Fluorine-modified natural rubber as well as preparation method and application thereof
By introducing highly electronegative fluorine-containing polyacrylate polymer side chains into natural rubber and utilizing its surface enrichment tendency to improve hydrophobicity and ozone resistance, the problem of limited application of natural rubber in special environments is solved and achieved It has improved efficient hydrophobicity and ozone aging resistance, making it suitable for industrial production and application.
Patent Information
- Application Number
- CN202410929696.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to its unsaturated structure, natural rubber has poor resistance to ozone, acid and alkali, and organic solvents, which limits its application in some special environments, especially in fields that require high hydrophobicity and ozone aging resistance.
By using in-situ reaction extrusion technology in a twin-screw extruder, fluorine-containing acrylate monomers are grafted to modified natural rubber, and fluorine-containing polyacrylate polymer side chains with high chemical stability and high electronegativity are introduced. , using its surface enrichment tendency to shield and protect the natural rubber molecular backbone, improving hydrophobicity and ozone aging resistance.
It effectively improves the hydrophobicity and ozone aging resistance of natural rubber, overcomes the problem of reduced hydrophobicity and ozone resistance in traditional methods, has a simple process and high production efficiency, is suitable for industrial applications, and avoids the use of organic solvents and environmental pollution. .
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of natural rubber, and in particular to a fluorine-modified natural rubber and a preparation method and application thereof. Background Art
[0002] Natural rubber has excellent comprehensive properties, such as high elasticity, wear resistance and biocompatibility [Yamashita S, et al. Annual Review of Biochemistry. 2020, 89: 821-851, De Souza Silva FK, et al. International Journal of Biological Macromolecules. 2023, 242: 124778-124790, Chen X, et al. Materials Today Communications. 2023, 34: 105372-105377], and is widely used in automobile tire manufacturing [Sattayanurak S, et al. Rubber Chemistry and Technology. 2020, 94 (1): 121-144], aerospace [Yu J, et al. Composites Part B: Engineering. 2021, 224: 109193] and medical devices [Guerra NB, et al. Materials Science and Technology. 2020, 94 (1): 121-14 ... Engineering: C. 2021, 126: 112126-112144] and other fields. However, the unsaturated structure of natural rubber itself makes its resistance to ozone, acid, alkali and organic solvents relatively poor [Cataldo F. Polymer Degradation and Stability. 2001, 73 (3): 511-520, Zheng TT, et al. Polymer Degradation and Stability. 2021, 186: 109514-109521, Yi MY, et al. Journal of Applied Polymer Science. 2023, 140 (12): 53653-53661, Zhang XM, et al.. RSC Adv. 2016, 6 (60): 54668-54678.], which limits the application of natural rubber in some special environments.Fluorine atoms have the highest electronegativity and the smallest atomic radius. Fluorinated polymers often exhibit unique chemical inertness [Améduri B.Macromol Chem Phys.2020,221(8):1900573-1900587], thermal stability [Lu XL,et al..Journal of Applied Science.2022,139(17):52016-52025], excellent hydrophobicity and oleophobicity [Liang L,et al.Molecules.2023,28(2):905-920], good solvent resistance and corrosion resistance [Indulekha K,et al.J Fluor Chem.2017;200:24-32, Liang JH,et al.Appl Surf Sci.2019,487:1000-1007]. In recent years, fluorinated polymers have been widely used in ozone-resistant materials [Cheng S, et al. Journal of Applied Polymer Science. 2023; 140 (34): 54309-54324], textile surfaces [Kredel J, et al. Acs Applied Polymer Materials. 2020, 2 (7): 2867-2879], corrosion-resistant coatings [Men PC, et al. Journal of Coatings Technology and Research. 2021, 18 (5): 1227-1235], biomaterials [Bajpai AK. Polymer International. 2007, 56 (6): 6424-6434] and fuel cells [Fazli A, et al. Materials. 2020, 13 (3): 782-812]. Therefore, fluorination of natural rubber is also expected to improve the hydrophobicity and ozone aging resistance of natural rubber.
