withstand the erosion of high-temperature flames and has excellent anti-ablation performance; the linear ablation rate of the hard high-silicon oxide layer is 0.072 mm / s, and the thermal conductivity is 0.49 W / (mK), which can reduce costs while ensuring the requirements of anti-ablation and thermal insulation performance; the density of the soft low-density layer is 0.3 g / cm3, and the thermal conductivity is 0.02 W / (mK), which can significantly reduce the overall average density of the material and weaken the heat transfer. Example 4

[0033] The ablation-resistant / lightweight multilayer composite material is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2):(0.5-2):(0.5-2).

[0034] The composition of the hard carbon fiber layer is as follows: 100 parts of phenolic resin, 5 parts of silicon carbide, 10 parts of low melting point glass, 50 parts of chopped carbon fiber, and 100 parts of solvent. The composition of the hard high silica layer is as follows: 100 parts of phenolic resin, 45 parts of chopped high silica fiber, and 30 parts of solvent. The soft low-density layer is aerogel material.

[0035] The specific steps of the preparation method of the ablation-resistant / lightweight multilayer composite material are as follows: The raw material ratio of the hard high-silica layer is weighed, phenolic resin and solvent are mixed to obtain a phenolic resin solution, the phenolic resin solution and short-cut high-silica fibers are evenly mixed, and pre-cured to obtain a hard high-silica layer.

[0036] The raw material ratio of the above-mentioned hard carbon fiber layer is weighed, the phenolic resin, functional filler and solvent are mixed to obtain a phenolic resin solution, and then the phenolic resin solution and the chopped carbon fiber are evenly mixed, and co-cured with the hard high-silica layer obtained by pre-curing to obtain a hard carbon fiber layer and a hard high-silica layer.

[0037] The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

[0038] The oxyacetylene linear ablation rate of the hard carbon fiber layer in the multi-layer composite material is 0.008 mm / s, which can effectively withstand the erosion of high-temperature flames and has excellent anti-ablation performance; the linear ablation rate of the hard high-silicon oxide layer is 0.076 mm / s, and the thermal conductivity is 0.45 W / (mK), which can reduce costs while ensuring the requirements of anti-ablation and thermal insulation performance. The density of the soft low-density layer is 0.3 g / cm3, and the thermal conductivity is 0.02 W / (mK), which can significantly reduce the overall average density of the material and weaken the heat transfer.

Claims

1. An ablation-resistant / lightweight multilayer composite material, which is made of a hard carbon fiber layer, a hard high-silicon oxide layer and a soft low-density layer with an interlayer thickness ratio of (0.5-2): (0.5-2): (0.5-2); characterized in that: The hard carbon fiber layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, functional filler: 5-50 parts, chopped carbon fiber: 30-100 parts, solvent: 50-150 parts.

2. The ablation-resistant / lightweight multilayer composite material according to claim 1, characterized in that: The hard high-silicon oxide layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, short-cut high-silica fiber: 30-100 parts, solvent: 20-150 parts; The soft, low-density layer is made of aerogel material; The hard carbon fiber layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, functional filler: 5-15 parts, chopped carbon fiber: 30-60 parts, solvent: 30-120 parts; The hard high-silicon oxide layer is made of the following raw materials in parts by weight: Phenolic resin: 100 parts, short-cut high-silica fiber: 30-75 parts, solvent: 30-120 parts; The soft low-density layer is aerogel material.

3. The ablation-resistant / lightweight multilayer composite material according to claim 1 or 2, characterized in that: The phenolic resin is one or more of aminophenolic resin, bariumphenolic resin, magnesiumphenolic resin and boronphenolic resin.

4. The ablation-resistant / lightweight multilayer composite material according to claim 1 or 2, characterized in that: The chopped carbon fiber is one or more of viscose-based carbon fiber, polyacrylonitrile-based carbon fiber, and asphalt-based carbon fiber.

5. The ablation-resistant / lightweight multilayer composite material according to claim 1 or 2, characterized in that: The functional filler is one or more of silicon carbide, silicon nitride, boron carbide, kaolin, silicon micropowder, and low-melting-point glass frit.

6. The ablation-resistant / lightweight multilayer composite material according to claim 1 or 2, characterized in that: The solvent is one or more of ethanol, methanol and acetone.

7. A method for preparing the ablation-resistant / lightweight multilayer composite material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: 1) weighing the raw materials of the hard high-silica layer according to the ratio, mixing the phenolic resin and the solvent to obtain a phenolic resin solution; after the phenolic resin solution is evenly mixed, the phenolic resin solution and the short-cut high-silica fibers are evenly mixed, and pre-curing is performed to obtain a hard high-silica layer; 2) weighing the raw materials of the hard carbon fiber layer according to the ratio, mixing the phenolic resin, the functional filler and the solvent to obtain a mixed liquid, and uniformly mixing the mixed liquid and the chopped carbon fiber to obtain a prefabricated liquid; co-curing the prefabricated liquid and the precuring molding to obtain a hard high-silica layer, thereby obtaining a hard carbon fiber layer and a hard high-silica layer bonded together; 3) The co-cured hard carbon fiber layer, the hard high-silica layer and the soft low-density layer are glued together to prepare an ablation-resistant / lightweight multilayer composite material.

Citation Information

Patent Citations

  • Heat insulation layer structure of solid rocket engine long-tail nozzle, and preparation method thereof

    CN112223856A

  • Aerogel composite material for thermal protection and preparation method thereof

    CN114714734A

  • Thermal insulation / ablation-resistant thermal protection structure and preparation method thereof

    CN115195254A

  • Gradient density thermal protection material and preparation method thereof

    CN117429143A

  • Ablation-resistant high-silica carbon fiber composite material and preparation method thereof

    CN117698221A