Preparation method of low-heat-conductivity and high-heat-preservation carbon-carbon composite porous material capable of being used at various temperatures
Through the composite processing of viscose fiber, carbon fiber and graphite fiber, the problems of high thermal conductivity and poor stability of existing high-temperature resistant materials are solved, and low thermal conductivity and high thermal insulation carbon-carbon composite porous materials suitable for various temperatures are prepared. Improved stability and applicability at high temperatures are achieved.
Patent Information
- Application Number
- CN202410737377.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing high-temperature insulation materials have high thermal conductivity, poor stability, difficult to control pore density, insufficient strength, and short service life, making them difficult to be suitable for high-temperature applications at various temperatures.
Using viscose fiber, carbon fiber and graphite fiber composite, through two steps of carbonization and graphitization, the pore size and density are adjusted to prepare a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation, ensuring the stability and applicability of the material at high temperatures. sex.
It achieves low thermal conductivity at a variety of temperatures. The thermal conductivity is significantly reduced at both normal and high temperatures. The pore size of the material is evenly distributed and the strength is improved. It is suitable for high temperature applications up to 3000°C and extends the service life.
Smart Images

Figure CN118745117A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a carbon-carbon composite porous material. Background Art
[0002] With the development of society and the advancement of technology, more and more new materials research and development and production processes need to be carried out at high temperatures. Therefore, thermal insulation materials that can be used at various temperatures, especially at higher temperatures, have become an indispensable basic material for modern industrial technology, and play an important role in the development of glass, ceramics, crystal growth, and more new materials.
[0003] Carbon / graphite materials have good physical and chemical stability and excellent thermal vibration resistance, and have long been introduced and applied to thermal vibration and corrosion resistant refractory materials. They are widely used as lining materials for converters, electric furnaces, ladles, etc. for steel smelting.
[0004] Porous materials play an important role in thermal insulation materials, and the porosity and distribution of the materials play an important role in the thermal insulation performance.
[0005] At present, the existing high-temperature resistant thermal insulation materials have the disadvantages of high thermal conductivity, poor stability at high temperatures, difficulty in accurately controlling the pore density and material density of porous materials, poor strength, and short service life.
[0006] Therefore, it is of great practical significance to develop porous carbon materials with lower thermal conductivity, adjustable porosity and density, and certain strength. Summary of the invention
[0007] In view of the deficiencies and shortcomings in the prior art, the present invention provides a method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures.
[0008] A method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures is specifically completed by the following steps:
[0009] 1. Carbonization:
[0010] First, the viscose fiber is placed in a high-temperature furnace with protective gas, and then the high-temperature furnace is heated to 600℃~800℃, and then carbonized at 600℃~800℃ for a period of time to obtain carbon fiber;
[0011] 2. preparing the viscose fiber, the carbon fiber prepared in step 1 and the graphite fiber into short fibers respectively, to obtain viscose short fibers, carbon short fibers and graphite short fibers;
[0012] 3. The viscose staple fibers, carbon staple fibers and graphite staple fibers are respectively removed from the materials by a demagnetizer to remove magnetic particles, and then put into a mixer together with the resin according to the required proportion and mix evenly to obtain a mixture;
[0013] 4. Filling the mixture obtained in step 3 into a mold for pressing to obtain a pressed mixture;
[0014] 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block;
[0015] 6. Put the solidified pressed block into a carbonization furnace for carbonization, and then put the carbonized pressed block into a graphitization furnace for graphitization treatment to obtain a low thermal conductivity and high thermal insulation carbon-carbon composite porous material that can be used at various temperatures.