[0003] So far, there are few reports at home and abroad on introducing highly electronegative fluorinated alkyl side chains into the main chain of natural rubber through in-situ reaction extrusion, and utilizing their low surface energy, good hydrophobicity and ozone resistance to prepare natural rubber with excellent hydrophobicity and good ozone resistance. Summary of the invention
[0004] In view of this, the embodiments of the present application provide a fluorine-modified natural rubber and a preparation method and application thereof. Natural rubber is used as raw material, and an in-situ reaction extrusion technology is adopted in a twin-screw extruder to graft-modify the natural rubber with a fluorine-containing acrylate monomer, and a fluorine-containing polyacrylate polymer side chain with high chemical stability and high electronegativity is introduced into the main chain of the natural rubber. Due to the surface enrichment tendency of the fluorine-containing polymer itself, it can play a shielding and protective role on the main chain of the natural rubber molecule, effectively improve the hydrophobicity and ozone aging resistance of the natural rubber, and can effectively overcome the defects existing in the above-mentioned prior art.
[0005] A first aspect of an embodiment of the present application provides a fluorine-modified natural rubber, which comprises the following raw materials in parts by weight: 100 parts of natural rubber, 10 to 50 parts of fluorine-containing acrylate monomers, 0 to 30 parts of styrene comonomers, and 0.4 to 0.8 parts of oxidative initiators.
[0006] In some embodiments that may include the above embodiments, the fluorine-modified natural rubber includes the following raw materials in parts by weight: 100 parts of natural rubber, 20-40 parts of fluorine-containing acrylate monomer, 20-30 parts of styrene comonomer, and 0.4-0.6 parts of oxidative initiator.
[0007] In some embodiments that may include the above embodiments, the fluorine-containing acrylate monomer is at least one of dodecafluoroheptyl methacrylate, hexafluorobutyl methacrylate, tridecafluorooctyl methacrylate, dodecafluoroheptyl acrylate, tridecafluorooctyl acrylate, and hexafluorobutyl acrylate.
[0008] In some embodiments, which may include the above embodiments, the oxidative initiator is an organic peroxide.
[0009] In some embodiments, which may include the above embodiments, the organic peroxide is at least one of dibenzoyl peroxide, cumene peroxide, and di-tert-butyl dicumyl peroxide.
[0010] A second aspect of the embodiment of the present application further provides a method for preparing the above-mentioned fluorine-modified natural rubber, comprising the following steps:
[0011] The natural rubber is added in batches to a preheated twin-screw extruder, and then a mixture solution of a fluorinated acrylate monomer, a styrene comonomer and an oxidative initiator is added in batches, and a melt extrusion reaction is carried out in a self-circulating passage. After the extruded sample is collected, it is dried in a vacuum oven to a constant weight to obtain a fluorine-modified natural rubber.
[0012] It should be noted that the fluorinated acrylate monomer and the styrene co-monomer are both oil-soluble liquids, and the oxidative initiator is an oil-soluble initiator. The oxidative initiator is dissolved in the above two liquids, so no organic solvent is required.
[0013] In some embodiments that may include the above embodiments, the following step is also included: mixing and vulcanizing the fluorine-modified natural rubber to obtain a fluorine-modified natural rubber vulcanizate.
[0014] In some embodiments that may include the above embodiments, the melt extrusion reaction temperature is 80 to 160° C., and the melt extrusion reaction time is 5 to 25 min; or
[0015] The melt extrusion reaction temperature is 120-160° C., and the melt extrusion reaction time is 5-15 minutes.
[0016] In some embodiments, which may include the above embodiments, the drying temperature is 40°C.
[0017] Preferably, a method for preparing the above-mentioned fluorine-modified natural rubber comprises the following steps:
[0018] (1) heating a twin-screw extruder to 80-160° C., taking 100 parts of natural rubber and cutting it into pieces, and dividing it into three equal parts; at the same time, mixing 10-50 parts of fluorine-containing acrylate monomer, 0-30 parts of styrene and 0-0.8 parts of oxidative initiator in proportion, and dividing it into three equal parts for standby use;
[0019] (2) adding 3 equal parts of natural rubber in batches into a preheated twin-screw extruder, adding 1 equal part of a mixture solution of a fluorinated acrylate monomer, styrene and an oxidative initiator when each equal part of natural rubber is added, and performing a melt extrusion in-situ fluorine modification reaction, the reaction time being 5 to 25 minutes;
[0020] (3) drying the extruded rubber sample in a vacuum drying oven at 40°C to a constant weight to obtain fluorine-modified natural rubber;
[0021] (4) The fluorine-modified natural rubber is kneaded and vulcanized on an open mixing mill to obtain a fluorine-modified natural rubber vulcanizate.
