Pyridine tridentate ligand iron complex, preparation method and application thereof, and preparation method of polyisobutene
By using a pyridine tridentate ligand iron complex as a catalyst to regulate the structure and reaction rate of polyisobutylene, the problem of uncontrollable polyisobutylene structure in the existing technology is solved, and the preparation of linear polyisobutylene with adjustable molecular weight is achieved. Costs are reduced and processes are simplified.
Patent Information
- Application Number
- CN202410822214.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-25
AI Technical Summary
It is difficult to control the polymerization structure and reaction rate of existing catalysts during the preparation of polyisobutylene, and it is easy to form network polymers, resulting in uncontrollable molecular weight.
The pyridine tridentate ligand iron complex is used as the catalyst, and through specific coordination and activation with the isobutylene monomer, the polymerization reaction is controlled to ensure that the polyisobutylene has a linear structure, and different molecular weights are obtained by adjusting the catalyst type and reaction time. product.
The controllability of the polyisobutylene structure and the regulation of the reaction rate are achieved, and linear polyisobutylene with adjustable molecular weight is obtained, which reduces the cost and simplifies the preparation method.
Smart Images

Figure CN118745202A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and specifically relates to a pyridine tridentate ligand iron complex, a preparation method and application thereof, and a preparation method of polyisobutylene. Background Art
[0002] Polyisobutylene is a colorless, odorless, non-toxic isobutylene homopolymer, and its chemical structure is a typical linear saturated polymer. The main part of the molecular skeleton is composed of repeating units -CH2-C(CH3)2-, with -CH3 at the head and -CH2-C(CH3)=CH2 or -CH=C(CH3)2 at the end. Due to different preparation methods and production processes, the molecular weight of polyisobutylene can vary over a wide range. According to molecular weight, polyisobutylene can be divided into high molecular weight polyisobutylene (Mn>100000), medium molecular weight polyisobutylene (100000>Mn>10000), and low molecular weight polyisobutylene (Mn<10000).
[0003] Polyisobutylene is resistant to acid, alkali, water, salt, ozone and aging, and has excellent properties such as good gas barrier and electrical insulation. It has good compatibility with asphalt, wax and polyethylene. At present, the polyisobutylene industry has developed a variety of polymerization methods to obtain polyisobutylene. From the perspective of catalysts, it can be divided into two categories, aluminum-based polyisobutylene (for example, ethylaluminum dichloride) and boron-based polyisobutylene. In essence, aluminum reagents or boron reagents form cations in the reaction system, thereby inducing polymerization of monomers.
[0004] In the process of forming the above-mentioned cationic induced polymerization reaction, side reactions such as intramolecular rearrangement, transfer, isomerization, etc. are prone to occur, resulting in the difficulty in controlling the structure and reaction rate of polyisobutylene. For example, when ethylaluminum dichloride is used as a catalyst to prepare polyisobutylene, it can be observed from experimental phenomena that the reaction is very fast, the reaction rate is uncontrollable, and the obtained polyisobutylene structure is often highly cross-linked (network polymer), insoluble, and the molecular weight cannot be measured. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a pyridine tridentate ligand iron complex and its preparation method and application, and a method for preparing polyisobutylene. The pyridine tridentate ligand iron complex provided by the present invention is used as a catalyst for preparing polyisobutylene, which can better regulate the structure and reaction rate of polyisobutylene to obtain linear polyisobutylene with adjustable molecular weight.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b:
[0008]
[0009] In formula a, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S;
[0010] In formula b, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
[0011] Preferably, formula a includes the structure shown by any one of the following Fe1 to Fe12:
[0012]
[0013] Formula b includes the structure shown in any one of the following Fe13 to Fe20:
[0014]
[0015] The present invention provides a method for preparing the pyridine tridentate ligand iron complex described in the above scheme, comprising the following steps:
[0016] Under the protection of a first inert gas, anhydrous FeCl3, a first organic solvent and a pyridine tridentate ligand solution are mixed and complexed to obtain a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b;
[0017] The pyridine tridentate ligand has a structure shown in formula c or formula d:
[0018]
[0019] In formula c, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S;
[0020] In formula d, R 1 , R 2 and R 3are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
[0021] Preferably, formula c includes the structure shown in any one of the following 1 to 12:
[0022]
[0023] Formula d includes the structures shown in any one of the following 13 to 20:
[0024]
[0025] Preferably, the molar ratio of the anhydrous FeCl3 to the pyridine tridentate ligand in the pyridine tridentate ligand solution is 1:1.05.