[0016] Beneficial effects of the present invention:
[0017] 1. The present invention provides a method for preparing a porous carbon material by compounding viscose fiber, carbon fiber and graphite fiber. The method can adjust the pore size of the prepared carbon material as needed;
[0018] 2. The present invention processes the pressed material through two steps of carbonization and graphitization, thereby avoiding the damage to the material structure caused by the uncontrolled escape of volatile components during the carbonization process, and ensuring that a carbon-carbon composite porous material with uniform pore size distribution is obtained after graphitization;
[0019] 3. The present invention can realize controllable preparation of porous carbon materials by adjusting factors such as raw material size and ratio, and can expand the application field and scope of the porous carbon materials;
[0020] 4. When the porous carbon material prepared by the present invention is used as a thermal insulation material, the thermal conductivity is not higher than 0.25 W / mK at room temperature (25°C) and not higher than 0.70 W / mK at high temperature (2000°C);
[0021] 5. The porous carbon material prepared by the present invention can be processed into the required size and shape according to the needs of different usage scenarios, which is convenient for use;
[0022] 6. The porous carbon material prepared by the present invention can be used for high-temperature applications up to 3000°C, has stable physical and chemical properties, is suitable for applications with high environmental requirements, and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the viscose fiber described in step 1 of Example 1;
[0024] Figure 2 This is a SEM image of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures and is prepared in Example 1;
[0025] Figure 3The thermal conductivity test results of the carbon-carbon composite porous material with low thermal conductivity and high thermal insulation at various temperatures prepared in Example 1 are as follows;
[0026] Figure 4 This is a SEM image of the carbon-carbon composite porous material prepared in Comparative Example 1;
[0027] Figure 5 This is a SEM image of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures and is prepared in Example 2;
[0028] Figure 6 This is a SEM image of the low thermal conductivity, high thermal insulation carbon-carbon composite porous material prepared in Example 3 and can be used at various temperatures. DETAILED DESCRIPTION
[0029] Specific implementation method 1: This implementation method is a method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures, which is specifically completed in the following steps:
[0030] 1. Carbonization:
[0031] First, the viscose fiber is placed in a high-temperature furnace with protective gas, and then the high-temperature furnace is heated to 600℃~800℃, and then carbonized at 600℃~800℃ for a period of time to obtain carbon fiber;
[0032] 2. preparing the viscose fiber, the carbon fiber prepared in step 1 and the graphite fiber into short fibers respectively, to obtain viscose short fibers, carbon short fibers and graphite short fibers;
[0033] 3. The viscose staple fibers, carbon staple fibers and graphite staple fibers are respectively removed from the materials by a demagnetizer to remove magnetic particles, and then put into a mixer together with the resin according to the required proportion and mix evenly to obtain a mixture;
[0034] 4. Filling the mixture obtained in step 3 into a mold for pressing to obtain a pressed mixture;
[0035] 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block;
[0036] 6. Put the solidified pressed block into a carbonization furnace for carbonization, and then put the carbonized pressed block into a graphitization furnace for graphitization treatment to obtain a low thermal conductivity and high thermal insulation carbon-carbon composite porous material that can be used at various temperatures.
[0037] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the protective gas in step 1 is one or a mixture of nitrogen and argon. The other steps are the same as those in specific implementation method 1.
[0038] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the heating rate in step 1 is 50°C / h to 55°C / h; the carbonization time in step 1 is not less than 10 hours. The other steps are the same as those in specific implementation method 1 or 2.
[0039] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the size of the viscose staple fibers in step 2 is 4 mm to 8 mm; the size of the carbon staple fibers in step 2 is 5 mm to 9 mm; the size of the graphite staple fibers in step 2 is 2 mm to 5 mm. The other steps are the same as those in specific embodiments 1 to 3.
[0040] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the mass ratio of viscose staple fibers, carbon staple fibers and graphite staple fibers described in step 3 is (10-20):(40-80):(10-40). The other steps are the same as those of specific embodiments 1 to 4.
[0041] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the mass of the resin described in step 3 accounts for 10% to 30% of the total mass of the viscose short fibers, carbon short fibers and graphite short fibers. The other steps are the same as specific implementation methods 1 to 5.
[0042] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the resin described in step 3 is phenolic resin, acrylic resin or polyurethane resin. The other steps are the same as those of specific embodiments 1 to 6.
[0043] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the curing temperature in step 5 is 200° C. to 210° C., and the curing time is not less than 100 hours. The other steps are the same as those of specific embodiments 1 to 7.
[0044] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the carbonization temperature in step 6 is 600°C to 800°C, and the carbonization time is not less than 50 hours; the graphitization temperature in step 6 is 2200°C to 2500°C, and the graphitization time is not less than 72 hours. The other steps are the same as those in specific embodiments 1 to 8.
[0045] Specific embodiment ten: This embodiment is a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures as a low thermal conductivity thermal insulation material or a high temperature resistant material.
