Preparation method of monatomic modified porous carbon material and application of monatomic modified porous carbon material in lithium-sulfur battery
The application of porous carbon materials modified by single atoms in lithium-sulfur batteries solves the problems of low conductivity, volume expansion and lithium dendrite growth of lithium-sulfur batteries, improves the discharge capacity and cycle performance of the battery, and realizes the deposition of lithium ions. Uniformity and stability.
Patent Information
- Application Number
- CN202410803261.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-20
AI Technical Summary
The performance and safety of lithium-sulfur batteries are affected by issues such as low conductivity, volume expansion, irreversible loss of polysulfides, and uncontrollable growth of lithium dendrites in the cathode material, and the catalytically active sites of existing catalysts are not fully utilized. .
Single-atom modified porous carbon materials are used to prepare zinc-based metal organic framework materials, phenolic resin coating and solution impregnation methods to load metal salts, and high-temperature carbonization to prepare high catalytic activity X-N/HNPC composite materials for the positive and negative electrodes of lithium-sulfur batteries. , improve catalytic activity and lithium ion deposition control.
It significantly improves the discharge capacity, cycle performance and rate performance of lithium-sulfur batteries, enhances polysulfide conversion kinetics and lithium ion deposition control, and improves battery stability and safety.
Smart Images

Figure CN118744979A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-sulfur battery materials, and in particular to a method for preparing a single-atom modified porous carbon material and application thereof in a lithium-sulfur battery. Background Art
[0002] The development of new energy has driven the progress of energy storage and increased the social demand for energy storage systems. However, due to the limitation of positive and negative electrode materials, the energy density of commercial lithium-ion battery development has approached its theoretical limit and is difficult to meet the needs of social development. Therefore, it is necessary to develop new energy storage systems to provide support for the development of green energy technology. Lithium-sulfur batteries are considered to be one of the most promising new electrochemical energy storage technologies due to their high theoretical energy density (2500 Wh / kg), abundant sulfur resources, low cost and low environmental pollution. However, lithium-sulfur batteries still face some problems. In terms of the positive electrode, the inherent insulating properties of the active substance sulfur and the discharge product lithium sulfide lead to low conductivity of the positive electrode material, which affects the electrochemical reaction rate; due to the different densities of sulfur and lithium sulfide, the volume expansion of the positive electrode material during charging and discharging will cause the pole piece to fall off; the intermediate product polysulfide generated during the redox process will dissolve in the electrolyte and shuttle to the negative electrode under the action of the concentration gradient to directly react with lithium, resulting in irreversible loss of active substances, which seriously affects the battery performance; the slow reaction kinetics of polysulfide also limits the battery capacity. In terms of the negative electrode, the uneven surface of the lithium negative electrode and the uneven distribution of current density lead to uneven deposition of lithium, forming lithium dendrites that continue to grow during the continuous deposition process, which may pierce the separator and affect the safety of the battery. Therefore, solving the above problems is the key to achieving the commercialization of lithium-sulfur batteries.
[0003] The development and design of multifunctional composite positive electrode materials and the protection of lithium negative electrodes are breakthroughs in solving the above problems. At present, in order to improve the conductivity of positive electrode materials, porous carbon materials are usually used as sulfur carriers. At the same time, porous carbon materials have a large specific surface area, which can provide more sulfur loading sites and improve the utilization rate of active sulfur. In addition, the rich pore structure can provide three-dimensional ion transmission channels and alleviate the volume expansion of positive electrode materials during charging and discharging, effectively improving the cycle stability of lithium-sulfur batteries. However, non-polar carbon materials have a weak effect on polysulfides and cannot effectively adsorb and catalyze the conversion of polysulfides. Therefore, in recent years, a series of electrocatalytic materials have been used in the design of positive electrode materials for lithium-sulfur batteries. Such as metal nitrides, metal oxides, metal sulfides, metal carbides, etc. However, since the catalytic conversion reactions of these catalysts are all carried out on the catalyst surface, the catalytic active sites cannot be fully utilized. Therefore, it is of great significance to develop catalytic materials with high atomic utilization and strong catalytic activity for use in lithium-sulfur batteries. In addition, the protection of the lithium negative electrode is also particularly important. The uncontrollable growth of lithium dendrites is mainly due to the uneven deposition of lithium ions. Studies have shown that it is feasible to regulate the deposition of lithium ions by developing lithiophilic materials as carriers of the lithium negative electrode.
[0004] The purpose of the present invention is to design a multifunctional high-activity catalytic material that has physical confinement, chemical adsorption and catalytic conversion of lithium polysulfide and a regulating effect on lithium ion deposition, and to apply it in the field of lithium-sulfur batteries to improve the discharge capacity, cycle stability and rate performance of lithium-sulfur batteries. Summary of the invention
[0005] In order to solve the problems existing in the above-mentioned lithium-sulfur batteries, the present invention provides a method for preparing a single-atom modified porous carbon material and its application in a lithium-sulfur battery. The composite material is applied in a lithium-sulfur battery, and the hollow porous structure can physically confine and chemically adsorb polysulfides. A large number of highly catalytically active sites can improve the conversion reaction kinetics of polysulfides, which can significantly improve the discharge specific capacity, cycle performance and rate performance of the lithium-sulfur battery.
[0006] The present invention solves the technical problem by adopting the following technical solutions: A method for preparing a composite material with high catalytic activity comprises the following steps: (1) Preparation of Zn-MOF particles; (2) coating Zn-MOF particles with phenolic resin (RF) to obtain Zn-MOF-RF particles; (3) The X metal salt is uniformly loaded onto the Zn-MOF-RF particles by solution impregnation method; (4) The material obtained in step (3) is carbonized at high temperature under an inert gas atmosphere to obtain a hollow porous carbon material (XN / HNPC) modified with a high catalytic activity X single atom catalyst.
[0007] Furthermore, the metal organic framework material in step (1) is a zinc-based metal organic framework material composed of a combination of zinc metal ions, 2-methylimidazole (C4H6N2) and hexadecyltrimethylammonium bromide (CTAB). The preparation method of the zinc-based metal organic framework material can be a commonly used method such as hydrothermal / solvothermal synthesis, ultrasonic method, microwave heating method, electrochemical method and mechanochemical synthesis method.
