Polyfunctional group UV resin, UV hydrolysis glue composition containing polyfunctional group UV resin and preparation method of polyfunctional group UV hydrolysis glue composition

By using multi-functional UV resin in UV hydrolyzable glue and adjusting the proportion of the composition, combined with high refractive index and hydrophilic monomers, the problems of slow curing and difficult balance of UV hydrolyzable glue in multi-layer electronic glass are solved, achieving rapid Curing and deep curing improve processing efficiency and hydrolysis resistance.

CN118745142AActive Publication Date: 2024-10-08HEFEI MICROCRYSTALLINE MATERIALS TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410731614.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Existing UV hydrolyzable adhesives are slow to cure and wrinkle in deep curing in multi-layer thinned electronic glass, and it is difficult to balance the need to resist hydrolysis in hot water after one curing and deep curing again, resulting in low processing efficiency and high damage rate. .

Method used

Using multifunctional UV resin and adjusting the proportion of each component in the UV hydrolyzable gum composition, the multifunctional UV resin is prepared through chemical reaction, and combined with two-functional high refractive index UV resin, hydrophilic UV monomer, hydrophobic UV monomer, Photoinitiator and wrinkle auxiliary form a UV hydrolyzable glue composition with excellent hydrolysis resistance and rapid curing.

Benefits of technology

It achieves rapid curing under lower exposure conditions, improves hydrolysis resistance and deep curing effect, solves the problem of light loss and balance during the curing process, and improves processing efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745142A_ABST
    Figure CN118745142A_ABST
Patent Text Reader

Abstract

The invention discloses a multifunctional UV (ultraviolet) resin which is synthesized by reacting the following resins and monomers, the molar ratio of the monomer C to the resin A to the monomer B is controlled to be (3-4): 1: (4-4.02), and the structure of the multifunctional UV resin is shown in the specification. The invention also discloses a UV hydrolytic adhesive composition which comprises the multifunctional UV resin, bifunctional high-refractive-index UV resin, a hydrophilic UV monomer, a hydrophobic UV monomer, a photoinitiator and a wrinkling auxiliary agent, and by adding the synthesized multifunctional UV resin and regulating and controlling the proportion of all the components in the UV hydrolytic adhesive composition, the wrinkling auxiliary agent can be prepared into the multifunctional UV hydrolytic adhesive composition. On one hand, the problem that the UV hydrolysis glue is relatively slow in curing and deep curing wrinkling in the multi-layer thinned electronic glass is solved, and on the other hand, the problem that the UV hydrolysis glue needs to resist hydrolysis in hot water after being cured for one time and needs to be quickly hydrolyzed after being subjected to deep curing wrinkling again after being cured for one time, and the two are difficult to balance is solved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of UV adhesives, in particular to a multifunctional UV resin and a UV hydrolyzed adhesive composition containing the same and a preparation method thereof. Background Art

[0002] Electronic glass is a high-tech glass product used in the fields of electronics, microelectronics and optoelectronics. The current development of technology and application is mainly reflected in the display glass and protective cover glass of terminal display products such as mobile phones, tablet computers, LCD TVs, touch screens, etc. With the development of information technology and the upgrading of consumer demand, people's requirements for thinner and lighter display terminals are also increasing. Therefore, thinned electronic glass is an important way to achieve thinner and lighter display terminal products.

[0003] CNC grinding is one of the commonly used methods in the electronic glass deep processing industry. However, thinned electronic glass will result in low processing efficiency and high damage rate when processed in a single piece. The lamination process is to bond multiple layers of thinned electronic glass with UV hydrolyzed glue, fix them with UV irradiation, and then uniformly perform CNC grinding, and then perform UV deep curing and wrinkling, and then hydrolyze and remove the UV glue, so that the laminated multi-layer glass falls off layer by layer to form a single piece.

[0004] However, the current UV hydrolyzed adhesive has the following problems in laminating multi-layer thinned electronic glass:

[0005] 1. UV hydrolyzed adhesive is slow to cure and deep cure in multi-layer thinned electronic glass, requiring higher irradiation energy and longer irradiation time;

[0006] 2. It is difficult to strike a balance between the need for UV hydrolyzed glue to be resistant to hydrolysis in hot water after one-time curing and the need for rapid hydrolysis after another deep curing and wrinkling after one-time curing.

