Nd-doped uncooled infrared detector and preparation method of nickelate ceramic for magnetic sensitivity
The Nd-doped Pr2-xNdxNiO4 ceramic target is prepared by the sol-gel method, which solves the problem of insufficient sensitivity of uncooled infrared detection devices at extreme temperatures, achieves high sensitivity and low resistivity in a wide temperature range, and is suitable for Applications of Uncooled Infrared Detectors.
Patent Information
- Application Number
- CN202410967789.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing uncooled infrared detection devices are difficult to maintain high sensitivity in extreme temperatures and room temperature environments, which limits their application scope.
The Nd-doped Pr2-xNdxNiO4 ceramic target is prepared by the sol-gel method. Through solution preparation, wet gel process, dry gel process, calcination process, powder pressing process and secondary calcination process, low resistivity, high Uncooled infrared detector materials for sensitivity and wide temperature range.
A non-toxic, non-polluting, high-density, low-resistivity ceramic sample was obtained, which has excellent room temperature resistance characteristics and temperature coefficient thermistor characteristics, and can maintain low resistivity in the temperature range of 150-350K, and maintain low resistance at room temperature. Demonstrates high sensitivity.
Smart Images

Figure CN118745114A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a Nd-doped non-refrigerated infrared detector and a method for preparing nickelate ceramics for magnetic sensitivity, belonging to the technical field of functional ceramic preparation. Background Art
[0002] With the continuous development of science and technology, the research and development of new materials has become one of the hot spots in the field of materials science. Infrared detection technology has important application value in the fields of military, security, medical treatment, etc. However, traditional refrigerated infrared detection technology has problems such as high cost, high energy consumption, and bulky size, which limits its promotion in practical applications. Non-refrigerated technology can reduce costs, improve portability, and bring new opportunities and challenges to the application of infrared detection technology. Therefore, the development of non-refrigerated infrared detection thermistors is one of the key factors to promote the continuous advancement of infrared detection technology and the expansion of its application. From VO x From traditional materials such as silicon (a-Si) and carbon nanotubes (CNTs) to new materials such as a few metal oxides, researchers pay special attention to their sensitivity, response speed and performance parameters. However, the selection of such materials is mainly based on the temperature coefficient of resistance (TCR), resistance value, noise characteristics, etc. However, it is difficult for existing uncooled infrared detection devices on the market to maintain high sensitivity requirements in both extreme temperatures and room temperature environments, which greatly limits the application of uncooled infrared detection devices. Therefore, in response to the above problems, it is urgently needed to design and prepare a thermosensitive material with low resistivity and high TCR in a wide temperature range.
[0003] Nickelates with the general structural formula A2BO4 of K2NiF4 type show very attractive and universal physical properties, such as superconductivity, magnetoresistance, mixed ion and electron conductivity, giant dielectric, low-loss microwave dielectric, thermoelectricity, etc., and have great application prospects in many energy and electronic device fields. Possible causes of various properties include coordination polyhedral distortion, charge polarization and polaron conductivity mechanism, etc. Since most of these oxides have many variable valence elements and high conductivity, their transport properties are widely studied. At present, the commonly used methods for preparing nickelates are: solid phase reaction method, sol-gel method, coprecipitation method, etc. Sol-gel method is a relatively mature means of preparing ceramic target materials. The prepared samples have high purity and uniform dispersion, low preparation cost, short preparation cycle, and can be used for mass production. Therefore, in view of the above problems, the present invention proposes to prepare a Nd-doped Pr2NiO4 ceramic target material by using sol-gel method to obtain a non-toxic, pollution-free, high-density, low-resistivity, high-TCR sensitive non-refrigerated detector reserve material with a wide temperature range. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity, and obtains a ceramic target material with low resistivity, high sensitivity and excellent comprehensive performance across room temperature, which can be used as a candidate material for an uncooled infrared detector.