[0008] Preferably, the zinc-based metal organic framework material prepared in step (1) has a cubic structure and a particle size of 30 nm to 2 μm, has a rich pore structure such as micropores and mesopores, and a specific surface area greater than 300 m 2 / g.
[0009] The zinc-based metal organic framework material prepared in step (1) contains nitrogen.
[0010] Preferably, in step (1), cetyltrimethylammonium bromide is introduced into the solvent to obtain cubic Zn-MOF nanoparticles, wherein the mass ratio of CTAB to zinc nitrate is 1:100 to 2:100.
[0011] The phenolic resin-formaldehyde coating in step (2) is coated on the Zn-MOF particles prepared in step (1) by epitaxial growth in a solvent. Specifically, the phenolic resin (RF) coating in step (2) is to uniformly disperse the Zn-MOF nanoparticles in a mixed solution of resorcinol and formaldehyde, stir magnetically at room temperature for 18 to 24 hours, collect the precipitate by centrifugation or suction filtration, wash with deionized water and ethanol, and dry in a vacuum oven at 60°C for 6 to 12 hours, wherein the mass ratio of resorcinol to formaldehyde in the mixed solution is 1:150, and the mass ratio of resorcinol to Zn-MOF nanoparticles is 5:100 to 10:100.
[0012] In step (3), the solution impregnation method is to uniformly disperse the Zn-MOF-RF material in the X metal salt solution, stir magnetically at room temperature for 12 to 24 hours, collect the precipitate by centrifugation or filtration, wash it with deionized water and ethanol, and dry it in a vacuum oven at 60°C for 6 to 12 hours. The metal element X in the X metal salt solution is one or more transition metal elements, and the X metal salt includes acetate, nitrate, chlorate, chloride, etc. of the X metal. The concentration of metal ions in the X metal salt solution is 0.1 to 5 mg / mL, and the solution can be deionized water, ethanol, etc.
[0013] Preferably, the transition metal element is vanadium, nickel, cobalt, iron, manganese, etc.
[0014] Preferably, the mass ratio of the Zn-MOF-RF material to the metal ions is 100:0.5 to 100:2.
[0015] Furthermore, in step (4), the inert gas is nitrogen or argon, the high temperature carbonization temperature is 900-1100°C, and the time is 2-5 hours. The zinc in the Zn-MOF evaporates along with the air flow at high temperature to obtain a porous carbon material XN / HNPC with uniform dispersion of X single atoms.
[0016] Preferably, the carbonization temperature is 900-1000° C., and the carbonization time is 3-5 hours.
[0017] The present invention also provides structural information of a single-atom-modified XN / HNPC composite material with high catalytic activity prepared by the preparation method, wherein the X single atom is uniformly dispersed on the surface of the porous carbon material. The mass fraction of the carbon-based carrier material ranges from 98% to 99.9%; the metal X exists in the form of a single atom, and the mass fraction ranges from 0.1% to 2%.
[0018] Preferably, the mass fraction of metal atoms is 0.5% to 2%.
[0019] Preferably, the specific surface area of the composite material is greater than 400 m 2 / g, with a particle size of 200 nm~2 μm and rich pore structures such as micropores and mesopores.
[0020] The present invention also provides a lithium-sulfur battery, wherein the positive electrode and / or negative electrode of the lithium-sulfur battery contains the single-atom-modified XN / HNPC composite material with high catalytic activity.
[0021] Preferably, a lithium-sulfur battery, wherein the positive electrode adopts a high catalytically active single-atom-loaded XN / HNPC composite material as a pole piece prepared as the positive electrode sulfur-carrying material of the lithium-sulfur battery, the negative electrode adopts a copper foil modified by a pre-lithium-plated XN / HNPC composite material, the electrolyte is composed of a lithium salt, a non-aqueous organic solvent and lithium nitrate, the electrolyte is lithium bistrifluoromethanesulfonyl imide (LiTFSI), the concentration is 1 mol / L, the non-aqueous organic solvent is a mixed solvent of dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a volume ratio of 1:1, and the added lithium nitrate accounts for 1% of the total electrolyte mass.
[0022] The present invention also provides an application of a porous carbon material modified by a single atom catalyst in a lithium-sulfur battery, wherein the XN / HNPC composite material is used as a positive electrode sulfur-carrying material and / or a negative electrode lithium carrier.
[0023] (i) Using the porous carbon material XN / HNPC modified with the above single atom catalyst as the positive electrode sulfur carrier material of the lithium-sulfur battery, the specific steps are as follows: (a) The sublimated sulfur and the XN / HNPC composite material are uniformly mixed in a corresponding mass ratio, and the sulfur / XN / HNPC composite cathode material is obtained by a melt diffusion method under vacuum or inert gas (nitrogen or argon) conditions. The melting heating temperature is 155 °C and the insulation time is 12 to 18 hours. The mass proportion of XN / HNPC in the composite cathode material is 10% to 50%.
[0024] Preferably, the sulfur loading method adopts sulfur loading in a vacuum state, and the mass proportion of XN / HNPC material in the obtained composite positive electrode material is 20%~40%.
[0025] (b) The sulfur / carbon composite positive electrode material obtained in step (a) is uniformly mixed with a conductive agent and a binder in a certain proportion, and nitrogen methyl pyrrolidone (NMP) is used as a solvent. The mixture is uniformly mixed to form a slurry, which is then coated on a current collector and vacuum dried to prepare a positive electrode sheet for a lithium-sulfur battery.
[0026] Preferably, the mass ratio of the sulfur / carbon composite positive electrode material, the conductive agent and the binder is (80-90):(5-10):(5-10).
[0027] The conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, and graphene, and the binder is polyvinylidene fluoride.
[0028] Preferably, the slurry is mixed evenly by ball milling, the ball milling time is 1 to 2 hours, and the sulfur loading of the positive electrode of the lithium-sulfur battery is 0.5 to 5 mg / cm 2 .
