Biomass hard carbon negative electrode material and preparation method thereof
Through the specific preparation process of biomass raw materials, the problems of limited resources and environmental pollution of traditional hard carbon anode materials are solved. Biomass hard carbon anode materials with excellent electrochemical performance and environmental protection characteristics are prepared, which are suitable for sodium-ion batteries and achieve Resource-rich and environmentally friendly energy storage applications.
Patent Information
- Application Number
- CN202410696473.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional hard carbon anode materials are mainly derived from fossil fuels, with limited resources and environmental pollution problems in the preparation process. It is necessary to develop a new, environmentally friendly, and renewable hard carbon anode material.
Biomass raw materials are used to prepare biomass hard carbon anode materials through the steps of pickling pretreatment, cleaning and drying, crushing, calcination, mixing, dehydration and solidification, carbonization, coating and drying to avoid the use of toxic and harmful materials. chemicals to ensure environmental protection and high efficiency.
The prepared biomass hard carbon anode material has excellent electrochemical properties, stable cycle charge and discharge performance, high specific surface area and good conductivity. It is suitable for sodium-ion batteries. It has wide sources of raw materials, low cost, and meets environmental protection requirements. .
Smart Images

Figure CN118744976A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials, and in particular to a biomass hard carbon negative electrode material and a preparation method thereof. Background Art
[0002] Graphite negative electrodes are difficult to apply to sodium batteries, and negative electrode materials need to be reselected. Negative electrode materials play an important role in loading sodium ions and are the core components of sodium batteries, which directly affect the battery's energy density, cycle performance, initial efficiency and other performance. Carbon-based materials are widely available and have strong sodium storage capacity. They have become the current mainstream choice. Carbon-based materials can be divided into hard carbon and soft carbon according to whether they will be graphitized after high-temperature treatment. Carbon that will not be graphitized after high-temperature treatment at 2800°C is called hard carbon, and soft carbon is carbon that can be graphitized after high-temperature treatment. Hard carbon materials have many sodium storage active sites and high specific capacity, and have obvious comparative advantages compared to soft carbon. The crystal arrangement inside hard carbon is disordered and has many types of reversible sodium storage sites with high sodium storage capacity. The sites for hard carbon to store sodium ions mainly include: 1) sodium storage through embedding reaction; 2) sodium storage by forming atomic clusters in closed pores; 3) sodium storage by capacitive adsorption on the electrolyte surface; 4) sodium storage by pseudocapacitance at defect sites. Hard carbon also has the advantages of small volume expansion after sodium embedding, good safety, stable structure, good conductivity, and environmental friendliness, and performs well in fast charging performance and low temperature performance. Currently, mainstream companies in the industry all use the hard carbon negative electrode route, and hard carbon has extremely strong commercialization potential.
[0003] With the popularity of electronic products such as electric vehicles and smart phones, the demand for high-performance energy storage materials is growing. Hard carbon negative electrode materials are widely used in the field of sodium ion batteries due to their high specific capacity, good cycle stability and low cost. However, traditional hard carbon negative electrode materials are mainly derived from fossil fuels. Not only are the resources limited, but there are also environmental pollution problems during the preparation process. Therefore, it is of great significance to develop a new, environmentally friendly and renewable hard carbon negative electrode material. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a biomass hard carbon negative electrode material and a preparation method thereof, which solves the problems mentioned in the above background technology.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a biomass hard carbon negative electrode material, specifically comprising the following steps:
[0006] S1. Pickling pretreatment: adding the biomass raw materials into acid solution for pickling pretreatment, and then washing with water until neutral;
[0007] S2. Cleaning and drying: Select the biomass material, put it into the cleaning box, clean the impurities therein, and after cleaning, put the biomass material into the drying box, dry it to constant weight at a temperature of 80-100°C for 48 hours to ensure the dryness and stability of the biomass material;
[0008] S3, pulverization: Use a mechanical pulverizer or a jet mill to pulverize the dried biomass material to obtain a precursor powder with uniform particle size distribution, and the average particle size is controlled between 5-20 μm;
[0009] S4, calcination treatment: under a protective atmosphere, the precursor particles obtained in S3 are heated to 400-600°C for pre-calcination for 1.5-2.5h, then cooled to room temperature with the furnace, then heated to 800-1600°C for calcination for 2-5h, and then naturally cooled;
[0010] S5, mixing treatment: add the precursor powder, silicon powder and modifier into the agitator in a certain proportion, with a mass ratio of 100:5:1, add an appropriate amount of deionized water, turn on the agitator for mixing, and control the mixing time to 30-60 minutes to ensure uniform mixing;
[0011] S6, dehydration and curing treatment: put the mixed materials into the dehydration and curing equipment, and perform dehydration and curing treatment at 60-80°C for about 2-4 hours. The purpose of this step is to remove excess water in the materials and make the materials form a stable structure;
[0012] S7, carbonization treatment: the dehydrated and solidified material is placed in a high-temperature carbonization furnace and carbonized at a high temperature of 1000-1400°C. The carbonization time depends on the type and thickness of the material and is generally controlled within 2-6 hours to ensure that the material is completely carbonized and obtain high-quality hard carbon negative electrode materials;
[0013] S8, coating and drying treatment: the hard carbon negative electrode material obtained by carbonization is mixed with a binder in a certain proportion, a mass ratio of 90:10, and then coated on an aluminum foil. The coated electrode sheet is placed in a vacuum drying oven and vacuum dried at 120°C for about 12 hours. After drying, the biomass hard carbon negative electrode material is obtained.