[0007] Therefore, it is urgent to provide a novel UV hydrolyzed adhesive to solve the above problems. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a multifunctional UV resin and a UV hydrolyzed adhesive composition containing the same and a preparation method thereof. By adding the synthesized multifunctional UV resin and adjusting the proportion of each component in the UV hydrolyzed adhesive composition, on the one hand, the problem of slow curing and deep curing wrinkling of UV hydrolyzed adhesive in multi-layer thinned electronic glass is solved; on the other hand, the problem of difficult balance between the need for UV hydrolyzed adhesive to resist hydrolysis in hot water after one-time curing and the need for rapid hydrolysis after deep curing and wrinkling of UV hydrolyzed adhesive after one-time curing is solved.

[0009] In order to solve the above technical problems, the first technical solution adopted by the present invention is: to provide a multifunctional UV resin, the structural formula of which is as follows:

[0010]

[0011] Wherein, R3 is H or methyl, R4 is H or methyl, and the structure of R1 is as follows:

[0012]

[0013] R2 is the following structure and contains at least H, or all are the following structures:

[0014]

[0015] In order to solve the above technical problems, the second technical solution adopted by the present invention is: to provide a method for preparing the multifunctional UV resin as described above, comprising the following steps:

[0016] Step 1: Add resin A into a container, heat to 100°C, first add 25% of the total mass of monomer B and inhibitor D, and then heat to 109-111°C again to obtain a first reaction solution; wherein the structure of the resin A is as follows:

[0017]

[0018] The structure of the monomer B is as follows:

[0019]

[0020] Wherein, R3 is H or methyl;

[0021] Step 2: Add a catalyst to the first reaction liquid, and slowly dropwise add the remaining mass of monomer B. In this stage, the reaction temperature is controlled at 110-125° C. to obtain a second reaction liquid;

[0022] Step 3: heating the second reaction liquid to 125-135° C., keeping the temperature for reaction, sampling and measuring the acid value until the acid value remains substantially unchanged to obtain a third reaction liquid;

[0023] Step 4: Cool the third reaction solution to 60-80° C., add polymerization inhibitor E and monomer C, react for 1-3 hours, and cool to room temperature to obtain the multifunctional UV resin; wherein the structure of monomer C is as follows:

[0024]

[0025] Wherein, R4 is H or methyl.

[0026] Chemical reaction equation:

[0027]

[0028] In a preferred embodiment of the present invention, the molar ratio of the resin A to the monomer B is 1:(4-4.02).

[0029] In a preferred embodiment of the present invention, the polymerization inhibitor D is methyl hydroquinone, and the added amount is 0.05% of the total mass of the resin A and the monomer B.

[0030] In a preferred embodiment of the present invention, the polymerization inhibitor E is one of hydroquinone, p-hydroxyanisole, 2-tert-butylhydroquinone and 2,5-di-tert-butylhydroquinone, and the added amount is 0.2% of the total mass of the resin A and the monomer B.

[0031] In a preferred embodiment of the present invention, the catalyst is triphenylphosphine, and the added amount is 0.25% of the total mass of the resin A and the monomer B.

[0032] In a preferred embodiment of the present invention, the molar ratio of the monomer C to the resin A is (3-4):1.

[0033] In order to solve the above technical problems, the third technical solution adopted by the present invention is: to provide a UV hydrolyzed adhesive composition, comprising the multifunctional UV resin as described above, and comprising the following components by weight:

[0034]

[0035]

[0036] In a preferred embodiment of the present invention, the difunctional high refractive index UV resin is selected from one of Youyang Trust-6601 and Youyang Trust-6602; the hydrophilic UV monomer is one of polyethylene glycol (600) dimethacrylate (PEG (600) DMA), methoxy polyethylene glycol methacrylate, and ethoxy polyethylene glycol methacrylate; the hydrophobic UV monomer is at least one of dicyclopentadiene acrylate (DCPA), isobornyl methacrylate (IBOMA), trimethylolpropane triacrylate (TMPTA), dipentaerythritol hexaacrylate (DPHA), and tris (2-hydroxyethyl) isocyanuric acid triacrylate (THEICTA).

[0037] In a preferred embodiment of the present invention, the photoinitiator is at least one of photoinitiator 1173, photoinitiator 651, photoinitiator 819, and photoinitiator ITX; the wrinkling aid is one of azobisisobutyronitrile (AIBN) and benzoyl peroxide (BPO).