[0029] Preferably, the positive electrode current collector used is carbon-coated aluminum foil.
[0030] (c) Assembling the positive electrode sheet and lithium sheet, separator, electrolyte and shell obtained in step (b) to obtain a lithium-sulfur battery for electrochemical testing.
[0031] (ii) Using the porous carbon material XN / HNPC composite material modified with the above single atom catalyst as a lithium negative electrode carrier material, the specific steps are as follows: (a) The XN / HNPC composite material is mixed with a conductive agent and a binder in a certain proportion, and nitrogen methyl pyrrolidone is used as a solvent. After mixing evenly, it is coated on the surface of the copper foil, and then vacuum dried to obtain the copper foil loaded with the XN / HNPC composite material.
[0032] Preferably, the mass ratio of the XN / HNPC composite material, the conductive agent and the binder is (80-90):(5-10):(5-10).
[0033] Preferably, the loading amount of XN / HNPC composite material on the copper foil surface is 0.5-0.8 mg / cm 2 .
[0034] (b) The copper foil modified with the XN / HNPC composite material obtained in step (a) was used as the electrode, the lithium sheet was used as the counter electrode, and the battery was assembled with the electrolyte and the shell. Negative electrode sheet preparation: The current density of the first three cycles was 0.2 mA / cm 2 , charge and discharge activation was performed between 0 and 1 V, and then 0.2 mA / cm 2 Li was pre-plated on XN / HNPC at a current density of 15 mAh / cm 2 , remove the pre-lithium-plated electrode and use it as the negative electrode.
[0035] (c) The pre-lithium-plated electrode is removed as the negative electrode, and the positive electrode, separator and electrolyte using commercial carbon nanotubes as sulfur carrier materials are assembled to obtain a lithium-sulfur battery.
[0036] (III) Using the above-mentioned single-atom modified porous carbon material XN / HNPC as a positive electrode sulfur-carrying material and as a negative electrode carrier material for lithium negative electrode protection, the specific steps are as follows: (1) Sublimated sulfur and XN / HNPC composite materials are uniformly mixed in a certain proportion, and sulfur / carbon composite cathode materials are obtained by melt-filling sulfur in a vacuum or inert gas atmosphere, wherein the heating temperature is 155 °C and the holding time is 12 to 18 hours. The mass proportion of single-atom-modified porous carbon material XN / HNPC in the sulfur / carbon composite cathode material is 20% to 50%; (2) The sulfur / carbon composite positive electrode material, conductive agent and binder obtained in step 1) are mixed in a certain proportion, and nitrogen methyl pyrrolidone is used as a solvent. The mixture is evenly mixed to form a slurry, and then the slurry is evenly coated on the current collector. After vacuum drying, a positive electrode sheet of a lithium-sulfur battery is obtained. The preparation of the positive electrode sheet is the same as the preparation method of the positive electrode sheet in (I); (3) The XN / HNPC composite material is mixed with a conductive agent and a binder in a certain proportion, and nitrogen methyl pyrrolidone is used as a solvent. The mixture is evenly mixed to form a slurry, and then coated on a copper foil. After vacuum drying, the copper foil modified with the XN / HNPC composite material is used as an electrode, and the lithium sheet is used as a counter electrode. A certain capacity of lithium is deposited on the surface of the copper foil modified with the XN / HNPC composite material to obtain a modified lithium negative electrode; specifically, the negative electrode sheet is prepared: the current density of the first three cycles is 0.2 mA / cm 2, charge and discharge activation was performed between 0 and 1 V, and then 0.2 mA / cm 2 Li was pre-plated on XN / HNPC at a current density of 15 mAh / cm 2 , remove the pre-lithium-plated electrode piece as the negative electrode; the preparation of the lithium negative electrode is the same as the preparation method of the lithium negative electrode in (II); (4) Assembling the lithium-sulfur battery positive electrode obtained in step (2) and the lithium negative electrode, separator and electrolyte obtained in step (3) to obtain a lithium-sulfur battery.
[0037] Beneficial effects of the present invention: The present invention provides a method for preparing a porous carbon material modified by a single atom catalyst, wherein Zn-MOF-RF particles are obtained by a solvothermal method and coating with a phenolic resin, and then a solution impregnation method is adopted to prepare a XN / HNPC composite material modified by a single atom catalyst by adsorbing metal salts and then carbonizing at a high temperature in an inert gas environment.