[0046] The following examples are used to verify the beneficial effects of the present invention:
[0047] Example 1: A method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures, which is specifically completed by the following steps:
[0048] 1. Carbonization:
[0049] First, the viscose fiber is placed in a high-temperature furnace filled with nitrogen, and then the high-temperature furnace is heated to 700°C at a heating rate of 50°C / h, and then carbonized at 700°C for 10 hours to obtain carbon fiber;
[0050] 2. Using a crusher, the viscose fiber, the carbon fiber prepared in step 1, and the graphite fiber are respectively prepared into short fibers to obtain viscose short fibers, carbon short fibers, and graphite short fibers;
[0051] The size of the viscose staple fibers described in step 2 is 5 mm;
[0052] The size of the carbon short fibers described in step 2 is 7 mm;
[0053] The size of the graphite short fibers described in step 2 is 4 mm;
[0054] 3. The viscose staple fibers, carbon staple fibers and graphite staple fibers are respectively removed from the materials by a demagnetizer, and then put into a mixer together with phenolic resin particles (PR12603) according to the required proportion and mixed evenly to obtain a mixture;
[0055] The mass ratio of the viscose staple fibers, carbon staple fibers and graphite staple fibers described in step 3 is 10:50:40;
[0056] The mass of the phenolic resin described in step 3 accounts for 15% of the total mass of the viscose staple fibers, carbon staple fibers and graphite staple fibers;
[0057] 4. Filling the mixture obtained in step 3 into a mold for pressing to obtain a pressed mixture;
[0058] The size of the mold described in step 4 is 50cm×30cm×20cm;
[0059] 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block;
[0060] The curing temperature in step 5 is 210° C. and the curing time is 110 h.
[0061] 6. Put the solidified pressed block into a carbonization furnace for carbonization, and then put the carbonized pressed block into a graphitization furnace for graphitization treatment to obtain a low thermal conductivity and high thermal insulation carbon-carbon composite porous material that can be used at various temperatures;
[0062] The carbonization temperature in step 6 is 700°C and the carbonization time is 60h;
[0063] The temperature of the graphitization treatment in step six is 2500° C., and the time of the graphitization treatment is 72 hours.
[0064] Figure 1 This is a SEM image of the viscose fiber described in step 1 of Example 1;
[0065] Figure 2 This is a SEM image of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures and is prepared in Example 1;
[0066] from Figure 1 It can be seen that the viscose fiber raw material is a long fiber with uniform fiber diameter and smooth surface, and is in a randomly stacked state.
[0067] from Figure 2 It can be seen that in the prepared carbon-carbon composite porous material, the size of the carbon fiber is about 20-100 μm, and the short fibers are bonded and stacked to form a porous structure.
[0068] The low thermal conductivity and high thermal insulation carbon-carbon composite porous material prepared in Example 1 and used at various temperatures was cut into 50×50×20 mm 3 The test sample blocks were tested for thermal conductivity at room temperature (25°C), 400°C, 800°C, 1200°C, 1600°C and 2000°C. Figure 3 Thermal conductivity test results.
[0069] Figure 3 The thermal conductivity test results of the carbon-carbon composite porous material with low thermal conductivity and high thermal insulation which can be used at various temperatures prepared in Example 1 at different temperatures;
[0070] The test results show that the thermal conductivity of the carbon-carbon composite porous material prepared by the present invention increases with the increase of the test temperature. The thermal conductivity at room temperature is 0.21 W / mK (see Table 1), and the thermal conductivity at 2000°C is 0.61 W / mK.
[0071] Comparative Example 1: A method for preparing a carbon-carbon composite porous material is specifically completed by the following steps:
[0072] 1. Carbonization:
[0073] First, the viscose fiber is placed in a high-temperature furnace filled with nitrogen, and then the high-temperature furnace is heated to 700°C at a heating rate of 50°C / h, and then carbonized at 700°C for 10 hours to obtain carbon fiber;
[0074] 2. Using a crusher, the viscose fiber, the carbon fiber prepared in step 1, and the graphite fiber are respectively prepared into short fibers to obtain viscose short fibers, carbon short fibers, and graphite short fibers;
[0075] The size of the viscose staple fibers described in step 2 is 9 mm;
[0076] The size of the carbon short fibers described in step 2 is 9 mm;
[0077] The size of the graphite short fibers described in step 2 is 6 mm;
[0078] 3. The viscose staple fibers, carbon staple fibers and graphite staple fibers are respectively removed from the materials by a demagnetizer, and then put into a mixer together with phenolic resin particles (PR12603) according to the required proportion and mixed evenly to obtain a mixture;
[0079] The mass ratio of the viscose staple fibers, carbon staple fibers and graphite staple fibers described in step 3 is 30:50:20;
[0080] The mass of the phenolic resin described in step 3 accounts for 15% of the total mass of the viscose staple fibers, carbon staple fibers and graphite staple fibers;
[0081] 4. Filling the mixture obtained in step 3 into a mold through a distribution device for pressing to obtain a pressed mixture;
[0082] The size of the mold described in step 4 is 50cm×30cm×20cm;
[0083] 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block;
[0084] The curing temperature in step 5 is 210° C. and the curing time is 110 h.