[0026] Preferably, the concentration of the pyridine tridentate ligand solution is 0.105 mol / L.
[0027] The present invention provides the use of the pyridine tridentate ligand iron complex described in the above scheme or the pyridine tridentate ligand iron complex prepared by the preparation method described in the above scheme as a catalyst in the preparation of polyisobutylene.
[0028] The present invention provides a method for preparing polyisobutylene, comprising the following steps:
[0029] Under the protection of a second inert gas, a co-catalyst solution, a pyridine tridentate ligand iron complex, an isobutylene monomer and a second organic solvent are mixed to carry out a polymerization reaction to obtain the polyisobutylene; the pyridine tridentate ligand iron complex is the pyridine tridentate ligand iron complex described in the above scheme or the pyridine tridentate ligand iron complex prepared by the preparation method described in the above scheme.
[0030] Preferably, the promoter solution is a toluene solution of the promoter; the promoter includes promoter MAO, promoter AlMe3, promoter AlEt3 or promoter Al i Bu3.
[0031] Preferably, the polymerization reaction temperature is -20 to 50°C and the time is 2 to 48 hours.
[0032] The present invention provides a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b:
[0033]
[0034] In formula a, R 1 , R 2 and R3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S;
[0035] In formula b, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
[0036] The whole skeleton of the pyridine tridentate ligand in the pyridine tridentate ligand iron complex provided by the present invention is a conjugated structure, and the heteroatom types at the X position are different, which will cause the iron center electropositivity of the ferrous chloride complexed with the ligand to become stronger, and it is easier to activate the isobutylene monomer, thereby improving the reaction activity; the nitrogen atom can also activate the isobutylene monomer, improve the reaction activity, and specifically, the lone pair of electrons on the nitrogen atom is coordinated with iron, so that the b-type complex has a special spatial structure, and the isobutylene monomer can be activated by the central metal iron in a specific direction, thereby promoting the progress of the polymerization reaction. The metal center is not easy to coordinate with isobutylene, and the nitrogen atom can form a channel with a certain structure with the ferric chloride, so that isobutylene and iron are well coordinated.
[0037] The metal complex (pyridine tridentate ligand iron complex) provided by the present invention has a complex spatial structure, so that the isobutylene monomer cannot coordinate with the metal center freely, and thus cannot react. Only in a suitable direction can the isobutylene monomer coordinate with the metal center smoothly, and then a polymerization reaction can occur, thereby regulating the polyisobutylene to be a linear structure, thereby solving the problem that the structure of polyisobutylene prepared by the existing catalyst is uncontrollable and a network polymer is easily formed (the existing catalyst ethyl aluminum dichloride itself is very active and has strong activity, and an active center can be formed at any position, and cross-linking is easily generated within the polyisobutylene chain and between chains, thereby forming a network polymer).
[0038] The invention uses a pyridine tridentate ligand iron complex as a catalyst, and the polymerization reaction rate is controllable. Linear polyisobutylene with different molecular weights can be obtained by adjusting the specific type of the catalyst and the polymerization reaction time.
[0039] Metallic iron (Fe) has unique physical properties, is inexpensive and highly active, and when complexed with a pyridine tridentate ligand, has a unique spatial structure, it can catalyze isobutylene polymerization very well.
[0040] Compared with the boron-based polyisobutylene catalyst, the pyridine tridentate ligand iron complex prepared by the invention has low cost and a simple preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0042] Figure 1 This is the GPC spectrum of the polyisobutylene prepared in Example 21;
[0043] Figure 2 This is the hydrogen spectrum of the polyisobutylene prepared in Example 21. DETAILED DESCRIPTION
[0044] The present invention provides a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b:
[0045]
[0046] In formula a, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S;
[0047] In formula b, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
[0048] Unless otherwise specified, the materials and equipment of the present invention are commercially available.
[0049] In the present invention, formula a preferably includes the structure represented by any one of the following Fe1 to Fe12:
[0050]
[0051] In the present invention, formula b preferably includes the structure shown in any one of the following Fe13 to Fe20:
[0052]
[0053] The entire skeleton of the pyridine tridentate ligand in the pyridine tridentate ligand iron complex provided by the present invention is a conjugated structure, and the types of heteroatoms at the X position are different, which will cause the iron center of the ferrous chloride complexed with the ligand to be more electrically positive, making it easier to activate the isobutylene monomer, thereby improving the reaction activity.