[0038] The beneficial effects of the present invention are:

[0039] (1) The present invention provides a multifunctional resin, wherein the four double bonds at both ends of the molecular chain are extremely active and can be rapidly cured under low exposure conditions to obtain a polymer having excellent hydrolysis resistance. In addition, a double bond monomer containing -NCO groups is further used to carry out a grafting reaction with the secondary hydroxyl groups in the resin, thereby increasing the number of double bonds and thus increasing the functionality of the resin system. On the one hand, the crosslinking density is increased, thereby further improving the hydrolysis resistance. On the other hand, the curing shrinkage of the resin system is enhanced, thereby promoting the wrinkling effect.

[0040] (2) The present invention provides a UV hydrolyzed adhesive composition, which, in addition to the multifunctional UV resin described above, also includes a difunctional high-refractive-index UV resin, a hydrophilic UV monomer, a hydrophobic UV monomer, a photoinitiator, and a wrinkling aid. Among them, the difunctional high-refractive-index UV resin used has a refractive index close to the refractive index of glass (1.50), which is beneficial to the effective penetration of UV light during the UV light curing process of the multi-layer thinned electronic glass with good lamination, thereby reducing light loss and further facilitating deep curing. During the deep curing process, the temperature of the sample will rapidly rise to above 120°C under the irradiation of high-energy UV light. At this time, the wrinkling aid contained in the system will rapidly decompose to produce N2 or CO2, which will help wrinkling and reduce the bonding strength of the film;

[0041] (3) The present invention solves the problem that the UV hydrolyzed adhesive is slow to cure and wrinkle in multi-layer thinned electronic glass during deep curing. On the other hand, it solves the problem that it is difficult to balance the need for the UV hydrolyzed adhesive to resist hydrolysis in hot water after one-time curing and the need for rapid hydrolysis after deep curing and wrinkling after one-time curing.

[0042] (4) The preparation method provided by the present invention has a simple operation process and the raw materials are easy to purchase, and can be produced and prepared on a large scale. DETAILED DESCRIPTION

[0043] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0044] Embodiments of the present invention include:

[0045] Embodiment 1:

[0046] A method for preparing a multifunctional UV resin comprises the following steps:

[0047] Put 192.10g of resin A into a 1L four-necked flask (kettle) equipped with a mechanical stirring device, place it in an oil bath for heating, and set the oil bath temperature to 100℃. When the mechanical stirring device can be turned smoothly manually, turn on the mechanical stirring device. Then weigh 146.2g of monomer B (methacrylic acid is used in this example), and control the molar ratio of resin A to monomer B (methacrylic acid) to be 1:4. When the temperature in the four-necked flask (kettle) rises to 100℃, add 25% of the total mass of monomer B (methacrylic acid), that is, 36.55g, and 0.17g of methylhydroquinone, and set the oil bath temperature to 110℃. Then, the remaining 109.65 g of monomer B (methacrylic acid) was added to the constant pressure dropping funnel. When the temperature in the four-necked flask (kettle) rose to 110° C., 0.85 g of triphenylphosphine was added, and then the valve of the constant pressure dropping funnel was slowly opened to allow monomer B (methacrylic acid) to slowly drip into the four-necked flask (kettle). Since the reaction was an exothermic reaction, the temperature in the four-necked flask (kettle) needed to be controlled at 110-115° C. After the monomer B (methacrylic acid) was dripped, the oil bath temperature was set to 125° C. When the temperature in the four-necked flask (kettle) rose to 125° C., the reaction was kept warm, and the acid value was measured by sampling until the acid value was substantially 0, and the reaction was completed.

[0048] The four-necked flask (kettle) was taken out from the oil bath and cooled naturally in the air. When the temperature in the four-necked flask (kettle) dropped to 80°C, the four-necked flask (kettle) was placed in a preheated oil bath at 80°C. 0.68g of 2,5-di-tert-butylhydroquinone and 340.43g of monomer C (R4 is methyl) were added, and the molar ratio of monomer C (R4 is methyl) to resin A was controlled to be 3:1. When the temperature in the four-necked flask (kettle) rose to 80°C, the reaction timer was started for 1h. After the reaction was completed, the heating was turned off, the four-necked flask (kettle) was taken out from the oil bath, and cooled naturally to room temperature in the air to obtain the final product, multifunctional UV resin, referred to as multifunctional UV resin 1.

[0049] The preparation method of the UV hydrolyzed adhesive composition of this embodiment is:

[0050] The raw material components including multifunctional UV resin, difunctional high refractive index UV resin, hydrophilic UV monomer, hydrophobic UV monomer, photoinitiator and wrinkling aid are mixed evenly to obtain a UV hydrolyzed adhesive composition.

[0051] The components of the UV hydrolyzed gel of compositions 1-4 are shown in Table 1.