[0038] The XN / HNPC composite material modified by a single atom catalyst prepared by the present invention has good electrical conductivity, a large specific surface area and pore structure, and maximizes the ion transfer rate and sulfur utilization rate. At the same time, the introduction of a single atom catalyst with high catalytic activity can increase the catalytic active sites in the composite material, enhance the adsorption capacity of the positive electrode material for polysulfides, thereby improving the conversion kinetics of polysulfides during the electrochemical reaction, alleviating the shuttle effect of polysulfides, and reducing battery polarization. When the XN / HNPC composite material modified by a single atom catalyst is used as a lithium negative electrode carrier, the deposition of lithium ions can be effectively regulated and the uncontrollable growth of lithium dendrites can be slowed down. Experimental results show that when the XN / HNPC composite material modified by a single atom catalyst is applied to the positive electrode material and negative electrode carrier of a lithium-sulfur battery, the discharge capacity, rate performance and cycle performance of the lithium-sulfur battery can be significantly improved. The preparation method of the present invention has mild reaction conditions and simple process, which can provide guidance for the commercial application of high-performance lithium-sulfur batteries in the future. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 The X-ray diffraction (XRD) pattern of the VN / HNPC material prepared in Example 1 of the present invention; Figure 2Scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the VN / HNPC material prepared in Example 1 of the present invention; Figure 3 The nitrogen isothermal adsorption / desorption curve and pore size distribution diagram of the VN / HNPC material prepared in Example 1 of the present invention; Figure 4 This is an X-ray absorption fine structure spectrum (XAFS) diagram of the VN / HNPC material prepared in Example 1 of the present invention; Figure 5 This is a data analysis diagram of the binding energy of Li2S6 for the materials prepared in Examples 1-5 of the present invention; Figure 6 The materials prepared in Example 1, Example 2 and Comparative Example 1 of the present invention are used in the performance diagram of symmetrical batteries assembled on the negative electrode side of lithium-sulfur batteries; Figure 7 This is a comparison chart of the cycle performance of application examples 1, 2 and 3 of the present invention respectively applied in lithium-sulfur batteries at 0.5 C; Figure 8 The materials prepared in Example 1, Example 2 and Comparative Example 1 of the present invention are simultaneously used as positive and negative electrode carrier materials in a lithium-sulfur battery with a cycle performance at a current density of 1 C; Among them, the XRD graph obtained has a diffraction angle (2θ) on the horizontal axis and a diffraction peak intensity (Intensity) on the vertical axis; the nitrogen isothermal adsorption-desorption curve obtained has a relative pressure on the horizontal axis and a nitrogen adsorption volume on the vertical axis; the X-ray absorption fine structure spectrum (XAFS) obtained has an absorption energy on the horizontal axis and an absorption intensity (Normalized date) on the vertical axis; the symmetric battery performance graph obtained has a time on the horizontal axis and a voltage on the vertical axis; the cycle performance graph obtained has a cycle number on the horizontal axis and a specific capacity on the vertical axis. DETAILED DESCRIPTION
[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1 The preparation method of the VN / HNPC composite material modified with a single atom catalyst in this embodiment is as follows: 1. Preparation of ZIF-8 Nanoparticles First, 4 mg of hexadecyltrimethylammonium bromide (CTAB) was evenly dispersed in 10 mL of deionized water, and then 295 mg of zinc nitrate (Zn(NO3)26H2O) was added to the above solution and mixed evenly to obtain a mixed solution A; then 4.54 g of 2-methylimidazole (C4H6N2) was added to another 70 mL of deionized water solution to obtain a mixed solution B. After the two mixed solutions were completely dissolved, the mixed solution B was added to the rapidly stirred mixed solution A, and magnetic stirring was performed at room temperature for 40 minutes. The precipitate was collected by centrifugation at a speed of 5000 r / min and a centrifugal time of 5 minutes. Finally, it was washed with ethanol solution for more than three times and dried in a vacuum oven at 60 °C for 6 hours to obtain ZIF-8 nanoparticles.
[0043] 2. Coating ZIF-8 nanoparticles with phenolic resin (RF) to obtain ZIF-8-RF particles First, 15 mg of resorcinol (C6H6O2), 15 mg of hexadecyltrimethylammonium bromide (CTAB) and 2.75 mL of formaldehyde solution were dissolved in 60 mL of deionized water. After stirring for 30 min, 200 mg of ZIF-8 nanoparticle precursor was added, and the material was evenly dispersed by ultrasonic treatment for 10 min. The material was magnetically stirred at room temperature for 24 hours, and the precipitate was collected by centrifugation at a speed of 5000 r / min for 5 min. Finally, it was washed with deionized water and dried in a vacuum oven at 60 °C for 6 hours to obtain ZIF-8-RF particles.
[0044] 3. Uniform loading of V metal salt onto ZIF-8-RF particles by solution impregnation 11 mg of vanadium diacetylacetonate (C 10 H 14 O5V) was dispersed in 40 mL of ethanol solution, and then 200 mg of ZIF-8-RF particles were weighed and evenly dispersed in the above mixed solution. After magnetic stirring at room temperature for 24 hours, the precipitate was collected by centrifugation, washed with ethanol solution 2 to 3 times, and finally placed in a vacuum oven at 60 ° C for 6 hours to obtain V metal salt-loaded ZIF-8-RF particles. The mass ratio of V to ZIF-8-RF is 1:100.
[0045] 4. Preparation of VN / HNPC composites modified with V single atoms with high catalytic activity The V metal salt-loaded ZIF-8-RF particles obtained in step 3 were added to a porcelain boat and placed in a tube furnace. The temperature was raised to 900 °C at a rate of 5 °C / min under an argon atmosphere. After keeping warm for 5 hours, the mixture was cooled to room temperature. The black powder material obtained was the V single atom-modified VN / HNPC composite material.
[0046] The XRD pattern of the VN / HNPC composite material with high catalytic activity modified by V single atom prepared in this example is as follows: Figure 1 As shown in the scanning electron microscope and transmission electron microscope images Figure 2 As shown in Figure 2, the nitrogen isothermal adsorption-desorption curve and pore size distribution are shown in Figure 2. Figure 3 As shown, the X-ray absorption fine structure spectrum is Figure 4 As shown. Figure 1 It can be seen that the composite material only shows the characteristic peaks belonging to graphite carbon, indicating that no metal particles and clusters are generated in the composite material; Figure 2 It can be seen that the composite material is a cubic structure with a uniform particle size of about 200-300 nm, and the carbon material is a hollow structure; Figure 3 It can be seen that the composite material has a large specific surface area (487.7870 m 2 / g); from Figure 4 It can be seen that V in the composite material exists in the form of a single atom and the coordination form is a V-N4 structure.
[0047] Example 2 This example is the preparation of Ni-N / HNPC composite material modified with Ni single atom and the performance test of its application in lithium-sulfur battery.
[0048] Different from Example 1, in the preparation process of the Ni-N / HNPC composite material modified with Ni single atom in Example 2, the preparation process of ZIF-8 and ZIF-8-RF particles is the same as the preparation process in Example 1, and ZIF-8-RF particles are obtained.
[0049] 1. Adsorption of Ni metal salt on ZIF-8-RF particles by solution impregnation Weigh 9 mg of nickel acetate (Ni(CH3COO)2·4(H2O)) and dissolve it in 40 mL of ethanol solution. Add 200 mg of ZIF-8-RF particles under stirring. After stirring for 24 hours, collect the precipitate by centrifugation, wash it three times with ethanol solution, transfer it to a vacuum oven and dry it at 60 °C for 12 hours to obtain ZIF-8-RF particles adsorbed with Ni metal salt.