[0005] The method for preparing the Nd-doped uncooled infrared detector and the nickelate ceramic for magnetic sensitivity of the present invention is characterized by comprising the following steps: (1) Solution preparation: Calculate and weigh all raw materials of praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, use the aqueous solution as the carrier of the mixed raw materials, use citric acid as the chelating agent, and use an appropriate amount of ethylene glycol as the dispersant; (2) Wet gel process: The mixed solution of step (1) is stirred in a constant temperature magnetic stirrer for reaction, and the temperature is set to about 95°C; (3) Dry gel process: the wet gel obtained in step (2) is placed in an oven to continue foaming, and then dried after the foaming is complete, to finally obtain a dry gel without precipitation; (4) Calcination process: The dry gel obtained in step (3) is ground into a powder with fine and uniform particles in an agate mortar for about 0.5 h, and then calcined once in an air atmosphere; (5) Powder pressing process: The powder obtained in step (4) is fully ground again and pressed into blocks using an automatic tablet press; (6) Secondary calcination process: calcining the block material obtained in step (5) in an air atmosphere.
[0006] Furthermore, the measurement error in step (1) is controlled within ±0.0005 g, the purity of all raw materials is AR, and the chemical formula of the prepared compound is Pr 2-x Nd x NiO4, where 0 ≤ x ≤ 0.4.
[0007] Furthermore, the gelling time of step (2) is about 1 hour, and no precipitate is formed after gelling. During the process of the mixed solution changing from a blue transparent state to a foaming, yellow fuming wet gel, the stirring speed is slowed down until it becomes a foaming wet gel state.
[0008] Furthermore, in step (3), the oven temperature is set at 140° C., and the drying time is 8-12 hours in normal pressure and air atmosphere.
[0009] Furthermore, the grinding time of step (4) is about 0.5 h, and the primary calcination is carried out in an air atmosphere at a calcination temperature of 400-800° C. and a heating rate of 1-5° C. / min.
[0010] Furthermore, in step (5), the grinding time of the precursor powder after the first calcination is about 0.5 h, the mold specification is 20 mm, the setting parameters of the automatic tablet press are 5-6 MPa, and the grinding time is about 20 min.
[0011] Furthermore, the secondary calcination temperature in step (6) is 1200-1500°C.
[0012] The beneficial effects of the present invention are: (1) The Pr prepared by the sol-gel method 2-x Nd x NiO4 ceramic target has high density of ceramic block, uniform composition and particle size distribution, stable preparation process and performance, and is non-toxic, pollution-free and easy to repeat. It has a short preparation cycle and can be used for mass production.
[0013] (2) The ceramic samples of the present invention have low resistivity (<100Ω·cm) in the temperature range of 150-350K, showing the characteristics of a typical insulator and a negative temperature coefficient thermistor. The room temperature resistivity can reach 0.06Ω·cm at best. Among them, the room temperature TCR can reach up to -4.43%·K -1 , can be maintained at -4%·K at room temperature and near room temperature -1 Up and down, compared with other NTC materials, the performance has relative advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The XRD diffraction pattern of the Nd-doped uncooled infrared detector and the nickelate ceramic for magnetic sensitivity of the present invention; Figure 2 This is the SEM spectrum of the Pr2NiO4 ceramic target obtained in Example 1 of the present invention; Figure 3 The resistance-temperature measurement curve of the Pr2NiO4 ceramic target obtained in Example 1 of the present invention; Figure 4 This is the TCR-T measurement curve of the Pr2NiO4 ceramic target obtained in Example 1 of the present invention; Figure 5 Pr obtained in Example 2 of the present invention 1.9 Ni 0.1 Resistance-temperature measurement curve of O4 ceramic target; Figure 6 Pr obtained in Example 2 of the present invention 1.9 Ni 0.1 TCR-T measurement curve of O4 ceramic target; Figure 7 Pr obtained in Example 3 of the present invention 1.8 Ni 0.2 Resistance-temperature measurement curve of O4 ceramic target; Figure 