[0052] Table 1

[0053]

[0054]

[0055] The test samples of each UV hydrolysis composition were prepared as follows:

[0056] 1. Apply the UV hydrolyzed adhesive composition on the thinned electronic glass, and laminate until there are 10 pieces of glass;

[0057] 2. Expose the laminated multi-layer thinned electronic glass under a UV lamp (18W, effective wavelength 365nm) for primary curing, with an exposure dose of 100mj / cm 2 , exposure time 4-8s;

[0058] 3. Boil the multi-layer thinned electronic glass after primary curing in 90°C hot water for 3-6 hours;

[0059] 4. The multi-layer thinned electronic glass after boiling is exposed to UV lamp (1000W, effective wavelength 365nm) for deep curing, with an exposure of 5000mj / cm 2 , exposure time 3-6min;

[0060] 5. Soak the deeply cured multi-layer thinned electronic glass in 40-90°C hot water for no more than 120 seconds, so that the laminated multi-layer glass falls off layer by layer to form a single piece.

[0061] The evaluation criteria and test results of each project are shown in Table 2.

[0062] Table 2

[0063]

[0064]

[0065] Note: ○ means it complies with the regulations, and × means it does not comply with the regulations

[0066] In compositions 1-4, the number of double bond functional groups of multifunctional UV resin 1 is 10. As shown in Table 2, compared with composition 3, composition 1 has a low total double bond content in the system, which leads to insufficient crosslinking density of the system, so that composition 1 is boiled at 90°C for 3-6h after primary curing, and water penetrates into the edge of the laminated glass. After deep curing, it is difficult for the film to have a large number of bubble lines, which eventually leads to hydrolysis (40-90°C / 120s) and only part of the glass layers can fall off. Compared with composition 3, composition 2 has a low refractive index of the system, which reduces the effective perspective of UV light and affects the primary curing. When the primary curing is 4s, the glass layers can still slide; when the primary curing is 8s, although there is no sliding between the glass layers, due to insufficient curing inside the system, water penetrates into the edge of the laminated glass after boiling at 90°C for 3-6h. Compared with composition 3, composition 4 does not add wrinkling aids, which affects deep curing wrinkling. When deep curing is performed for 3 minutes, there are no large number of bubble lines on the film; when deep curing is performed for 6 minutes, although a large number of bubble lines appear on the film, due to the lack of wrinkling aid, only part of the glass layers can fall off after hydrolysis (40-90℃ / 120s).

[0067] Embodiment 2:

[0068] A method for preparing a multifunctional UV resin comprises the following steps:

[0069] 192.10g of resin A is added to a 1L four-necked flask (kettle) equipped with a mechanical stirring device, and placed in an oil bath for heating. The oil bath temperature is set to 100°C. When the mechanical stirring device can be turned smoothly manually, turn on the mechanical stirring device. Then weigh 123.01g of monomer B (acrylic acid is used in this example), and control the molar ratio of resin A to monomer B (acrylic acid) to be 1:4.02. When the temperature in the four-necked flask (kettle) rises to 100°C, add 25% of the total mass of monomer B (acrylic acid), i.e. 30.75g, and 0.16g of methylhydroquinone, and the oil bath temperature is set to 110°C. Then add the remaining monomer B (acrylic acid) 92.26g to the constant pressure dropping funnel, and when the temperature in the four-necked flask (kettle) rises to 110°C, add 0.79g of triphenylphosphine, then slowly open the valve of the constant pressure dropping funnel, and let the monomer B (acrylic acid) slowly drip into the four-necked flask (kettle). Since the reaction is an exothermic reaction, it is necessary to control the temperature in the four-necked flask (kettle) to 115-120°C. After the monomer B (acrylic acid) is dripped, the oil bath temperature is set to 130°C, and when the temperature in the four-necked flask (kettle) rises to 130°C, keep the reaction warm, take samples to measure the acid value until the acid value is about 1.51mgKOH / g, and the reaction is completed.

[0070] The four-necked flask (kettle) was taken out from the oil bath and cooled naturally in the air. When the temperature in the four-necked flask (kettle) dropped to 60°C, the four-necked flask (kettle) was placed in a preheated oil bath at 60°C. 0.63g of p-hydroxyanisole and 406.30g of monomer C (R4 is hydrogen) were added, and the molar ratio of monomer C (R4 is hydrogen) to resin A was controlled to be 4:1. When the temperature in the four-necked flask (kettle) rose to 60°C, the reaction timer was started for 3h. After the reaction was completed, the heating was turned off, the four-necked flask (kettle) was taken out from the oil bath, and cooled naturally to room temperature in the air to obtain the final product, multifunctional UV resin, referred to as multifunctional UV resin 2.