[0014] Preferably, in S1, the biomass raw material is any one or more of pine cones, coconut shells, walnut shells, wheat straw, rice husks, blue algae, bean dregs, banana peels, cotton, asphalt, peat, seaweed, and cotton husks.
[0015] Preferably, in S1, the acid solution is any one or more of 0.1-0.2 mol / L hydrochloric acid, sulfuric acid solution, and a mixed acid containing 0.1 mol / L hydrochloric acid, 0.1 mol / L nitric acid, and 0.1 mol / L hydrofluoric acid.
[0016] Preferably, the protective atmosphere is any one of argon or nitrogen, and the protective gas flow rate for forming the protective atmosphere is 40-200 sccm for every 10 g of precursor particles.
[0017] Preferably, the purpose of step S6 is to remove excess moisture in the material so that the material forms a stable structure.
[0018] Preferably, in S5, the modifier is one or more of potassium permanganate, perchloric acid, sodium hypochlorite, sodium ferrate, hematite, metallic tin, and phosphorus-tin alloy.
[0019] Preferably, in S4, the temperature is first raised to 400-600°C at a rate of 0.5-10°C / min for pre-calcination for 1.5-2.5h, then cooled to room temperature, and then raised to 800-1600°C at a rate of 0.5-10°C / min for calcination for 2-5h, cooled to room temperature after pre-calcination, and then heated again for calcination after cleaning and impurity removal, wherein the cleaning and impurity removal refers to washing with water, filtering, and vacuum drying. The washing water is preferably deionized water, and the vacuum drying temperature is 80-120°C.
[0020] The present invention also provides a biomass hard carbon negative electrode material obtained by the above preparation method.
[0021] Beneficial Effects
[0022] The invention provides a biomass hard carbon negative electrode material and a preparation method thereof. Compared with the prior art, the invention has the following beneficial effects: the preparation method of the biomass hard carbon negative electrode material specifically comprises the following steps: S1, pickling pretreatment; S2, cleaning and drying; S3, crushing treatment; S4, calcination treatment; S5, mixing treatment; S6, dehydration and solidification treatment; S7, carbonization treatment; S8, coating and drying treatment; the biomass hard carbon negative electrode material is obtained by using biomass as raw material through a specific preparation process, which not only has abundant raw material sources and low cost, but also has excellent electrochemical properties, and no toxic and harmful chemicals are required in the preparation process, which meets environmental protection requirements. The biomass hard carbon negative electrode material is suitable for energy storage equipment such as sodium ion batteries, and the process is optimized. The biomass raw material is first pickled to remove impurities, and the degree of graphitization is low, the surface defects are few, and it has a larger charge and discharge specific capacity. The performance is stable during the cyclic charge and discharge process. The prepared biomass hard carbon negative electrode material has a high specific surface area, good electrical conductivity and reversible energy storage performance. At the same time, due to the wide source of raw materials, renewable and environmentally friendly, the biomass hard carbon negative electrode material has broad application prospects in the field of energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of the steps of the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] See also Figure 1 The present invention provides three technical solutions: a method for preparing a biomass hard carbon negative electrode material, specifically including the following embodiments:
[0026] Embodiment 1
[0027] S1. Pickling pretreatment: adding the biomass raw materials into acid solution for pickling pretreatment, and then washing with water until neutral;
[0028] S2, cleaning and drying: select biomass materials, put them into a cleaning box, clean out impurities, and after cleaning, put the biomass materials into a drying box, dry them at 90°C for 48 hours to constant weight, to ensure that the biomass materials are dry and stable;