[0050] 2. Preparation of Ni-N / HNPC composites modified with Ni single atoms The Ni metal salt-loaded ZIF-8-RF particles obtained in step 1 are added to a porcelain boat and placed in a tube furnace. The temperature is raised to 900 °C at a rate of 5 °C / min under an argon atmosphere. After keeping the temperature for 5 hours, the mixture is cooled to room temperature. The black powder material collected is the Ni-N / HNPC composite material modified with a single Ni atom.
[0051] The binding energy of Ni atom to Li2S6 is Figure 5 shown.
[0052] Example 3 This example is the preparation of Co-N / HNPC composite material containing Co single atom modification: Different from Example 1, in the preparation process of the Co-N / HNPC composite material modified with Co single atom in Example 3, the preparation process of ZIF-8 and ZIF-8-RF particles is the same as the preparation process in Example 1, and ZIF-8-RF particles are obtained.
[0053] 1. Adsorption of Co metal salt on ZIF-8-RF particles by solution impregnation 10 mg of cobalt nitrate hexahydrate (Co(NO3)2·6(H2O)) was weighed and dissolved in 40 mL of ethanol solution. 200 mg of ZIF-8-RF particles were added under stirring. After stirring for 24 hours, the precipitate was collected by centrifugation and finally washed three times with ethanol solution. The precipitate was transferred to a vacuum oven and dried at 60°C for 12 hours to obtain ZIF-8-RF particles adsorbed with Co metal salt.
[0054] 2. Preparation of Co-N / HNPC composites modified with Co single atoms The Ni metal salt-loaded ZIF-8-RF particles obtained in step 1 are added to a porcelain boat and placed in a tube furnace. The temperature is raised to 900 °C at a rate of 5 °C / min under an argon atmosphere. After keeping the temperature for 5 hours, the mixture is cooled to room temperature. The black powder material collected is the Co-N / HNPC composite material modified with a single Co atom.
[0055] The binding energy of Co atom to Li2S6 is Figure 5 shown.
[0056] Example 4 This example is the preparation of Fe-N / HNPC composite material containing Fe single atom modification: Different from Example 1, in the preparation process of the Fe-N / HNPC composite material modified with single Fe atoms in Example 4, the preparation process of ZIF-8 and ZIF-8-RF particles is the same as that in Example 1, and ZIF-8-RF particles are obtained.
[0057] 1. Adsorption of Fe metal salts on ZIF-8-RF particles by solution impregnation 14 mg of ferric nitrate nonahydrate (Fe(NO3)3·9(H2O)) was weighed and dissolved in 40 mL of ethanol solution. 200 mg of ZIF-8-RF particles were added under stirring. After stirring for 24 hours, the precipitate was collected by centrifugation and finally washed three times with ethanol solution. The mixture was transferred to a vacuum oven and dried at 60 °C for 12 hours to obtain ZIF-8-RF particles adsorbed with Fe metal salt.
[0058] 2. Preparation of Fe-N / HNPC composites modified with Fe single atoms The Ni metal salt-loaded ZIF-8-RF particles obtained in step 1 are added to a porcelain boat and placed in a tube furnace. The temperature is raised to 900 °C at a rate of 5 °C / min under an argon atmosphere. After being kept warm for 5 hours, the mixture is cooled to room temperature. The black powder material collected is the Fe-N / HNPC composite material modified with a single Fe atom.
[0059] The binding energy of Fe atom to Li2S6 is Figure 5 shown.
[0060] Example 5 This example is the preparation of Mn-N / HNPC composite material containing Mn single atom modification: Different from the embodiment, in the preparation process of the Mn-N / HNPC composite material modified with a single Mn atom in Comparative Example 2, the preparation process of ZIF-8 and ZIF-8-RF particles is the same as the preparation process in Example 1, and ZIF-8-RF particles are obtained.
[0061] 1. Adsorption of Mn metal salt on ZIF-8-RF particles by solution impregnation 9 mg of manganese acetate tetrahydrate (Mn(CH3COO)2·4(H2O)) was weighed and dissolved in 40 mL of ethanol solution. 200 mg of ZIF-8-RF particles were added under stirring. After stirring for 24 hours, the precipitate was collected by centrifugation and finally washed three times with ethanol solution. The mixture was transferred to a vacuum oven and dried at 60 °C for 12 hours to obtain ZIF-8-RF particles adsorbed with Mn metal salt.
[0062] 2. Preparation of Mn-N / HNPC composites modified with Mn single atoms The Mn metal salt-loaded ZIF-8-RF particles obtained in step 1 are added to a porcelain boat and placed in a tube furnace. The temperature is raised to 900 °C at a rate of 5 °C / min under an argon atmosphere. After being kept warm for 5 hours, the mixture is cooled to room temperature. The black powder material collected is the Mn-N / HNPC composite material modified with a single Mn atom.
[0063] The binding energy of Mn atom to Li2S6 is Figure 5 shown.
[0064] Application Example 1 In this application example, the VN / HNPC composite material prepared in Example 1 is used only as a positive electrode sulfur-carrying material in the field of lithium-sulfur batteries, and the specific steps are as follows: Sublimed sulfur and VN / HNPC composite materials with a mass ratio of 7:3 were weighed and placed in a mortar, and fully ground to mix evenly. The mixed materials were then placed in a glass tube and evacuated by a vacuum pump until the vacuum degree in the glass tube reached below 10 mbar and maintained for 10 minutes, and then sealed with an acetylene spray gun. The sealed glass tube was placed in an oven at 155 °C for 12 hours, and the sulfur / VN / HNPC composite material was obtained after cooling.
[0065] The obtained sulfur / VN / HNPC composite material, Super P and PVDF were mixed in a mass ratio of 8:1:1, and nitrogen methyl pyrrolidone (NMP) was used as a solvent. The materials were mixed evenly to form a slurry by ball milling. The ball milling speed was 350 r / min and the ball milling time was 2 hours. The mixed slurry was evenly coated on the carbon-coated aluminum foil current collector by a coater, and then transferred to a vacuum oven at 60 ° C for 12 hours. The coater blade height was 400 μm, and the obtained pole piece sulfur loading was 1 mg / cm 2 .