[0054] The metal complex (pyridine tridentate ligand iron complex) provided by the present invention has a complex spatial structure, so that the isobutylene monomer cannot coordinate with the metal center freely, and thus cannot react. Only in a suitable direction can the isobutylene monomer coordinate with the metal center smoothly, and then a polymerization reaction can occur, thereby regulating the polyisobutylene to be a linear structure, thereby solving the problem that the polyisobutylene prepared by the existing catalyst has an uncontrollable structure and is easy to form a network polymer.
[0055] The invention uses a pyridine tridentate ligand iron complex as a catalyst, and the polymerization reaction rate is controllable. Linear polyisobutylene with different molecular weights can be obtained by adjusting the specific type of the catalyst and the polymerization reaction time.
[0056] Metallic iron (Fe) has unique physical properties, is inexpensive and highly active, and when complexed with pyridine tridentate ligands, has a unique spatial structure, which can catalyze isobutylene polymerization very well.
[0057] The present invention provides a method for preparing the pyridine tridentate ligand iron complex described in the above scheme, comprising the following steps:
[0058] Under the protection of a first inert gas, anhydrous FeCl3, a first organic solvent and a pyridine tridentate ligand solution are mixed and complexed to obtain a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b; the pyridine tridentate ligand has a structure shown in formula c or formula d:
[0059]
[0060] In formula c, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S;
[0061] In formula d, R 1 , R 2 and R 3 are independently H-, Me-, CH3CH2-, CH3CH2CH2-, i Pr-,t Bu-, F-, Cl-, Br-, OMe- or Ph-.
[0062] In the present invention, the first inert gas preferably comprises argon. In the present invention, the complexation is preferably performed in a glove box.
[0063] In the present invention, the mixing of anhydrous FeCl 3 , a first organic solvent and a pyridine tridentate ligand solution preferably comprises: mixing anhydrous FeCl 3 and a first organic solvent, and then dropping the pyridine tridentate ligand solution.
[0064] In the present invention, the first organic solvent is preferably toluene. The present invention has no special requirements on the amount of the first organic solvent, and any amount known in the art can be used.
[0065] In the present invention, the pyridine tridentate ligand solution is preferably obtained by dissolving the pyridine tridentate ligand in an organic solvent (referred to as the third organic solvent). In the present invention, the third organic solvent preferably includes toluene.
[0066] In the present invention, the molar ratio of the pyridine tridentate ligand in the anhydrous FeCl3 and the pyridine tridentate ligand solution is preferably 1:1.05; the concentration of the pyridine tridentate ligand solution is preferably 0.105 mol / L.
[0067] In the present invention, the complexing temperature is preferably room temperature, and the complexing time is preferably 48 hours.
[0068] After the complexation is completed, the present invention preferably filters the obtained reaction solution, washes the obtained solid with n-hexane three times, and vacuum evacuates to obtain the pyridine tridentate ligand iron complex. In the present invention, the filtration is preferably carried out under an argon atmosphere.
[0069] In the present invention, formula c preferably includes the structure shown in any one of the following 1 to 12:
[0070]
[0071] In the present invention, formula d preferably includes the structure shown in any one of the following 13 to 20:
[0072]
[0073] In the present invention, compounds 1 to 12 in formula c and compounds 13 to 20 in formula d are preferably obtained by purchase.
[0074] The present invention provides the use of the pyridine tridentate ligand iron complex described in the above scheme or the pyridine tridentate ligand iron complex prepared by the preparation method described in the above scheme as a catalyst in the preparation of polyisobutylene.
[0075] The present invention provides a method for preparing polyisobutylene, comprising the following steps:
[0076] Under the protection of a second inert gas, a co-catalyst solution, a pyridine tridentate ligand iron complex, an isobutylene monomer and a second organic solvent are mixed to carry out a polymerization reaction to obtain the polyisobutylene; the pyridine tridentate ligand iron complex is the pyridine tridentate ligand iron complex described in the above scheme or the pyridine tridentate ligand iron complex prepared by the preparation method described in the above scheme.
[0077] In the present invention, the second inert gas preferably includes argon. In the present invention, the second organic solvent preferably includes toluene.