[0029] S3, pulverization: Use a mechanical pulverizer or a jet mill to pulverize the dried biomass material to obtain a precursor powder with uniform particle size distribution, and the average particle size is controlled between 13 μm;
[0030] S4, calcination treatment: under a protective atmosphere, the precursor particles obtained in S3 were heated to 500°C for pre-calcination for 2 hours, then cooled to room temperature with the furnace, then heated to 1200°C for calcination for 4 hours, and then naturally cooled;
[0031] S5, mixing treatment: add the precursor powder, silicon powder and modifier into the agitator in a certain proportion, with a mass ratio of 100:5:1, add an appropriate amount of deionized water, turn on the agitator for mixing, and control the mixing time to 45 minutes to ensure uniform mixing;
[0032] S6, dehydration and curing treatment: the mixed materials are placed in a dehydration and curing device, and dehydration and curing treatment is carried out at 70°C for about 3 hours. The purpose of this step is to remove excess water in the materials and form a stable structure of the materials;
[0033] S7, carbonization treatment: the dehydrated and solidified material is placed in a high-temperature carbonization furnace and carbonized at a high temperature of 1200°C. The carbonization time depends on the type and thickness of the material and is generally controlled within 4 hours to ensure that the material is completely carbonized and obtain high-quality hard carbon negative electrode materials;
[0034] S8, coating and drying treatment: the hard carbon negative electrode material obtained by carbonization is mixed with a binder in a certain proportion, a mass ratio of 90:10, and then coated on an aluminum foil. The coated electrode sheet is placed in a vacuum drying oven and vacuum dried at 120°C for about 12 hours. After drying, the biomass hard carbon negative electrode material is obtained.
[0035] Embodiment 2
[0036] S1. Pickling pretreatment: adding the biomass raw materials into acid solution for pickling pretreatment, and then washing with water until neutral;
[0037] S2, cleaning and drying: select biomass materials, put them into a cleaning box, clean out impurities, and after cleaning, put the biomass materials into a drying box, dry them at 80°C for 48 hours to constant weight, to ensure that the biomass materials are dry and stable;
[0038] S3, pulverization: Use a mechanical pulverizer or a jet mill to pulverize the dried biomass material to obtain a precursor powder with uniform particle size distribution, and the average particle size is controlled between 5 μm;
[0039] S4, calcination treatment: under a protective atmosphere, the precursor particles obtained in S3 were heated to 400°C for pre-calcination for 1.5 hours, then cooled to room temperature with the furnace, then heated to 800°C for calcination for 2 hours, and then naturally cooled;
[0040] S5, mixing treatment: add the precursor powder, silicon powder and modifier into the agitator in a certain proportion, with a mass ratio of 100:5:1, add an appropriate amount of deionized water, turn on the agitator for mixing, and control the mixing time within 30 minutes to ensure uniform mixing;
[0041] S6, dehydration and curing treatment: put the mixed materials into the dehydration and curing equipment, and perform dehydration and curing treatment at 60°C for about 2 hours. The purpose of this step is to remove excess water in the materials and make the materials form a stable structure;
[0042] S7, carbonization treatment: the dehydrated and solidified material is placed in a high-temperature carbonization furnace and carbonized at a high temperature of 1000°C. The carbonization time depends on the type and thickness of the material and is generally controlled within 2 hours to ensure that the material is completely carbonized and obtain high-quality hard carbon negative electrode materials;
[0043] S8, coating and drying treatment: the hard carbon negative electrode material obtained by carbonization is mixed with a binder in a certain proportion, a mass ratio of 90:10, and then coated on an aluminum foil. The coated electrode sheet is placed in a vacuum drying oven and vacuum dried at 120°C for about 12 hours. After drying, the biomass hard carbon negative electrode material is obtained.