[0085] 6. Put the solidified pressed block into a carbonization furnace for carbonization, and then put the carbonized pressed block into a graphitization furnace for graphitization treatment to obtain a low thermal conductivity and high thermal insulation carbon-carbon composite porous material that can be used at various temperatures;
[0086] The carbonization temperature in step 6 is 700°C and the carbonization time is 60h;
[0087] The temperature of the graphitization treatment in step six is 2500° C., and the time of the graphitization treatment is 72 hours.
[0088] Figure 4 This is a SEM image of the carbon-carbon composite porous material prepared in Comparative Example 1;
[0089] from Figure 4 It can be seen that the carbon-carbon composite porous material prepared in Control Example 1 has obvious agglomeration phenomenon.
[0090] The thermal conductivity of the carbon-carbon composite porous material prepared in Comparative Example 1 is 0.35 W / mK at room temperature (see Table 1).
[0091] Comparative Example 2: A method for preparing a carbon-carbon composite porous material is specifically completed by the following steps:
[0092] 1. Carbonization:
[0093] First, the viscose fiber is placed in a high-temperature furnace filled with nitrogen, and then the high-temperature furnace is heated to 700°C at a heating rate of 50°C / h, and then carbonized at 700°C for 10 hours to obtain carbon fiber;
[0094] 2. Using a crusher, the polyester fiber, the carbon fiber prepared in step 1, and the graphite fiber are respectively prepared into short fibers to obtain polyester short fibers, carbon short fibers, and graphite short fibers;
[0095] The size of the polyester staple fiber described in step 2 is 5 mm;
[0096] The size of the carbon short fibers described in step 2 is 7 mm;
[0097] The size of the graphite short fibers described in step 2 is 4 mm;
[0098] 3. The polyester short fibers, carbon short fibers and graphite short fibers are respectively removed from the materials by a demagnetizer to remove magnetic particles, and then put into a mixer together with phenolic resin particles (PR12603) according to the required proportion and mix evenly to obtain a mixture;
[0099] The mass ratio of the polyester short fibers, carbon short fibers and graphite short fibers described in step 3 is 10:50:40;
[0100] The mass of the phenolic resin described in step 3 accounts for 15% of the total mass of the viscose staple fibers, carbon staple fibers and graphite staple fibers;
[0101] 4. Filling the mixture obtained in step 3 into a mold through a distribution device for pressing to obtain a pressed mixture;
[0102] The size of the mold described in step 4 is 50cm×30cm×20cm;
[0103] 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block;
[0104] The curing temperature in step 5 is 210° C. and the curing time is 110 h.
[0105] 6. Put the solidified pressed blocks into a carbonization furnace for carbonization; after carbonization, cool to room temperature;
[0106] The carbonization temperature in step 6 is 700°C and the carbonization time is 60h;
[0107] During the carbonization process, the polyester fibers in the solidified pressed blocks melt and decompose to produce an aromatic smell and black smoke, making it difficult to carry out subsequent processes, and a porous structure cannot be effectively formed, so that a carbon-carbon composite porous material cannot be obtained.
[0108] Example 2: The difference between this example and Example 1 is that the size of the viscose staple fiber described in step 2 is 6 mm; the size of the carbon staple fiber described in step 2 is 8 mm; the size of the graphite staple fiber described in step 2 is 4 mm; the mass ratio of the viscose staple fiber, the carbon staple fiber and the graphite staple fiber described in step 3 is 20:40:40; the mass of the phenolic resin described in step 3 accounts for 20% of the total mass of the viscose staple fiber, the carbon staple fiber and the graphite staple fiber. The other steps and parameters are the same as those in Example 1.
[0109] Figure 5 This is a SEM image of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures and is prepared in Example 2;
[0110] from Figure 5 It can be seen that the low thermal conductivity and high thermal insulation carbon-carbon composite porous material prepared in Example 2 and applicable to various temperatures is almost the same as that in Example 1 and is at the same level.
[0111] After testing, the room temperature thermal conductivity of the carbon-carbon composite porous material prepared in Example 2 is 0.22 W / mK, which is almost the same as that in Example 1 and is at the same level.
[0112] Example 3: The difference between this example and Example 1 is that in step 1, the viscose fiber is first loaded into a high-temperature furnace filled with nitrogen and argon (the volume ratio of nitrogen and argon is 9:1), and then the high-temperature furnace is heated to 700°C at a heating rate of 50°C / h, and then carbonized at 700°C for 10 hours to obtain carbon fiber; the size of the viscose staple fiber described in step 2 is 4mm; the size of the carbon staple fiber described in step 2 is 5mm; the size of the graphite staple fiber described in step 2 is 3mm; the mass ratio of the viscose staple fiber, carbon staple fiber and graphite staple fiber described in step 3 is 10:80:10; the mass of the phenolic resin described in step 3 accounts for 20% of the total mass of the viscose staple fiber, carbon staple fiber and graphite staple fiber. Other steps and parameters are the same as those in Example 1.