[0066] The prepared positive electrode was cut into a 12 mm diameter electrode sheet as the positive electrode, the lithium sheet as the negative electrode, a polypropylene separator (celgard 2400) as the separator, and an electrolyte containing 1 mol / L lithium bistrifluoromethanesulfonyl imide (LiTFSI) lithium salt and 1% lithium nitrate in 1,3-dioxolane (DOL) / ethylene glycol dimethyl ether (DME) (volume ratio of 1:1) solvent was added to assemble a button cell. The battery was tested for cycle performance, and the test voltage range was 1.7~2.8 V.
[0067] The binding energy of V atom to Li2S6 is Figure 5 The battery cycle performance of VN / HNPC composite material as the cathode carrier at 0.5 C is shown in Figure 7 shown.
[0068] Application Example 2 In this application example, the VN / HNPC composite material prepared in Example 1 is used as a negative electrode carrier material in a lithium-sulfur battery, and the specific steps are as follows: VN / HNPC composite material, Super P and PVDF were mixed in a mass ratio of 8:1:1, and nitrogen methyl pyrrolidone (NMP) was used as solvent. The slurry was prepared by ball milling. It was coated on the copper foil current collector by a coater and then dried in a vacuum oven at 60°C for 12 hours. The coater blade height was 400 μm and the coating surface density was 1 mg / cm 2 .
[0069] The VN / HNPC-coated copper foil obtained above was cut into a pole piece with a diameter of 12 mm as an electrode, a lithium sheet as a counter electrode, a polypropylene separator (celgard 2400) as a separator, and an electrolyte containing 1 mol / L lithium bistrifluoromethanesulfonyl imide (LiTFSI) lithium salt and 1% lithium nitrate in 1,3-dioxolane (DOL) / ethylene glycol dimethyl ether (DME) (volume ratio of 1:1) solvent was used to assemble a button cell. Symmetrical battery cycle performance test: The current density of the first three cycles was 0.2 mA / cm 2 , charge and discharge activation was performed between 0 and 1 V. Then, the 2 The current density of the pre-deposition was 5 mAh / cm 2 of lithium, and then 1 mA / cm 2 The current density is 1 mAh / cm 2 The symmetrical battery performance of VN / HNPC composite material as negative electrode carrier is shown in Figure 6 shown.
[0070] Negative electrode preparation: The current density of the first three cycles is 0.2 mA / cm 2 , charge and discharge activation was performed between 0 and 1 V, and then 0.2 mA / cm 2 Li was pre-plated on VN / HNPC at a current density of 15 mAh / cm 2 , remove the pre-lithium-plated electrode and use it as the negative electrode.
[0071] The positive electrode uses commercial carbon nanotubes as the sulfur carrier material, and a polypropylene separator (celgard2400) is used as the separator. The electrolyte containing 1 mol / L lithium bistrifluoromethanesulfonyl imide (LiTFSI) lithium salt and 1% lithium nitrate in 1,3-dioxolane (DOL) / ethylene glycol dimethyl ether (DME) (volume ratio of 1:1) solvent is added to assemble the button cell. The battery is tested for cycle performance, and the test voltage range is 1.7~2.8V.
[0072] The battery cycling performance at 0.5 C of VN / HNPC composite material as negative electrode carrier is shown in Figure 7 shown.
[0073] Application Example 3 In this application example, the VN / HNPC composite material prepared in Example 1 is used as both a positive electrode sulfur-carrying material and a negative electrode carrier material in a lithium-sulfur battery. The specific steps are as follows: The preparation process of the electrode sheet of the VN / HNPC composite material as the positive electrode sulfur-carrying material is the same as that of Application Example 1; the preparation process of the VN / HNPC composite material as the negative electrode carrier material is the same as that of Application Example 2.
[0074] The prepared positive electrode was cut into a 12 mm diameter electrode sheet as the positive electrode, the pre-lithium-plated electrode sheet was removed as the negative electrode, a polypropylene separator (celgard 2400) was used as the separator, and an electrolyte containing 1 mol / L lithium bistrifluoromethanesulfonyl imide (LiTFSI) lithium salt and 1% lithium nitrate in 1,3-dioxolane (DOL) / ethylene glycol dimethyl ether (DME) (volume ratio of 1:1) solvent was added to assemble a button cell. The battery was tested for cycle performance, and the test voltage range was 1.7~2.8 V.
[0075] The VN / HNPC composite material was used as both positive and negative electrode carrier materials in lithium-sulfur batteries. The cycle performance at a current rate of 0.5 C was as follows: Figure 7 As shown, the cycling performance at 1 C is Figure 8 shown.
[0076] like Figure 7 The VN / HNPC composite materials shown in the figure are used as positive and negative electrode carriers of lithium-sulfur batteries, and as positive and negative electrode carriers to assemble button batteries. The results show that the positive electrode material has a great influence on the battery cycle performance. When there is no negative electrode modification, the capacity of the S@VN / HNPC||Li button battery decays to 607.9 mAh / g after 200 cycles. When the VN / HNPC composite materials are used as positive and negative electrode carriers, the capacity of the S@VN / HNPC||Li@VN / HNPC button battery remains at 862.2 mAh / g after 200 cycles. Therefore, after the negative electrode modification of VN / HNPC, the cycle capacity has been significantly improved, and the capacity decay rate has been reduced.
[0077] Application Example 4 In this application example, the Ni-N / HNPC composite material prepared in Example 2 is used as both a positive electrode sulfur-carrying material and a negative electrode carrier material in a lithium-sulfur battery.
[0078] The Ni-N / HNPC composite material is used as the positive electrode carrier material, and the sulfur loading process, preparation of the positive electrode plate, assembly of the lithium-sulfur battery, and the Ni-N / HNPC composite material is used as the negative electrode carrier material, preparation of the negative electrode plate, and testing steps are the same as those in Application Example 3.
[0079] The performance of symmetric batteries assembled with Ni-N / HNPC composites as negative electrode carriers is shown in Figure 6 As shown in the figure, the Ni-N / HNPC composite material is used as both the positive and negative electrode carrier materials in lithium-sulfur batteries. The cycle performance at 1 C rate is shown in Figure 8 shown.