[0071] The preparation method of the UV hydrolyzed adhesive composition of this embodiment is the same as the preparation method of the UV hydrolyzed adhesive composition in Example 1, and will not be described in detail here.

[0072] The components of the UV hydrolyzed gel of compositions 5-8 are shown in Table 3.

[0073] Table 3

[0074]

[0075] According to the same method as in Example 1, test samples were prepared for each UV hydrolyzable composition.

[0076] The evaluation criteria and test results of each project are shown in Table 4.

[0077] Table 4

[0078]

[0079] Note: ○ means it complies with the regulations, and × means it does not comply with the regulations

[0080] In composition 5-8, the number of double bond functional groups of multifunctional UV resin 2 is 12. It can be seen from Table 4 that compared with composition 7, composition 5 has a lower total double bond content in the system, which leads to insufficient crosslinking density of the system. Although composition 5 has no water penetration at the edge of the laminated glass after being boiled at 90°C for 3 hours after primary curing, water has penetrated into the edge of the laminated glass after being boiled at 90°C for 6 hours. In addition, it is difficult for the film to have a large number of bubble lines after deep curing, and only part of the glass layers can fall off after hydrolysis (40-90°C / 120s). Compared with composition 7, composition 6 has a lower refractive index in the system, which reduces the effective perspective of UV light and affects the primary curing. When the primary curing is 4s, the glass layers can still slide; when the primary curing is 8s, although there is no sliding between the glass layers, due to insufficient curing inside the system, water has penetrated into the edge of the laminated glass after being boiled at 90°C for 3-6 hours. Compared with composition 7, composition 8 has no wrinkling aid added, which affects deep curing wrinkling. Deep curing lasts for 3-6 minutes. Although a large number of bubble lines appear on the film, due to the lack of wrinkling aid, only part of the glass layers can fall off after hydrolysis (40-90℃ / 120s).

[0081] Embodiment 3:

[0082] A method for preparing a multifunctional UV resin comprises the following steps:

[0083] 192.10g of resin A was added to a 1L four-necked flask (kettle) equipped with a mechanical stirring device, and placed in an oil bath for heating. The oil bath temperature was set to 100°C. When the mechanical stirring device can be turned smoothly manually, turn on the mechanical stirring device. Then weigh 146.57g of monomer B (methacrylic acid in this example), and control the molar ratio of resin A to monomer B (methacrylic acid) to be 1:4.01. When the temperature in the four-necked flask (kettle) rises to 100°C, 25% of the total mass of monomer B (methacrylic acid), i.e. 36.64g, and 0.17g of methylhydroquinone were added, and the oil bath temperature was set to 110°C. Then, the remaining 109.93 g of monomer B (methacrylic acid) was added to the constant pressure dropping funnel. When the temperature in the four-necked flask (kettle) rose to 110° C., 0.85 g of triphenylphosphine was added, and then the valve of the constant pressure dropping funnel was slowly opened to allow monomer B (methacrylic acid) to slowly drip into the four-necked flask (kettle). Since the reaction was an exothermic reaction, the temperature in the four-necked flask (kettle) needed to be controlled at 120-125° C. After the monomer B (methacrylic acid) was dripped, the oil bath temperature was set to 135° C. When the temperature in the four-necked flask (kettle) rose to 135° C., the reaction was kept warm, and the acid value was measured by sampling until the acid value was about 0.7 mgKOH / g, and the reaction was completed.

[0084] The four-necked flask (kettle) was taken out from the oil bath and cooled naturally in the air. When the temperature in the four-necked flask (kettle) dropped to 70°C, the four-necked flask (kettle) was placed in a preheated oil bath at 70°C. 0.68g of 2-tert-butylhydroquinone and 355.51g of monomer C (R4 is hydrogen) were added, and the molar ratio of lipid monomer C (R4 is hydrogen) to resin A was controlled to be 3.5:1. When the temperature in the four-necked flask (kettle) rose to 70°C, the reaction timer was started for 2h. After the reaction was completed, the heating was turned off, the four-necked flask (kettle) was taken out from the oil bath, and cooled naturally to room temperature in the air to obtain the final product, multifunctional UV resin, referred to as multifunctional UV resin 3.

[0085] The preparation method of the UV hydrolyzed adhesive composition of this embodiment is the same as the preparation method of the UV hydrolyzed adhesive composition in Example 1, and will not be described in detail here.