[0044] Embodiment 3
[0045] S1. Pickling pretreatment: adding the biomass raw materials into acid solution for pickling pretreatment, and then washing with water until neutral;
[0046] S2, cleaning and drying: select biomass materials, put them into a cleaning box, clean out impurities, and after cleaning, put the biomass materials into a drying box, dry them at 100°C for 48 hours to constant weight, to ensure that the biomass materials are dry and stable;
[0047] S3, pulverization: Use a mechanical pulverizer or a jet mill to pulverize the dried biomass material to obtain a precursor powder with uniform particle size distribution, and the average particle size is controlled between 20 μm;
[0048] S4, calcination treatment: under a protective atmosphere, the precursor particles obtained in S3 were heated to 600°C for pre-calcination for 2.5 hours, then cooled to room temperature with the furnace, then heated to 1600°C for calcination for 5 hours, and then naturally cooled;
[0049] S5, mixing treatment: add the precursor powder, silicon powder and modifier into the agitator in a certain proportion, with a mass ratio of 100:5:1, add an appropriate amount of deionized water, turn on the agitator for mixing, and control the mixing time to 60 minutes to ensure uniform mixing;
[0050] S6, dehydration and curing treatment: the uniformly mixed materials are placed in a dehydration and curing device, and dehydration and curing treatment is performed at 80°C for about 4 hours. The purpose of this step is to remove excess water in the materials and form a stable structure of the materials;
[0051] S7, carbonization treatment: the dehydrated and solidified material is placed in a high-temperature carbonization furnace and carbonized at a high temperature of 1400°C. The carbonization time depends on the type and thickness of the material and is generally controlled within 6 hours to ensure that the material is completely carbonized and obtain high-quality hard carbon negative electrode materials;
[0052] S8, coating and drying treatment: the hard carbon negative electrode material obtained by carbonization is mixed with a binder in a certain proportion, a mass ratio of 90:10, and then coated on an aluminum foil. The coated electrode sheet is placed in a vacuum drying oven and vacuum dried at 120°C for about 12 hours. After drying, the biomass hard carbon negative electrode material is obtained.
[0053] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0054] Effect Example
[0055] Battery assembly: The hard carbon negative electrode materials obtained in Examples 1 to 3 were respectively used as active materials, mixed in a mass ratio of active material: ultrafine carbon powder (SP): polyvinylidene fluoride of 90:5:5, N-methylpyrrolidone (NMP) was added to make a viscous glue, coated on an aluminum foil, and baked in a vacuum drying oven at 120°C for 12 h to obtain a negative electrode sheet. A metal sodium sheet was used as a counter electrode, glass fiber (Waterman) was used as a diaphragm, and 1 mol / LNaPF6 (the solvent was EC and DMC in a volume ratio of 1:1) was used as an electrolyte. A 2032 button-type sodium ion battery was assembled in an Ar protective glove box.
[0056] A battery production factory simultaneously tested the button-type sodium-ion batteries produced by Example 1, Example 2, and Example 3, respectively, and the button-type sodium-ion batteries commonly used on the market, and operated them at the same time and under the same conditions to test the electrochemical performance of the button batteries. The specific testing method is: discharging to 0V at a discharge rate of 0.05C, and recording the discharge capacity at this time as the first discharge capacity; then charging to 2V at a charging rate of 0.1C, and recording the charging capacity at this time as the first charging capacity; first coulomb efficiency = first charging capacity / first discharge capacity × 100%. During the testing process, statistical data is simultaneously collected and statistical tables and graphs are prepared.
[0057]
[0058] It can be seen from the above table that the biomass hard carbon negative electrode material is obtained by using biomass as raw material through a specific preparation process. It not only has abundant raw material sources and low cost, but also has excellent electrochemical properties. No toxic and harmful chemicals are required in the preparation process, which meets environmental protection requirements. The biomass hard carbon negative electrode material is suitable for energy storage equipment such as sodium ion batteries. The process is optimized, and the biomass raw materials are first acid-washed to remove impurities. The degree of graphitization is low, the surface defects are few, and it has a larger charge and discharge specific capacity. The performance is stable during the cyclic charge and discharge process. The prepared biomass hard carbon negative electrode material has a high specific surface area, good electrical conductivity and reversible energy storage performance. At the same time, due to the wide source of raw materials, renewable and environmentally friendly, the biomass hard carbon negative electrode material has broad application prospects in the field of energy storage.