[0080] Comparative Example 1 Preparation of metal-free single atom carbon materials (HNPC) and performance testing of their application in lithium-sulfur batteries.
[0081] Different from Example 1, the preparation process of ZIF-8-RF particles in Comparative Example 1 is the first two steps of the preparation process of Example 1 to obtain ZIF-8-RF particles.
[0082] Preparation of nitrogen-doped carbon material free of metal single atoms: Add ZIF-8-RF particles to a porcelain boat and place it in a tube furnace. Heat the boat to 900 °C at a rate of 5 °C / min under an argon atmosphere, keep it warm for 5 hours, and then cool it to room temperature. The collected black powder material is the nitrogen-doped carbon material free of metal single atoms.
[0083] Application Comparative Example 1 The performance of symmetric batteries assembled with nitrogen-doped carbon materials without metal single atoms as negative electrode carriers is as follows Figure 6 shown.
[0084] The nitrogen-doped carbon material without metal single atoms is used as the positive electrode carrier material. The sulfur loading process, preparation of positive electrode plates, assembly of lithium-sulfur batteries, and the nitrogen-doped carbon material without metal single atoms as the negative electrode carrier material, preparation of negative electrode plates, and testing are the same as those in Application Example 3. The cycling performance at 1 C current is shown in FIG. Figure 8 shown.
[0085] like Figure 5 The figure shows the binding energy of different metal single atom catalysts to Li2S6. Figure 5 It can be concluded that V atoms have stronger interactions with Li2S6 than other metal single atoms, making them more suitable for use as catalytic materials in lithium-sulfur batteries.
[0086] like Figure 6 The symmetrical battery performance diagrams of the materials prepared in Example 1, Example 2 and Comparative Example 1, respectively, as negative electrode carriers (corresponding to Application Example 2, Application Example 4 and Comparative Example 1, respectively), at 1 mA / cm 2 Current density, 1 mAh / cm 2 At a deposition capacity of , Application Example 2 has a smaller polarization voltage and a more stable cycle than Application Example 4 and Application Comparative Example 1.
[0087] like Figure 8 The materials prepared in Example 1, Example 2 and Comparative Example 1 are shown as the positive and negative electrode carrier materials in the lithium-sulfur battery at 1 C current density. The discharge capacity of Example 3 after 200 cycles is 598.6 mAh / g, and the discharge capacity of Example 4 and Comparative Example 1 after 200 cycles is 422.8 mAh / g and 193.8 mAh / g, respectively. The discharge capacity and cycle stability of Example 3 are significantly higher than those of Example 4 and Comparative Example 1. It shows that the VN / HNPC composite material can effectively improve the electrochemical reaction kinetics and inhibit the shuttle effect of polysulfides. At the same time, it slows down the growth of lithium dendrites and enhances battery stability.
[0088] Therefore, it can be seen from the experimental data that the VN / HNPC composite material modified with a V single atom catalyst is used as a positive and negative electrode carrier material in a lithium-sulfur battery and exhibits better electrochemical performance. Therefore, the application of the VN / HNPC composite material modified with a V single atom catalyst proposed in the present invention as a positive and negative electrode carrier material in a lithium-sulfur battery is feasible.
[0089] The present invention provides a method for preparing a VN / HNPC composite material modified with a V single atom catalyst, wherein the V single atom is uniformly distributed on a porous carbon skeleton, the porous carbon material exhibits high conductivity, the VN site has high catalytic activity, and the V atom has good lithium affinity. It exhibits excellent electrochemical performance in lithium-sulfur batteries, significantly improving discharge capacity and cycle stability. It provides a new method and new ideas for solving the problems of lithium-sulfur battery shuttle effect, volume expansion, lithium dendrite growth, etc., and the preparation method has mild reaction conditions and simple process, and has good application prospects.
[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a single-atom modified porous carbon material, characterized in that: The following steps are involved: (1) Preparation of Zn-MOF particles; (2) coating Zn-MOF nanoparticles with phenolic resin (RF) to obtain Zn-MOF-RF nanoparticles; (3) The X metal salt is uniformly loaded onto the Zn-MOF-RF nanoparticles by solution impregnation method; (4) The material obtained in step (3) is carbonized at high temperature in an inert gas atmosphere to obtain a hollow porous carbon material (XN / HNPC) modified with a single X atom and having high catalytic activity.
2. The method for preparing a single-atom modified porous carbon material according to claim 1, characterized in that: The phenolic resin (RF) coating in step (2) is to uniformly disperse the Zn-MOF nanoparticles in a mixed solution of resorcinol and formaldehyde, and after magnetic stirring at room temperature for 18 to 24 hours, collect the precipitate by centrifugation or filtration, wash it with deionized water and ethanol, and dry it in a vacuum oven at 60°C for 6 to 12 hours, wherein the mass ratio of resorcinol to formaldehyde in the mixed solution is 1:150, and the mass ratio of resorcinol to Zn-MOF nanoparticles is 5:100 to 10:
100.
3. The method for preparing a single-atom modified porous carbon material according to claim 1, characterized in that: In step (3), the solution impregnation method is to uniformly disperse the Zn-MOF-RF nanoparticles in the X metal salt solution, magnetically stir at room temperature for 12 to 24 hours, collect the precipitate by centrifugation or filtration, wash it with deionized water and ethanol, and dry it in a vacuum oven at 60° C. for 6 to 12 hours, wherein the metal element X in the X metal salt solution is one or more transition metal elements, including nickel, cobalt, iron, manganese, and vanadium, the X metal salt includes acetate, nitrate, chlorate, and chloride of the X metal, the concentration of metal ions in the X metal salt solution is 0.1 to 5 mg / mL, and the mass ratio of Zn-MOF-RF nanoparticles to metal ions in the X metal salt solution is 100:0.5 to 100:
2.
4. The method for preparing a single-atom modified porous carbon material according to claim 1, characterized in that: The inert gas in step (4) is nitrogen or argon, the high temperature carbonization temperature is 900-1100°C, and the time is 2-5 hours.