[0086] The components of the UV hydrolyzed gel of compositions 9-12 are shown in Table 5.

[0087] Table 5

[0088]

[0089] According to the same method as in Example 1, test samples were prepared for each UV hydrolyzable composition.

[0090] The evaluation criteria and test results of each project are shown in Table 6.

[0091] Table 6

[0092]

[0093] Note: ○ means it complies with the regulations, and × means it does not comply with the regulations

[0094] In compositions 9-12, the number of double bond functional groups of multifunctional UV resin 3 is 11. As shown in Table 6, compared with composition 11, composition 9 has a low total double bond content in the system, which leads to insufficient crosslinking density of the system, so that composition 9 is boiled at 90°C for 3-6h after primary curing, and water penetrates into the edge of the laminated glass. After deep curing, it is difficult for the film to have a large number of bubble lines, which eventually leads to hydrolysis (40-90°C / 120s) and only part of the glass layers can fall off. Compared with composition 11, composition 10 has a low refractive index of the system, which reduces the effective perspective of UV light and affects the primary curing. When the primary curing is 4s, the glass layers can still slide; when the primary curing is 8s, although there is no sliding between the glass layers, due to insufficient curing inside the system, water penetrates into the edge of the laminated glass after boiling at 90°C for 3-6h. Compared with composition 11, composition 12 does not add a wrinkling aid, which affects the deep curing wrinkling. When deep curing is performed for 3 minutes, there are no large number of bubble lines on the film; when deep curing is performed for 6 minutes, although a large number of bubble lines appear on the film, due to the lack of wrinkling aid, only part of the glass layers can fall off after hydrolysis (40-90℃ / 120s).

[0095] Comparative Example 1:

[0096] The preparation method of the multifunctional UV resin in this comparative example is different from that in Example 3 in that the molar ratio of resin A to monomer B (methacrylic acid) is 1:3.9. The specific preparation method is as follows:

[0097] Put 192.10g of resin A into a 1L four-necked flask (kettle) equipped with a mechanical stirring device, place it in an oil bath for heating, and set the oil bath temperature to 100℃. When the mechanical stirring device can be turned smoothly manually, turn on the mechanical stirring device. Then weigh 142.55g of monomer B (methacrylic acid), and control the molar ratio of resin A to monomer B (methacrylic acid) to be 1:3.9. When the temperature in the four-necked flask (kettle) rises to 100℃, add 25% of the total mass of monomer B (methacrylic acid), i.e. 35.64g, and 0.17g of methylhydroquinone, and set the oil bath temperature to 110℃. Then, the remaining 106.91 g of monomer B (methacrylic acid) was added to the constant pressure dropping funnel. When the temperature in the four-necked flask (kettle) rose to 110° C., 0.84 g of triphenylphosphine was added, and then the valve of the constant pressure dropping funnel was slowly opened to allow monomer B (methacrylic acid) to slowly drip into the four-necked flask (kettle). Since the reaction was an exothermic reaction, the temperature in the four-necked flask (kettle) needed to be controlled at 120-125° C. After the monomer B (methacrylic acid) was dripped, the oil bath temperature was set to 135° C. When the temperature in the four-necked flask (kettle) rose to 135° C., the reaction was kept warm, and the acid value was measured by sampling until the acid value was substantially 0, and the reaction was completed.

[0098] The four-necked flask (kettle) was taken out from the oil bath and cooled naturally in the air. When the temperature in the four-necked flask (kettle) dropped to 70°C, the four-necked flask (kettle) was placed in a preheated oil bath at 70°C. 0.67g of 2-tert-butylhydroquinone and 355.51g of monomer C (R4 is hydrogen) were added, and the molar ratio of monomer C (R4 is hydrogen) to resin A was controlled to be 3.5:1. When the temperature in the four-necked flask (kettle) rose to 70°C, the reaction timer was started for 2h. After the reaction was completed, the heating was turned off, the four-necked flask (kettle) was taken out from the oil bath, and cooled naturally to room temperature in the air to obtain the final product, multifunctional UV resin, referred to as multifunctional UV resin 4.