[0078] In the present invention, the concentration of the promoter solution is preferably 1.5 mol / L. In the present invention, the promoter solution is preferably a toluene solution of the promoter; the promoter preferably includes the promoter MAO, the promoter AlMe3, the promoter AlEt3 or the promoter Al i Bu3.
[0079] In the present invention, the molar ratio of the pyridine tridentate ligand iron complex to the volume ratio of the second organic solvent is preferably 1 mol:(5-50) mL, more preferably 1 mol:(10-40) mL, and even more preferably 1 mol:(20-30) mL.
[0080] In the present invention, the molar ratio of the pyridine tridentate ligand iron complex to the co-catalyst is preferably 1:(5-1000), more preferably 1:(20-500), and even more preferably 1:(40-400).
[0081] In the present invention, the molar ratio of the pyridine tridentate ligand iron complex to the isobutylene monomer is preferably 1:50-1000, more preferably 1:(100-500), and more preferably 1:(200-400).
[0082] In the present invention, the polymerization reaction temperature is preferably -20 to 50° C., more preferably 5 to 40° C., and more preferably 10 to 30° C. In the present invention, the polymerization reaction time is preferably 2 to 48 h, more preferably 5 to 40 h, and more preferably 10 to 30 h.
[0083] After the polymerization reaction is completed, the present invention preferably quenches the obtained reaction solution with methanol, and sequentially washes, filters and dries to obtain the polyisobutylene.
[0084] In the present invention, the washing solvent is preferably methanol.
[0085] In order to further illustrate the present invention, a pyridine tridentate ligand iron complex provided by the present invention, its preparation method and application, and a preparation method of polyisobutylene are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0086] Examples 1 to 12
[0087] In a glove box, anhydrous FeCl3 (1.0 equiv., 1 mmol) and toluene (8 mL) were added to a dry Schlenk tube (50 mL) in sequence, and pyridine tridentate ligands 1 to 12 (1.05 equiv., 1.05 mmol) were dissolved in toluene (10 mL) respectively, and added dropwise to the Schlenk tube of FeCl3 under stirring, and stirred at room temperature for 48 h. After the reaction was completed, the solid was filtered under an argon atmosphere, and the obtained solid was washed 3 times with n-hexane and vacuum-dried to obtain pyridine tridentate ligand iron complexes Fe1 to Fe12, with yields of 96%, 90%, 76%, 98%, 88%, 93%, 75%, 85%, 93%, 95%, 80%, and 63%, respectively.
[0088] Examples 13 to 20
[0089] In a glove box, anhydrous FeCl3 (1.0 equiv., 1 mmol) and toluene (8 mL) were added to a dry Schlenk tube (50 mL) in sequence, and pyridine tridentate ligands 13-20 (1.05 equiv., 1.05 mmol) were dissolved in toluene (10 mL) respectively, and added dropwise to the Schlenk tube of FeCl3 under stirring, and stirred at room temperature for 48 h. After the reaction was completed, the solid was filtered under an argon atmosphere, and the obtained solid was washed 3 times with n-hexane and vacuum-dried to obtain pyridine tridentate ligand iron complexes Fe13-Fe20, with yields of 71%, 83%, 80%, 90%, 62%, 93%, 55%, and 88%, respectively.
[0090] Embodiment 21
[0091] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (0.5 mmol, 50 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0092] The yield of low molecular weight polyisobutylene in this example is 76%, the molecular weight is 125963 g / mol, and the PDI is 1.8.
[0093] Figure 1 The GPC spectrum of the polyisobutylene prepared in Example 21 is as follows: Figure 1 As shown, there is one peak of polyisobutylene, indicating that only one active center is formed during the polymerization process, wherein the red is the light scattering signal and the blue is the differential signal, both of which are a means of detecting the sample. The appearance of these signals indicates that the sample flows out of the chromatography column and is detected by the detector. The polyisobutylene GPC spectra obtained in Examples 22 to 58 are similar to those in Example 21.
[0094] Figure 2 is the hydrogen spectrum of the polyisobutylene prepared in Example 21, as shown Figure 2 As shown, the peak at the chemical shift of 1.65 ppm is the two hydrogen atoms on the methylene group of the polyisobutylene molecular chain, and the peak at the chemical shift of 1.41 ppm is the peak of the hydrogen atoms on the two methyl groups. The integral ratio is 1:2, which is consistent with the arrangement of hydrogen atoms on the polyisobutylene molecular chain.