8 Pr obtained in Example 3 of the present invention 1.8 Ni 0.2 TCR-T measurement curve of O4 ceramic target; Fig. 9 Pr obtained in Example 4 of the present invention 1.7 Ni 0.3 Resistance-temperature measurement curve of O4 ceramic target; Fig.10 Pr obtained in Example 4 of the present invention 1.7 Ni 0.3 TCR-T measurement curve of O4 ceramic target; Fig.11 Pr obtained in Example 5 of the present invention 1.6 Ni 0.4 SEM image of O4 ceramic target; Fig.12 Pr obtained in Example 5 of the present invention 1.6 Ni 0.4 Resistance-temperature measurement curve of O4 ceramic target; Fig.13 Pr obtained in Example 5 of the present invention 1.6 Ni 0.4 TCR-T measurement curve of O4 ceramic target; DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0016] Example 1 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0017] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x =0) ceramic target material, weigh all raw materials including praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, and the weighing error of the raw materials is controlled within ±0.0005g, the aqueous solution is used as the carrier of the mixed raw materials, citric acid is used as the chelating agent, and an appropriate amount of ethylene glycol is used as the dispersant; (2) Wet gel process: The mixed solution of step (1) is placed in a 95°C constant temperature magnetic stirrer and stirred for 1 h. During the process of the mixed solution changing from a blue transparent state to a foaming, yellow smoke wet gel, the stirring speed is slowed down until it becomes a foaming wet gel state; (3) Dry gel process: The wet gel obtained in step (2) is placed in a constant temperature oven for further foaming at a temperature of 140°C for 8-12 hours. After the foaming is complete, the dry gel is fully dried to obtain a dry gel without precipitation. (4) Calcination process: The dry gel from step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar for about 0.5 h, and then calcined once in an air atmosphere for 8 h at a temperature of 600 °C; (400-800 °C) (5) Powder pressing process: After the powder in step (4) is fully ground again for 0.5 h, it is pressed into blocks on an automatic tablet press with a mold size of 20 mm and the parameters of the automatic tablet press set to 5-6 MPa for 20 min; (6) Secondary calcination process: Calcine the block obtained in step (5) in air atmosphere for 12 hours at a calcination temperature of 1350°C. (1200-1500°C) The Nd-doped uncooled infrared detector and magnetically sensitive nickelate ceramic obtained in Example 1 are Figure 2 The SEM spectrum shows that the crystal quality is good and the surface is dense. The room temperature resistivity is 0.13Ω·cm and the room temperature TCR reaches -3.4%·K -1 .
[0018] Example 2 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0019] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x =0.1) Ceramic target material, weigh all raw materials of praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, use aqueous solution as carrier of mixed raw materials, use citric acid as chelating agent, and use appropriate amount of ethylene glycol as dispersant; (2) Wet gel process: The mixed solution of step (1) is stirred and reacted in a constant temperature magnetic stirrer at 95°C. The mixed solution changes from a blue transparent state to a wet gel that foams and emits yellow smoke. (3) Dry gel process: the wet gel obtained in step (2) is placed in an oven to continue foaming, and then dried after the foaming is complete, to finally obtain a loose dry gel without precipitation; (4) Calcination process: The dry gel prepared in step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar for 0.5 h, and then calcined once in an air atmosphere; (5) Powder pressing process: The powder obtained in step (4) is fully ground again and pressed into blocks using an automatic tablet press; (6) Secondary calcination process: The block material obtained in step (5) is secondary calcined in an air atmosphere, the calcination holding time is 12 h, and the calcination temperature is 1350°C.
[0020] The Nd-doped uncooled infrared detector and the magnetic sensitive Pr 1.9 Nd 0.1 NiO4 nickelate ceramics, through Figure 5 and 6 The room temperature resistivity has an increasing trend, reaching 0.42 Ω·cm, and the room temperature TCR reaches -4.43%·K -1 .