[0022] From the perspective of environmental friendliness and ease of industrial production, the embodiments of the present application graft a fluorine-containing acrylate polymer onto natural rubber through melt extrusion in-situ reactive extrusion technology to prepare fluorine-modified natural rubber with excellent hydrophobicity and good ozone aging resistance, which has good application prospects.
[0023] The third aspect of the embodiments of the present application also provides the use of the above-mentioned fluorine-modified natural rubber in self-lubricating medical supplies, aerospace tires, high-altitude sounding balloons, shock-absorbing seals and industrial protective rubber products.
[0024] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0025] 1. The embodiment of the present application is based on in-situ reaction extrusion technology, using natural rubber as raw material, generating fluorine-modified natural rubber by melt extrusion in-situ reaction in a twin-screw extruder, introducing highly electronegative fluoroalkyl side chains on the main chain of the natural rubber molecule, and vulcanizing it, and further preparing fluorine-modified natural rubber vulcanizate. Due to the surface enrichment trend of the fluorine-containing polymer itself, it can play an isolating and shielding protective role on the main chain of the natural rubber molecule. At the same time, due to the surface migration of the fluorine-containing polymer, it will be enriched on the surface of the natural rubber, thereby improving the hydrophobicity and ozone aging resistance of the natural rubber. The preparation process of the embodiment of the present application is simple, the production efficiency is high, the environment is friendly and easy to industrialize, and it meets the current social requirements for the green and high-performance development and application of natural rubber;
[0026] 2. The embodiments of the present application use fluorinated acrylate monomers as reaction reagents, do not use any organic solvents, and do not require complicated post-treatment, which can avoid environmental pollution and health risks caused by highly toxic organic small molecules during production and use. It also overcomes the problems of reduced hydrophobicity and ozone aging resistance and poor quality consistency caused by the gradual reduction of small molecules during use in traditional methods;
[0027] 3. The embodiments of the present application adopt a peroxide initiation system and use styrene as a co-monomer reaction reagent, which effectively reduces the chain breakage of the natural rubber molecular chain caused by extrusion shear and heat during the melt extrusion process, so that the fluorine-modified natural rubber vulcanizate exhibits mechanical properties that are not inferior to those of natural rubber, as well as excellent hydrophobicity and good resistance to organic solvents. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0029] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.
[0030] The equipment involved in the melt extrusion reaction used in the embodiments of the present application is a conical twin-screw extruder (model WLG10AG), and it is equipped with a self-circulating channel system.
[0031] In the following examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0032] Example 1
[0033] The method for preparing the fluorine-modified natural rubber of this embodiment comprises the following steps:
[0034] (1) heating a twin-screw extruder to 140° C., taking 100 parts of natural rubber and cutting it into pieces, dividing it into three equal parts, mixing 30 parts of dodecafluoroheptyl methacrylate, 22.5 parts of styrene and 0.4 parts of dibenzoyl peroxide in proportion, and dividing it into three equal parts;
[0035] (2) adding 1 part of natural rubber to a twin-screw extruder preheated to a set temperature, and simultaneously adding 1 part of the mixture solution of fluorinated acrylate monomer, styrene and oxidative initiator in step (1), and adding the natural rubber and the mixture solution of fluorinated acrylate monomer, styrene and oxidative initiator to the feeding port of the twin-screw extruder in three portions in sequence, to carry out an in-situ reaction extrusion fluorine modification reaction, and the melt extrusion reaction time in the self-circulating system is 10 minutes;
[0036] (3) After the sample is extruded, it is vacuum dried at 40°C to obtain fluorine-modified natural rubber;
[0037] (4) The fluorine-modified natural rubber is then kneaded and vulcanized on an open mill to obtain a fluorine-modified natural rubber vulcanizate.