[0095] Embodiment 22
[0096] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (1 mmol, 100 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0097] The yield of low molecular weight polyisobutylene in this example is 87%, the molecular weight is 196577 g / mol, and the PDI is 2.0.
[0098] Embodiment 23
[0099] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0100] The yield of low molecular weight polyisobutylene in this example is 93%, the molecular weight is 203359 g / mol, and the PDI is 2.2.
[0101] Embodiment 24
[0102] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst AlMe3 (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0103] The yield of low molecular weight polyisobutylene in this example is 62%, the molecular weight is 136469 g / mol, and the PDI is 2.2.
[0104] Embodiment 25
[0105] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst AlEt3 (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0106] The yield of low molecular weight polyisobutylene in this example is 51%, the molecular weight is 109527 g / mol, and the PDI is 2.8.
[0107] Embodiment 26
[0108] Under argon atmosphere, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL anhydrous toluene, and co-catalyst Al were added in sequence into a 25 mL Schlenk bottle. i Bu3 (2 mmol, 200 equiv., 1.5 M toluene) and isobutylene (4 mmol, 400 equiv.), the system was placed at 25°C for reaction for 12 hours, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0109] The yield of low molecular weight polyisobutylene in this example is 50%, the molecular weight is 129321 g / mol, and the PDI is 1.8.
[0110] Comparative Example 1
[0111] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h. After quenching with methanol, no polyisobutylene was generated after washing with methanol, filtering and vacuum drying.
[0112] Comparative Example 2
[0113] Under argon atmosphere, 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added sequentially into a 25 mL Schlenk bottle, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuo, and no polyisobutylene was generated.
[0114] Embodiment 27
[0115] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe2 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuum to obtain polyisobutylene.
[0116] The yield of low molecular weight polyisobutylene in this example is 83%, the molecular weight is 174560 g / mol, and the PDI is 2.0.
[0117] Embodiment 28
[0118] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe3 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuo to obtain polyisobutylene.
[0119] The yield of low molecular weight polyisobutylene in this example is 96%, the molecular weight is 166551 g / mol, and the PDI is 1.8.
[0120] Embodiment 29
[0121] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe4 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuum to obtain polyisobutylene.
[0122] The yield of low molecular weight polyisobutylene in this example is 86%, the molecular weight is 140933 g / mol, and the PDI is 2.3.
[0123] Embodiment 30
[0124] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe5 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuum to obtain polyisobutylene.
[0125] The yield of low molecular weight polyisobutylene in this example is 74%, the molecular weight is 169020 g / mol, and the PDI is 2.3.
[0126] Embodiment 31
[0127] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe6 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0128] The yield of low molecular weight polyisobutylene in this example is 90%, the molecular weight is 183572 g / mol, and the PDI is 2.2.
[0129] Embodiment 32
[0130] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe7 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0131] The yield of low molecular weight polyisobutylene in this example is 48%, the molecular weight is 230477 g / mol, and the PDI is 2.0.
[0132] Embodiment 33
[0133] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe8 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0134] The yield of low molecular weight polyisobutylene in this example is 95%, the molecular weight is 157527 g / mol, and the PDI is 2.6.
[0135] Embodiment 34
[0136] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe9 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0137] The yield of low molecular weight polyisobutylene in this example is 80%, the molecular weight is 169627 g / mol, and the PDI is 2.6.
[0138] Embodiment 35
[0139] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe10 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0140] The yield of low molecular weight polyisobutylene in this example is 65%, the molecular weight is 183527 g / mol, and the PDI is 3.0.
[0141] Embodiment 36
[0142] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe11 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, i.e., polyisobutylene.
[0143] The yield of low molecular weight polyisobutylene in this example is 71%, the molecular weight is 130527 g / mol, and the PDI is 2.3.
[0144] Embodiment 37
[0145] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe12 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0146] The yield of low molecular weight polyisobutylene in this example is 74%, the molecular weight is 117927 g / mol, and the PDI is 2.3.
[0147] Embodiments 38 to 41
[0148] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe1 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C. and reacted for 2 h, 4 h, 8 h, and 16 h, respectively. The reaction was quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0149] The yields of low molecular weight polyisobutylene in Examples 38 to 41 are 42%, 60%, 83% and 95%, the molecular weights are 60634 g / mol, 85699 g / mol, 179542 g / mol and 218620 g / mol, respectively, and the PDIs are 2.1, 2.6, 2.4 and 2.5, respectively.