[0021] Example 3 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0022] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x =0.2) ceramic target, weigh all raw materials of praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, use aqueous solution as solvent, and use citric acid and ethylene glycol as chelating agent and dispersant respectively; (2) Wet gel process: The mixed solution of step (1) is stirred in a magnetic stirrer to react until the mixed solution changes from a blue transparent state to a wet gel that foams and emits yellow smoke; (3) Dry gel process: The wet gel obtained in step (2) is placed in a 140°C oven for rapid foaming. After complete foaming, it is dried for 8-12 hours to finally obtain a precipitate-free and loose dry gel; (4) Calcination process: The dry gel prepared in step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar for 0.5 h, and then calcined once in an air atmosphere; (5) Powder pressing process: The powder obtained in step (4) is fully ground again and pressed into blocks using an automatic tablet press; (6) Secondary calcination process: The block material obtained in step (5) is secondary calcined in an air atmosphere, the calcination holding time is 12 h, and the calcination temperature is 1350°C.
[0023] The Nd-doped uncooled infrared detector and the magnetic sensitive Pr 1.8 Nd 0.2 NiO4 nickelate ceramics, through Figure 7 and 8 , the resistivity of 300K is 0.13 Ω·cm, TCR=-3.44%·K -1 In the test temperature range, the highest TCR reaches -7.13%·K -1 The corresponding temperature is 337.5K, which provides good applicable conditions for the sensitivity and response speed of uncooled infrared detectors.
[0024] Example 4 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0025] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x =0.3) ceramic target, weigh all raw materials including praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, use aqueous solution as solvent, and use citric acid and ethylene glycol as chelating agent and dispersant, respectively; (2) Wet gel process: The mixed solution of step (1) is stirred in a magnetic stirrer to react until the mixed solution changes from a blue transparent state to a wet gel that foams and emits yellow smoke; (3) Dry gel process: The wet gel obtained in step (2) is placed in a 140°C constant temperature oven for rapid foaming. After complete foaming, it is dried for 8-12 hours to finally obtain a precipitate-free and loose dry gel; (4) Calcination process: The dry gel prepared in step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar, and then calcined once in an air atmosphere; (5) Powder pressing process: The powder obtained in step (4) is fully ground again and then pressed into blocks by an automatic tablet press; (6) Secondary calcination process: The block material obtained in step (5) is secondary calcined in an air atmosphere.
[0026] The Nd-doped uncooled infrared detector and the magnetic sensitive Pr 1.7 Nd 0.3 NiO4 nickelate ceramics, through Fig. 9 and 10 , the resistivity of 300K is 0.17 Ω·cm, and the TCR is -4.29 %·K -1 .
[0027] Example 5 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0028] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x =0.4) ceramic target, weigh all raw materials of praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, use aqueous solution as solvent, and use citric acid and ethylene glycol as chelating agent and dispersant respectively; (2) Wet gel process: The mixed solution of step (1) was placed in a 95°C constant temperature magnetic stirrer and stirred for 1 h. The mixed solution changed from a blue transparent state to a wet gel with foam and yellow smoke. (3) Dry gel process: The wet gel obtained in step (2) is placed in a 140°C constant temperature oven for rapid foaming. After complete foaming, it is dried for 8 hours to finally obtain a precipitate-free and loose dry gel; (4) Calcination process: The dry gel prepared in step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar for about 0.5 h, and then calcined once in an air atmosphere for 8 h at a temperature of 400 °C; (5) Powder pressing process: After the powder in step (4) is fully ground again for 0.5 h, it is pressed into blocks by an automatic tablet press. The mold specification is 20 mm, the setting parameters of the automatic tablet press are 5 MPa, and the pressing time is about 20 min. (6) Secondary calcination process: The block material obtained in step (5) is secondary calcined in an air atmosphere at a calcination temperature of 1200°C.
[0029] The Nd-doped uncooled infrared detector and the magnetic sensitive Pr 1.6 Nd 0.4 NiO4 nickelate ceramics, by SEM spectrum Fig.11 , it can be seen that there is a precipitated phase Pr6O 11 , the element Nd increases the average grain size, resulting in lattice distortion. Among them, the room temperature resistivity reaches a minimum of 0.06 Ω·cm, and the TCR is -3.25 %·K -1 .
[0030] Example 6 The method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity described in this embodiment specifically includes the following steps.