[0113] Figure 6 This is a SEM image of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures and is prepared in Example 3;
[0114] from Figure 6It can be seen that the low thermal conductivity and high thermal insulation carbon-carbon composite porous material prepared in Example 3 and applicable to various temperatures is almost the same as that in Example 1 and is at the same level.
[0115] After testing, the room temperature thermal conductivity of the carbon-carbon composite porous material prepared in Example 2 is 0.22 W / mK, which is almost the same as that in Example 1 and is at the same level.
[0116] Table 1
[0117]
Claims
1. A method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures, characterized in that The preparation method is specifically completed according to the following steps:
1. Carbonization: First, the viscose fiber is placed in a high-temperature furnace with protective gas, and then the high-temperature furnace is heated to 600℃~800℃, and then carbonized at 600℃~800℃ for a period of time to obtain carbon fiber; 2. preparing the viscose fiber, the carbon fiber prepared in step 1 and the graphite fiber into short fibers respectively, to obtain viscose short fibers, carbon short fibers and graphite short fibers; 3. The viscose staple fibers, carbon staple fibers and graphite staple fibers are respectively removed from the materials by a demagnetizer to remove magnetic particles, and then put into a mixer together with the resin according to the required proportion and mix evenly to obtain a mixture; 4. Filling the mixture obtained in step 3 into a mold for pressing to obtain a pressed mixture; 5. Put the pressed mixed material into a box furnace for curing to obtain a cured pressed block; 6. Put the solidified pressed block into a carbonization furnace for carbonization, and then put the carbonized pressed block into a graphitization furnace for graphitization treatment to obtain a low thermal conductivity and high thermal insulation carbon-carbon composite porous material that can be used at various temperatures.
2. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The protective gas described in step 1 is one or a mixture of nitrogen and argon.
3. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The heating rate in step 1 is 50°C / h to 55°C / h; the carbonization time in step 1 is not less than 10 hours.
4. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The size of the viscose staple fibers described in step 2 is 4 mm to 8 mm; the size of the carbon staple fibers described in step 2 is 5 mm to 9 mm; the size of the graphite staple fibers described in step 2 is 2 mm to 5 mm.
5. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The mass ratio of the viscose staple fibers, carbon staple fibers and graphite staple fibers described in step three is (10-20):(40-80):(10-40).
6. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The mass of the resin described in step three accounts for 10% to 30% of the total mass of the viscose staple fibers, carbon staple fibers and graphite staple fibers.
7. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The resin described in step 3 is phenolic resin, acrylic resin or polyurethane resin.
8. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The curing temperature in step 5 is 200° C. to 210° C., and the curing time is not less than 100 hours.
9. The method for preparing a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures according to claim 1, characterized in that The carbonization temperature in step six is 600° C. to 800° C., and the carbonization time is not less than 50 hours; the graphitization temperature in step six is 2200° C. to 2500° C., and the graphitization time is not less than 72 hours.
10. Application of a carbon-carbon composite porous material with low thermal conductivity and high thermal insulation that can be used at various temperatures prepared by the preparation method according to claim 1, characterized in that A carbon-carbon composite porous material with low thermal conductivity and high thermal insulation can be used at various temperatures as a low thermal conductivity thermal insulation material or a high temperature resistant material.
Citation Information
Patent Citations
Method for manufacturing high-density rigid carbon-fiber heat-insulation material
CN101628816A
Compound thermal insulation material manufactured by using waste fibers and manufacturing method thereof
CN103467000A
Electrode material made of waste fibers and manufacturing method thereof
CN103474125A
Fast preparation method of carbon fiber reinforcement
CN104894869A
Preparation method of high-temperature furnace hardening insulation material
CN105541365A
Cited By
High-purity low-thermal-conductivity low-density carbon fiber / carbon composite thermal field material and preparation method thereof
CN119822863A
A high-purity, low-thermal-conductivity and low-density carbon fiber / carbon composite thermal field material and its preparation method
CN119822863B
Carbon fiber reinforced porous resin carbon thermal insulation material as well as preparation method and application thereof
CN120504549A
High-purity low-thermal-conductivity low-density carbon fiber / carbon composite thermal field material and preparation method therefor
WO2026194309A1