[0059] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a biomass hard carbon negative electrode material, characterized in that: The specific steps include: S1. Pickling pretreatment: adding the biomass raw materials into acid solution for pickling pretreatment, and then washing with water until neutral; S2. Cleaning and drying: Select the biomass material, put it into the cleaning box, clean the impurities therein, and after cleaning, put the biomass material into the drying box, dry it to constant weight at a temperature of 80-100°C for 48 hours to ensure the dryness and stability of the biomass material; S3, pulverization: Use a mechanical pulverizer or a jet mill to pulverize the dried biomass material to obtain a precursor powder with uniform particle size distribution, and the average particle size is controlled between 5-20 μm; S4, calcination treatment: under a protective atmosphere, the precursor particles obtained in S3 are heated to 400-600°C for pre-calcination for 1.5-2.5h, then cooled to room temperature with the furnace, then heated to 800-1600°C for calcination for 2-5h, and then naturally cooled; S5, mixing treatment: add the precursor powder, silicon powder and modifier into the agitator in a certain proportion, with a mass ratio of 100:5:1, add an appropriate amount of deionized water, turn on the agitator for mixing, and control the mixing time to 30-60 minutes to ensure uniform mixing; S6, dehydration and curing treatment: put the mixed materials into the dehydration and curing equipment, and perform dehydration and curing treatment at 60-80°C for about 2-4 hours. The purpose of this step is to remove excess water in the materials and make the materials form a stable structure; S7, carbonization treatment: the dehydrated and solidified material is placed in a high-temperature carbonization furnace and carbonized at a high temperature of 1000-1400°C. The carbonization time depends on the type and thickness of the material and is generally controlled within 2-6 hours to ensure that the material is completely carbonized and obtain high-quality hard carbon negative electrode materials; S8, coating and drying treatment: the hard carbon negative electrode material obtained by carbonization is mixed with a binder in a certain proportion, a mass ratio of 90:10, and then coated on an aluminum foil. The coated electrode sheet is placed in a vacuum drying oven and vacuum dried at 120°C for about 12 hours. After drying, the biomass hard carbon negative electrode material is obtained.
2. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: In S1, the biomass raw material is any one or more of pine cones, coconut shells, walnut shells, wheat straw, rice husks, blue algae, bean dregs, banana peels, cotton, asphalt, peat, seaweed, and cotton husks.
3. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: In the S1, the acid solution is any one or more of 0.1-0.2 mol / L hydrochloric acid, sulfuric acid solution, and a mixed acid containing 0.1 mol / L hydrochloric acid, 0.1 mol / L nitric acid, and 0.1 mol / L hydrofluoric acid.
4. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: The protective atmosphere is any one of argon gas and nitrogen gas. For every 10 g of precursor particles, the protective gas flow rate for forming the protective atmosphere is 40-200 sccm.
5. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: The purpose of step S6 is to remove excess water from the material so that the material forms a stable structure.
6. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: In S5, the modifier is one or more of potassium permanganate, perchloric acid, sodium hypochlorite, sodium ferrate, hematite, metallic tin, and phosphorus-tin alloy.
7. The method for preparing a biomass hard carbon negative electrode material according to claim 1, characterized in that: In the S4, the temperature is first raised to 400-600°C at a rate of 0.5-10°C / min for pre-calcination for 1.5-2.5h, then cooled to room temperature, and then raised to 800-1600°C at a rate of 0.5-10°C / min for calcination for 2-5h, cooled to room temperature after pre-calcination, and then heated again for calcination after cleaning and impurity removal, wherein the cleaning and impurity removal refers to washing with water, filtering, and vacuum drying. The washing water is preferably deionized water, and the vacuum drying temperature is 80-120°C.
8. A biomass hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Biomass-based hard carbon / alloy anode composite material as well as preparation method and application thereof
CN117691073A
Preparation method of biomass hard carbon composite silicon carbon negative electrode material
CN117996047A
Cited By
Phycocyanin-based pea-shaped sodium ion battery hard carbon negative electrode material and preparation method thereof
CN119370826A
A phycocyanin-based pea-shaped sodium ion battery hard carbon negative electrode material and its preparation method
CN119370826B
Biomass-based sodium ion battery hard carbon negative electrode material and preparation method and application thereof
CN120589726A
Bagasse hard carbon negative electrode material low-cost iron removal process based on bacterial biological method
CN120922848A
A low-cost iron removal process for sugarcane bagasse hard carbon negative electrode material based on bacterial biological method