[0099] Comparative Example 2:

[0100] The preparation method of the multifunctional UV resin in this comparative example is different from that in Example 3 in that the molar ratio of monomer C (R4 is hydrogen) to resin A is 2.5:1. The specific preparation method is as follows:

[0101] Put 192.10g of resin A into a 1L four-necked flask (kettle) equipped with a mechanical stirring device, place it in an oil bath for heating, and set the oil bath temperature to 100℃. When the mechanical stirring device can be turned smoothly manually, turn on the mechanical stirring device. Then weigh 146.57g of monomer B (methacrylic acid), and control the molar ratio of resin A to monomer B (methacrylic acid) to be 1:4.01. When the temperature in the four-necked flask (kettle) rises to 100℃, add 25% of the total mass of monomer B (methacrylic acid), i.e. 36.64g, and 0.17g of methylhydroquinone, and set the oil bath temperature to 110℃. Then, the remaining 109.93 g of monomer B (methacrylic acid) was added to the constant pressure dropping funnel. When the temperature in the four-necked flask (kettle) rose to 110° C., 0.85 g of triphenylphosphine was added, and then the valve of the constant pressure dropping funnel was slowly opened to allow monomer B (methacrylic acid) to slowly drip into the four-necked flask (kettle). Since the reaction was an exothermic reaction, the temperature in the four-necked flask (kettle) needed to be controlled at 120-125° C. After the monomer B (methacrylic acid) was dripped, the oil bath temperature was set to 135° C. When the temperature in the four-necked flask (kettle) rose to 135° C., the reaction was kept warm, and the acid value was measured by sampling until the acid value was about 0.7 mgKOH / g, and the reaction was completed.

[0102] The four-necked flask (kettle) was taken out from the oil bath and cooled naturally in the air. When the temperature in the four-necked flask (kettle) dropped to 70°C, the four-necked flask (kettle) was placed in a preheated oil bath at 70°C. 0.68g of 2-tert-butylhydroquinone and 253.94g of monomer C (R4 is hydrogen) were added, and the molar ratio of monomer C (R4 is hydrogen) to resin A was controlled to be 2.5:1. When the temperature in the four-necked flask (kettle) rose to 70°C, the reaction timer was started for 2h. After the reaction was completed, the heating was turned off, the four-necked flask (kettle) was taken out from the oil bath, and cooled naturally to room temperature in the air to obtain the final product, multifunctional UV resin, referred to as multifunctional UV resin 5.

[0103] The preparation methods of the UV hydrolyzed adhesive compositions of Comparative Examples 1 and 2 are the same as those of the UV hydrolyzed adhesive composition of Example 3, except that different multifunctional UV resins are used, as shown in Table 7.

[0104] Table 7

[0105]

[0106]

[0107] According to the same method as in Example 1, test samples were prepared for each UV hydrolyzable composition.

[0108] The evaluation criteria and test results of each project are shown in Table 8.

[0109] Table 8

[0110]

[0111] Note: ○ means it complies with the regulations, and × means it does not comply with the regulations

[0112] In composition 11, the multifunctional UV resin 3 of Example 3 is used. Since the molar ratio of resin A to monomer B (methacrylic acid) is 1:4.01, the four epoxy groups at both ends of the molecular chain in resin A can be completely reacted to form four double bonds, and the four double bonds at both ends of the molecular chain are very active and can be quickly cured under low exposure conditions to obtain a polymer with excellent hydrolysis resistance. In addition, the molar ratio of monomer C (R4 is hydrogen) to resin A is 3.5:1, and the final number of double bond functional groups of multifunctional UV resin 3 is 11. On the one hand, the crosslinking density is large, which further improves its hydrolysis resistance. On the other hand, it strengthens the curing shrinkage of the resin system and promotes the wrinkling effect. Combined with the formula composition, all the properties in composition 11 can meet the requirements.

[0113] In composition 13, the multifunctional UV resin 4 of comparative example 1 is used. Since the molar ratio of resin A to monomer B (methacrylic acid) in multifunctional UV resin 4 is 1:3.9, the four epoxy groups at both ends of the molecular chain in resin A are not completely reacted to form four double bonds. Therefore, when the curing is performed for 4 seconds, the glass layers can still slide and cannot be cured quickly; when the curing is performed for 8 seconds, although there is no sliding between the glass layers, the system is affected by the curing, resulting in water infiltration at the edge of the laminated glass after boiling at 90°C for 6 hours. In addition, the deep curing speed is also affected. After 3 minutes of deep curing, the film has only some bubble lines; after 6 minutes of deep curing, although a large number of bubble lines appear on the film, only some of the glass layers can fall off after hydrolysis at 40°C. Although the glass falls off layer by layer after hydrolysis at 90°C, there is residual glue on the glass.