5. The single-atom modified porous carbon material prepared by the preparation method according to any one of claims 1 to 4, characterized in that: Porous carbon as a carbon-based carrier material has a large specific surface area and rich pore structure. The specific surface area of the composite material is greater than 400 m 2 / g, the particle size is 200 nm~2 μm, it has rich micropore and mesopore pore structure, the mass fraction of carbon-based carrier material is 98%~99.9%, and the mass fraction of single atom catalyst is 0.1%~2%.
6. A lithium-sulfur battery, characterized in that: The positive electrode and / or negative electrode of the lithium-sulfur battery contains the single-atom-modified porous carbon material according to claim 5.
7. Use of the single-atom modified porous carbon material according to claim 6 in a lithium-sulfur battery, characterized in that: The single-atom modified porous carbon material XN / HNPC is used as a positive electrode sulfur-carrying material and / or a negative electrode carrier material.
8. The use according to claim 7, characterized in that: The single-atom modified porous carbon material XN / HNPC is used as the positive electrode sulfur-carrying material. The specific steps are as follows: 1) The sublimated sulfur and the XN / HNPC composite material are uniformly mixed in a certain proportion, and the sulfur / carbon composite cathode material is obtained by melt-filling sulfur under vacuum or inert gas atmosphere, wherein the heating temperature is 155 °C, the holding time is 12-18 hours, and the mass proportion of the single-atom-modified porous carbon material XN / HNPC in the sulfur / carbon composite cathode material is 20%-50%; 2) The sulfur / carbon composite positive electrode material, conductive agent and binder obtained in step 1) are mixed in a certain proportion, and nitrogen methyl pyrrolidone is used as a solvent. The mixture is evenly mixed to form a slurry, and then the slurry is evenly coated on the current collector, and the positive electrode sheet of the lithium-sulfur battery is obtained after vacuum drying; 3) The lithium-sulfur battery positive electrode, lithium negative electrode, separator, electrolyte and battery shell obtained in step 2) are assembled into a lithium-sulfur battery.
9. The use according to claim 7, characterized in that: The single-atom modified porous carbon material XN / HNPC is used as the negative electrode carrier material for lithium negative electrode protection. The specific steps are as follows: (1) XN / HNPC composite material was mixed with conductive agent and binder in a certain proportion, and nitrogen methyl pyrrolidone was used as solvent. The mixture was evenly mixed to form a slurry, which was then coated on copper foil. The loading amount of XN / HNPC composite material on the copper foil surface was 0.5~0.8 mg / cm 2 ; After vacuum drying, the copper foil modified with XN / HNPC composite material was used as the electrode, and the lithium sheet was used as the counter electrode. A certain capacity of lithium was deposited on the surface of the copper foil modified with XN / HNPC composite material to obtain the modified lithium negative electrode; the specific preparation method is as follows: the current density of the first three cycles is 0.2 mA / cm 2 , charge and discharge activation was performed between 0 and 1 V, and then 0.2 mA / cm 2 Li was pre-plated on XN / HNPC at a current density of 15 mAh / cm 2 , remove the pre-lithium-plated electrode piece as the negative electrode; (2) Assembling the modified lithium negative electrode obtained in step (1) and a positive electrode sheet using commercial carbon nanotubes as a sulfur carrier material, a separator and an electrolyte to obtain a lithium-sulfur battery.
10. The use according to claim 7, characterized in that: The single-atom modified porous carbon material XN / HNPC is used as a positive electrode sulfur-carrying material and a negative electrode carrier material for lithium negative electrode protection. The specific steps are as follows: (1) Sublimated sulfur and XN / HNPC composite materials are uniformly mixed in a certain proportion, and sulfur / carbon composite cathode materials are obtained by melt-filling sulfur in a vacuum or inert gas atmosphere, wherein the heating temperature is 155 °C and the holding time is 12 to 18 hours. The mass proportion of single-atom-modified porous carbon material XN / HNPC in the sulfur / carbon composite cathode material is 20% to 50%; (2) The sulfur / carbon composite positive electrode material, conductive agent and binder obtained in step 1) are mixed in a certain proportion, and nitrogen methyl pyrrolidone is used as a solvent. The mixture is evenly mixed to form a slurry, and then the slurry is evenly coated on a carbon-coated aluminum foil. After vacuum drying, a positive electrode sheet of a lithium-sulfur battery is obtained; (3) Mixing the XN / HNPC composite material with a conductive agent and a binder in a certain proportion, using nitrogen methyl pyrrolidone as a solvent, mixing them evenly to form a slurry, and then coating it on a copper foil. After vacuum drying, the copper foil modified with the XN / HNPC composite material is used as an electrode, and the lithium sheet is used as a counter electrode. A certain capacity of lithium is deposited on the surface of the copper foil modified with the XN / HNPC composite material to obtain a modified lithium negative electrode; (4) Assembling the lithium-sulfur battery positive electrode obtained in step (2) and the lithium negative electrode, separator and electrolyte obtained in step (3) into a lithium-sulfur battery.
Citation Information
Patent Citations
Method for in-situ construction of surface coating layer based on metal-organic framework material
CN112397690A
Sodium-ion battery negative electrode material
CN112467070A
Preparation method of monatomic-containing carbon material and application of monatomic-containing carbon material in lithium-sulfur battery
CN115148977A
Preparation method of carbonized Zn-MOF modified diaphragm for lithium-sulfur battery as well as product and application of carbonized Zn-MOF modified diaphragm
CN115939662A
Preparation method of high-catalytic-activity composite material and application of high-catalytic-activity composite material in lithium-sulfur battery
CN117038901A
Cited By
Preparation method of integrated phenolic resin-based monatomic catalytic electrode plate material and method for selective electrochemical hydrogenation of nitrogen heterocyclic organic matter
CN120700534A
Iron monatomic loaded cobalt phosphide nano material as well as preparation method and application thereof
CN121060572A
Phenolic resin microsphere-based porous carbon conductive composite material and preparation method thereof
CN122091301A