[0031] (1) Solution preparation: Preparation of Pr by sol-gel method 2-x Nd x NiO4( x=0.4) Ceramic target material, weigh all raw materials including praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid according to the stoichiometric ratio, the weighing error of raw materials is controlled within ±0.0005g, aqueous solution is used as the carrier of mixed raw materials, citric acid is used as the chelating agent, and appropriate amount of ethylene glycol is used as the dispersant; (2) Wet gel process: The mixed solution of step (1) is placed in a 95°C constant temperature magnetic stirrer and stirred for 1 h. During the process of the mixed solution changing from a blue transparent state to a foaming, yellow smoke wet gel, the stirring speed is slowed down until it becomes a foaming wet gel state; (3) Dry gel process: The wet gel obtained in step (2) is placed in a constant temperature oven for further foaming at a temperature of 140°C for 12 hours. After the foaming is complete, the dry gel is fully dried to obtain a dry gel without precipitation. (4) Calcination process: The dry gel prepared in step (3) is ground into a precursor powder with fine and uniform particles in an agate mortar for about 0.5 h, and then calcined once in an air atmosphere for 8 h at a temperature of 800 °C; (5) Powder pressing process: After the powder in step (4) is fully ground again for 0.5 h, it is pressed into a block material under an automatic tablet press. The mold specification is 20 mm, the automatic tablet press setting parameters are 6 MPa, and the time is 20 min; (6) Secondary calcination process: The block material obtained in step (5) is calcined in an air atmosphere for 12 h at a calcination temperature of 1500°C.
[0032] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity, characterized in that: The specific steps include: (1) Solution preparation: praseodymium nitrate, neodymium nitrate, nickel nitrate and citric acid are weighed and dissolved in an aqueous solution according to the required stoichiometric ratio, and an appropriate amount of ethylene glycol is added as a dispersant to obtain a uniformly mixed solution; (2) Wet gel process: Place the uniform solution obtained in step (1) on a 95°C constant temperature magnetic stirrer and stir and heat to react; (3) Dry gel process: the wet gel obtained in step (2) is subjected to a short-term rapid foaming reaction in a constant temperature oven, and then dried to obtain a dry gel; (4) Calcination process: grinding the dry gel formed in step (3) into a powder with fine and uniform particles, and calcining it in an air atmosphere; (5) Powder pressing process: the powder formed in step (4) is fully ground again and pressed into a block material using an automatic tablet press; (6) Secondary calcination process: The block material obtained by pressing in step (5) is calcined in an air atmosphere.
2. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: In step (1), the weighing error of all raw materials is controlled within ±0.0005 g. The chemical formula of the prepared compound is Pr 2-x Nd x NiO4, where 0 ≤ x ≤ 0.
4.
3. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: The stirring and heating time in step (2) is about 1 hour. During the process in which the mixed solution changes from a blue transparent state to a foaming, yellow fuming wet gel, the stirring speed is slowed down until it becomes a foaming wet gel state.
4. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: In step (3), the temperature of the constant temperature oven is 140° C., and the drying time in normal pressure and air atmosphere is 8-12 hours.
5. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: The grinding time in step (4) is about 0.5 h, and the calcination temperature in air atmosphere is 400-800° C.
6. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: The powder grinding time in step (5) is about 0.5 h, the mold specification is 20 mm, the setting parameters of the automatic tablet press are 5-6 MPa, and the pressing time is about 20 min.
7. A method for preparing a Nd-doped uncooled infrared detector and a nickelate ceramic for magnetic sensitivity according to claim 1, characterized in that: The secondary calcination temperature in step (6) is 1200-1500°C.
Citation Information
Patent Citations
Pyroelectric infrared detector and used detecting member
CN101043065A
Composition for fuel cell electrode
US20160020470A1
Ultralow concentration sensing of bio-matter with perovskite nickelate devices and arrays
US20220025425A1
Nd-based sintered magnet and manufacturing method thereof
WO2010064578A1
Ultralow concentration sensing of BIO-matter with perovskite nickelate devices and arrays
WO2020131475A1