[0114] In composition 14, the multifunctional UV resin 5 of comparative example 2 is used. Since the molar ratio of monomer C (R4 is hydrogen) to resin A in the multifunctional UV resin 5 is 2.5:1, the number of double bond functional groups in the multifunctional UV resin 5 is 9. As a result, the total double bond content in the system is low, resulting in insufficient crosslinking density of the system, which in turn leads to the failure to meet the requirements of 90°C boiling, deep curing and hydrolysis.

[0115] In composition 15, no multifunctional UV resin was added, which ultimately resulted in various properties failing to meet the requirements.

[0116] This embodiment is only a preferred embodiment of the present invention, and is not intended to limit the present invention in other forms. Any person skilled in the art may use the above content as inspiration to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent changes and modifications listed in the above embodiment that do not deviate from the technical essence of the claims of the present invention still fall within the scope of protection of the claims of the present invention.

Claims

1. A multifunctional UV resin, characterized in that: The structural formula is as follows: Wherein, R3 is H or methyl, R4 is H or methyl, and the structure of R1 is as follows: R2 is the following structure and contains at least H, or all are the following structures:

2. A method for preparing a multifunctional UV resin as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Add resin A into a container, heat to 100°C, first add 25% of the total mass of monomer B and inhibitor D, and then heat to 109-111°C again to obtain a first reaction solution; wherein the structure of the resin A is as follows: The structure of the monomer B is as follows: Wherein, R3 is H or methyl; Step 2: Add a catalyst to the first reaction liquid, and slowly dropwise add the remaining mass of monomer B. In this stage, the reaction temperature is controlled at 110-125° C. to obtain a second reaction liquid; Step 3: heating the second reaction liquid to 125-135° C., keeping the temperature for reaction, sampling and measuring the acid value until the acid value remains substantially unchanged to obtain a third reaction liquid; Step 4: Cool the third reaction solution to 60-80° C., add polymerization inhibitor E and monomer C, react for 1-3 hours, and cool to room temperature to obtain the multifunctional UV resin; wherein the structure of monomer C is as follows: Wherein, R4 is H or methyl.

3. The method for preparing a multifunctional UV resin according to claim 2, characterized in that: The molar ratio of the resin A to the monomer B is 1:(4-4.02).

4. The method for preparing a multifunctional UV resin according to claim 2, characterized in that: The polymerization inhibitor D is methyl hydroquinone, and the added amount is 0.05% of the total mass of the resin A and the monomer B.

5. The method for preparing a multifunctional UV resin according to claim 2, characterized in that: The polymerization inhibitor E is one of hydroquinone, p-hydroxyanisole, 2-tert-butylhydroquinone and 2,5-di-tert-butylhydroquinone, and the added amount is 0.2% of the total mass of the resin A and the monomer B.

6. The method for preparing a multifunctional UV resin according to claim 2, characterized in that: The catalyst is triphenylphosphine, and the added amount is 0.25% of the total mass of the resin A and the monomer B.

7. The method for preparing a multifunctional UV resin according to claim 2, characterized in that: The molar ratio of the monomer C to the resin A is (3-4):

1.

8. A UV hydrolyzed adhesive composition, characterized in that: The multifunctional UV resin according to claim 1 comprises the following components by weight:

9. The UV hydrolyzed adhesive composition according to claim 8, characterized in that: The bifunctional high refractive index UV resin is selected from one of Youyang Trust-6601 and Youyang Trust-6602; the hydrophilic UV monomer is one of polyethylene glycol (600) dimethacrylate, methoxy polyethylene glycol methacrylate, and ethoxy polyethylene glycol methacrylate; the hydrophobic UV monomer is at least one of dicyclopentadiene acrylate, isobornyl methacrylate, trimethylolpropane triacrylate, dipentaerythritol hexaacrylate, and tris(2-hydroxyethyl)isocyanuric acid triacrylate.

10. The UV hydrolyzed adhesive composition according to claim 8, characterized in that: The photoinitiator is at least one of photoinitiator 1173, photoinitiator 651, photoinitiator 819 and photoinitiator ITX; the wrinkling aid is one of azobisisobutyronitrile and benzoyl peroxide.

Citation Information

Patent Citations

  • Tetra-functionality urethane acrylate based on pentaerythritol and preparation method and application tetra-functionality urethane acrylate

    CN105859587A

  • Hexa-functionality urethane acrylate based on dipentaerythritol and preparation method and application of hexa-functionality urethane acrylate

    CN105860026A

  • One-pack type adhesive composition for dental use

    CN1917845A

  • Dental adhesive composition

    JP2005179282A

  • One-pack type dental adhesive composition

    JP2005179283A