[0038] Performance indicators of fluorine-modified natural rubber vulcanizate: side chain fluorine modification rate is 37.93wt%, water contact angle is 104o, and the time for 1mm microcrack to appear is 4h.
[0039] It should be noted that the side chain fluorine modification rate is calculated by titration. The hydrophobicity is measured by contact angle goniometer (JC2000C). The ozone aging resistance is measured by ozone aging chamber (OZ-0500BC), and the test conditions are: test temperature is 40℃, humidity is 45%, ozone concentration is 100pphm, and the time for the appearance of surface microcracks with a length of 1mm is used as a reference. For details, please refer to GB / T 7762-2014.
[0040] Example 2
[0041] The method for preparing the fluorine-modified natural rubber of this embodiment comprises the following steps:
[0042] (1) heating a twin-screw extruder to 120° C., taking 100 parts of natural rubber and cutting it into pieces, dividing it into three equal parts, mixing 30 parts of hexafluorobutyl methacrylate, 0 parts of styrene and 0.4 parts of cumene peroxide in a certain proportion, and dividing it into three equal parts;
[0043] (2) adding 1 part of natural rubber to a twin-screw extruder preheated to a set temperature, and adding 1 part of the mixture solution of fluorinated acrylate monomer, styrene and oxidative initiator in step (1) at the same time, the natural rubber and the mixture solution of monomer, styrene and oxidative initiator are added to the feeding port of the twin-screw extruder in three portions, and an in-situ reaction extrusion fluorine modification reaction is carried out, and the melt extrusion reaction time in the self-circulating system is 6 minutes;
[0044] (3) After the sample is extruded, it is vacuum dried at 40°C to obtain fluorine-modified natural rubber;
[0045] (4) The fluorine-modified natural rubber is kneaded and vulcanized on an open mixing mill to obtain a fluorine-modified natural rubber vulcanizate.
[0046] Performance indicators of fluorine-modified natural rubber vulcanizate: side chain fluorine modification rate is 24.88wt%, water contact angle is 98o, and the time for 1mm microcrack to appear is 2h.
[0047] Example 3
[0048] The method for preparing the fluorine-modified natural rubber of this embodiment comprises the following steps:
[0049] (1) heating a twin-screw extruder to 130° C., taking 100 parts of natural rubber and cutting it into pieces, dividing it into three equal parts, mixing 10 parts of tridecafluorooctyl methacrylate, 0 parts of styrene and 0.4 parts of di-tert-butyl diisopropylbenzene peroxide in proportion, and evenly dividing it into three equal parts;
[0050] (2) adding 1 part of natural rubber to a twin-screw extruder preheated to a set temperature, and simultaneously adding 1 part of a mixture solution of a fluorinated acrylate monomer, styrene and an oxidative initiator in step (1), and adding the natural rubber and the mixture solution of the monomer, styrene and an oxidative initiator to the feeding port of the twin-screw extruder in three portions in sequence, to carry out an in-situ reaction extrusion fluorine modification reaction, and the melt extrusion reaction time in the self-circulating system is 8 minutes;
[0051] (3) After the sample is extruded, it is vacuum dried at 40°C to obtain fluorine-modified natural rubber;
[0052] (4) The fluorine-modified natural rubber is kneaded and vulcanized on an open mixing mill to obtain a fluorine-modified natural rubber vulcanizate.
[0053] Performance indicators of fluorine-modified natural rubber vulcanizate: side chain fluorine modification rate is 14.64wt%, water contact angle is 89o, and the time for 1mm microcrack to appear is 1h.
[0054] Example 4
[0055] The preparation method of the fluorine-modified natural rubber provided in this embodiment can refer to Example 1, except that the fluorine-containing acrylate monomer is dodecafluoroheptyl acrylate.
[0056] Example 5
[0057] The preparation method of the fluorine-modified natural rubber provided in this embodiment can refer to Example 1, except that the fluorine-containing acrylate monomer is tridecafluorooctyl acrylate.
[0058] Example 6
[0059] The preparation method of the fluorine-modified natural rubber provided in this embodiment can refer to Example 1, except that the fluorine-containing acrylate monomer is hexafluorobutyl acrylate.