[0150] Embodiment 42
[0151] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.) and 5 mL of anhydrous toluene, co-catalyst MAO (0.5 mmol, 50 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0152] The yield of low molecular weight polyisobutylene in this example is 45%, the molecular weight is 223698 g / mol, and the PDI is 1.8.
[0153] Embodiment 43
[0154] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (1 mmol, 100 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, i.e., polyisobutylene.
[0155] The yield of low molecular weight polyisobutylene in this example is 68%, the molecular weight is 196577 g / mol, and the PDI is 2.0.
[0156] Embodiment 44
[0157] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0158] The yield of low molecular weight polyisobutylene in this example is 92%, the molecular weight is 168532 g / mol, and the PDI is 2.1.
[0159] Embodiment 45
[0160] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst AlMe3 (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, i.e., polyisobutylene.
[0161] The yield of low molecular weight polyisobutylene in this example is 85%, the molecular weight is 132569 g / mol, and the PDI is 2.2.
[0162] Embodiment 46
[0163] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst AlEt3 (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0164] The yield of low molecular weight polyisobutylene in this example is 80%, the molecular weight is 113527 g / mol, and the PDI is 2.7.
[0165] Embodiment 47
[0166] Under argon atmosphere, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, and co-catalyst Al iBu3 (2 mmol, 200 equiv., 1.5 M toluene) and isobutylene (4 mmol, 400 equiv.), the system was placed at 25°C for reaction for 12 hours, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0167] The yield of low molecular weight polyisobutylene in this example is 77%, the molecular weight is 109521 g / mol, and the PDI is 1.8.
[0168] Comparative Example 3
[0169] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried, and no polyisobutylene was generated.
[0170] Comparative Example 4
[0171] Under argon atmosphere, anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added sequentially into a 25 mL Schlenk bottle, and the system was reacted at 25 °C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuo, and no polyisobutylene was generated.
[0172] Embodiment 48
[0173] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe14 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuo to obtain polyisobutylene.
[0174] The yield of low molecular weight polyisobutylene in this example is 90%, the molecular weight is 186551 g / mol, and the PDI is 1.7.
[0175] Embodiment 49
[0176] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe15 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuum to obtain polyisobutylene.
[0177] The yield of low molecular weight polyisobutylene in this example is 90%, the molecular weight is 186551 g / mol, and the PDI is 1.7.
[0178] Embodiment 50
[0179] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe16 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and dried in vacuo to obtain polyisobutylene.
[0180] The yield of low molecular weight polyisobutylene in this example is 95%, the molecular weight is 161931 g / mol, and the PDI is 2.3.
[0181] Embodiment 51
[0182] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe17 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain polyisobutylene.
[0183] The yield of low molecular weight polyisobutylene in this example is 94%, the molecular weight is 169920 g / mol, and the PDI is 2.3.
[0184] Embodiment 52
[0185] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe18 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0186] The yield of low molecular weight polyisobutylene in this example is 90%, the molecular weight is 183572 g / mol, and the PDI is 2.2.
[0187] Embodiment 53
[0188] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe19 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0189] The yield of low molecular weight polyisobutylene in this example is 98%, the molecular weight is 202469 g / mol, and the PDI is 2.5.
[0190] Embodiment 54
[0191] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe20 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, i.e., polyisobutylene.
[0192] The yield of low molecular weight polyisobutylene in this example is 85%, the molecular weight is 169527 g / mol, and the PDI is 2.2.
[0193] Embodiments 55 to 58
[0194] Under argon atmosphere, in a 25 mL Schlenk bottle, Fe complex Fe13 (10 μmol, 1 equiv.), 5 mL of anhydrous toluene, co-catalyst MAO (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added in sequence, and the system was placed at 25 ° C. and reacted for 2 h, 4 h, 8 h, and 16 h, respectively. The reaction was quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a colorless viscous polymer, namely polyisobutylene.
[0195] The yields of low molecular weight polyisobutylene in Examples 55 to 58 are 20%, 56%, 80% and 93% respectively, the molecular weights are 119634 g / mol, 135699 g / mol, 178532 g / mol and 196620 g / mol respectively, and the PDIs are 2.1, 2.7, 2.4 and 2.5 respectively.