[0060] Example 7
[0061] The preparation method of the fluorine-modified natural rubber provided in this embodiment can refer to Example 1, except that the addition amount of each raw material is: 100 parts of natural rubber, 10 parts of dodecafluoroheptyl methacrylate, 30 parts of styrene, and 0.8 parts of dibenzoyl peroxide.
[0062] Example 8
[0063] The preparation method of the fluorine-modified natural rubber provided in this embodiment can refer to Example 1, except that the addition amount of each raw material is: 100 parts of natural rubber, 50 parts of dodecafluoroheptyl methacrylate, 10 parts of styrene comonomer, and 0.4 parts of dibenzoyl peroxide.
[0064] Comparative Example 1
[0065] As a comparative example, the performance indicators of the natural rubber vulcanizate obtained by mixing and vulcanizing the pure natural rubber without fluorine modification on an open mill are as follows: the side chain fluorine modification rate is 0wt%, the water contact angle is 86o, and the time for the appearance of 1mm microcracks is 0.5h.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A fluorine-modified natural rubber, characterized in that: The fluorine-modified natural rubber comprises the following raw materials in parts by weight: 100 parts of natural rubber, 10-50 parts of fluorine-containing acrylate monomers, 0-30 parts of styrene comonomers, and 0.4-0.8 parts of oxidative initiators.
2. The fluorine-modified natural rubber according to claim 1, characterized in that: The fluorine-modified natural rubber comprises the following raw materials in parts by weight: 100 parts of natural rubber, 20-40 parts of fluorine-containing acrylate monomers, 20-30 parts of styrene comonomers, and 0.4-0.6 parts of oxidative initiators.
3. The fluorine-modified natural rubber according to claim 1, characterized in that: The fluorine-containing acrylic ester monomer is at least one of dodecafluoroheptyl methacrylate, hexafluorobutyl methacrylate, tridecafluorooctyl methacrylate, dodecafluoroheptyl acrylate, tridecafluorooctyl acrylate and hexafluorobutyl acrylate.
4. The fluorine-modified natural rubber according to claim 1, characterized in that: The oxidative initiator is an organic peroxide.
5. The fluorine-modified natural rubber according to claim 4, characterized in that: The organic peroxide is at least one of dibenzoyl peroxide, cumene peroxide and di-tert-butyl dicumyl peroxide.
6. A method for preparing the fluorine-modified natural rubber according to any one of claims 1 to 5, characterized in that: The following steps are involved: The natural rubber is added in batches to a preheated twin-screw extruder, and then a mixture solution of a fluorinated acrylate monomer, a styrene comonomer and an oxidative initiator is added in batches, and a melt extrusion reaction is carried out in a self-circulating passage. After the extruded sample is collected, it is dried in a vacuum oven to a constant weight to obtain a fluorine-modified natural rubber.
7. The method for preparing fluorine-modified natural rubber according to claim 6, characterized in that: The method also includes the following steps: mixing and vulcanizing the fluorine-modified natural rubber to obtain a fluorine-modified natural rubber vulcanizate.
8. The method for preparing fluorine-modified natural rubber according to claim 6, characterized in that: The melt extrusion reaction temperature is 80 to 160° C., and the melt extrusion reaction time is 5 to 25 minutes; or The melt extrusion reaction temperature is 120-160° C., and the melt extrusion reaction time is 5-15 minutes.
9. The method for preparing fluorine-modified natural rubber according to claim 6, characterized in that: The drying temperature is 40°C.
10. Use of the fluorine-modified natural rubber according to any one of claims 1 to 5 in self-lubricating medical products, aerospace tires, high-altitude sounding balloons, shock-absorbing seals and industrial protective rubber products.
Citation Information
Patent Citations
Polypropylene material with low surface tension and method for preparing the same
CN101200524A
Chemically-modified natural rubber and preparation method thereof
CN106632862A
Preparation method of fluorine-containing grafted polyolefin material
CN112608412A
Fluorine-modified natural rubber with high storage stability and preparation method thereof
CN116178628A
Graft copolymers containing fluoroaliphatic groups
US5336717A