[0196] Comparative Example 5
[0197] In an argon atmosphere, anhydrous toluene (5 mL), a cocatalyst ethylaluminum dichloride (2 mmol, 200 equiv., 1.5 M toluene solution) and isobutylene (4 mmol, 400 equiv.) were added to a 25 mL Schlenk bottle in sequence, and the system was placed at 25° C. for 12 h, quenched with methanol, washed with methanol, filtered and vacuum dried to obtain a white powder polymer, i.e., polyisobutylene, with a yield of >99%. The polyisobutylene in this example is a highly cross-linked polymer that cannot be dissolved and characterized.
[0198] In summary, the present invention uses a pyridine tridentate ligand iron complex as a catalyst, the polymerization reaction rate is controllable, and linear polyisobutylene with different molecular weights can be obtained by adjusting the specific type of the catalyst and the polymerization reaction time.
[0199] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A pyridine tridentate ligand iron complex, It is characterized in that Having the structure shown in formula a or formula b: In formula a, R 1 , R 2 and R 3 are independently H-, Me-, CH 3 CH 2 -、CH 3 CH 2 CH 2 -、 i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S; In formula b, R 1 , R 2 and R 3 are independently H-, Me-, CH 3 CH 2 -、CH 3 CH 2 CH 2 -、 i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
2. The pyridine tridentate ligand iron complex according to claim 1, It is characterized in that Formula a includes the structure shown by any one of the following Fe1 to Fe12: Formula b includes the structure shown in any one of the following Fe13 to Fe20:
3. A method for preparing the pyridine tridentate ligand iron complex according to claim 1 or 2, It is characterized in that The following steps are involved: Under the protection of the first inert gas, anhydrous FeCl 3 , mixing a first organic solvent and a pyridine tridentate ligand solution, and performing complexation to obtain a pyridine tridentate ligand iron complex having a structure shown in formula a or formula b; The pyridine tridentate ligand has a structure shown in formula c or formula d: In formula c, R 1 , R 2 and R 3 are independently H-, Me-, CH 3 CH 2 -、CH 3 CH 2 CH 2 -、 i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-; X is O or S; In formula d, R 1 , R 2 and R 3 are independently H-, Me-, CH 3 CH 2 -、CH 3 CH 2 CH 2 -、 i Pr-, t Bu-, F-, Cl-, Br-, OMe- or Ph-.
4. The preparation method according to claim 3, It is characterized in that Formula c includes the structure shown in any one of the following 1 to 12: Formula d includes the structures shown in any one of the following 13 to 20:
5. The preparation method according to claim 3 or 4, It is characterized in that The anhydrous FeCl 3 The molar ratio of the pyridine tridentate ligand in the pyridine tridentate ligand solution is 1:1.
05.
6. The preparation method according to claim 3 or 4, It is characterized in that The concentration of the pyridine tridentate ligand solution is 0.105 mol / L.
7. Use of the pyridine tridentate ligand iron complex according to claim 1 or 2 or the pyridine tridentate ligand iron complex prepared by the preparation method according to any one of claims 3 to 6 as a catalyst in the preparation of polyisobutylene.
8. A method for preparing polyisobutylene, It is characterized in that The following steps are involved: Under the protection of a second inert gas, a co-catalyst solution, a pyridine tridentate ligand iron complex, an isobutylene monomer and a second organic solvent are mixed to carry out a polymerization reaction to obtain the polyisobutylene; the pyridine tridentate ligand iron complex is the pyridine tridentate ligand iron complex according to claim 1 or 2 or the pyridine tridentate ligand iron complex prepared by the preparation method according to any one of claims 3 to 6.
9. The preparation method according to claim 8, It is characterized in that The co-catalyst solution is a toluene solution of the co-catalyst; the co-catalyst includes co-catalyst MAO, co-catalyst AlMe 3 , promoter AlEt 3 Or promoter Al i Bu 3 .
10. The preparation method according to claim 8 or 9, It is characterized in that The polymerization reaction temperature is -20 to 50°C and the reaction time is 2 to 48 hours.
Citation Information
Patent Citations
Catalyst for polymerization and method for producing polymer and polymer
JP2002363212A
Method for manufacturing carbon material
JP2020059619A
Transition metal complexes and olefin polymerization process
WO2000069923A1