Topological structure polymer

By introducing a topological structure of four-arm dynamic cross-linking points and multiple dynamic bonds into the polymer, the contradiction in processing and recycling of thermosetting plastics is solved, a combination of high mechanical properties and good processing performance is achieved, and self-healing and reversible properties are provided. properties, for high-performance and recyclable elastomers.

CN118745240AActive Publication Date: 2024-10-08DONGHUA UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410793689.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-08
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

There are contradictions in processing and recycling of existing thermoset plastics, and it is difficult to have high mechanical properties and good processability at the same time.

Method used

A topological polymer with four-arm dynamic cross-linking points is used to couple the locking units through dynamic amidine-urea bonds and oxime-urethane bonds, and combined with the four-functional cross-linking agent diaminoglyoxime (DAG) to construct a A network of triple dynamic bonds improves mechanical properties and facilitates flow at high temperatures.

Benefits of technology

It achieves high tensile strength, reversibility and good processing properties of the polymer, eliminates the contradiction between mechanical strength and reprocessing properties, and provides a unique design of self-healing elastomers suitable for high performance and recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745240A_ABST
    Figure CN118745240A_ABST
Patent Text Reader

Abstract

The invention relates to a polymer with a topological structure. The structure of the polymer is shown as a general formula I, the self-repairing elastomer is successfully prepared, and the contradiction between the processing performance and the mechanical performance is decoupled. A novel dynamic amidine-urea bond and oxime-carbamate bond coupling locking unit is designed to construct an elastomer with high performance and good processability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymers, and in particular relates to a topological structure polymer. Background Art

[0002] Thermosets and thermoplastics are two traditional classifications of polymers. Thermosets are strong and stable and are typically synthesized through covalent cross-linking of polymer chains, forming a network throughout the sample. However, stability, a hallmark of thermosets, comes at the expense of being unable to be recycled through traditional methods such as direct mechanical reprocessing. As the demand for sustainable materials continues to increase, prioritizing polymers that combine the mechanical properties of thermosets with the processability and recyclability of thermoplastics can effectively reduce the carbon footprint of the plastics industry.

[0003] Considerable efforts have been devoted to developing reversible crosslinks in covalent adaptive networks (CANs), which enable the destruction and reorganization of connections between polymer chains, blurring the boundary between thermosets and thermoplastics. Despite the widespread use of a variety of dynamic covalent bonds in thermosets, achieving CANs with excellent processability and high mechanical strength remains a challenge in polymer science. This is due to the fundamental trade-off between sufficient chain mobility for dynamic exchange and sufficiently stable structure for robust mechanical properties. Therefore, discovering innovative dynamic chemical strategies or topological network designs that effectively reconcile this dichotomy is a top priority for polymer researchers. Since Wudl's seminal report on thermally repairable networks utilizing Diels-Alder reactions in 2001, many other reversible processes (e.g., urea bonds, boron-oxygen bonds, and disulfide bonds) have been explored to address processing challenges associated with thermoset polymers. The Yan group has been working on designing exquisite microtopological networks to tune macroscopic material properties. Recently, in 2022, they proposed a polymer network inspired by interlaced woven fibers that successfully balanced dynamic behavior and robust stability using Cu(I) ion coordination crosslinks. While these dynamic responses and network designs endow dynamic polymers with adaptable and responsive properties, the inherent contradiction between the mechanical properties and processing performance of the materials still exists. Summary of the invention

[0004] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a topological structure polymer, in particular a topological structure polymer with four-arm dynamic cross-linking points.

[0005] The present invention provides a polymer represented by the following general formula I:

[0006]

[0007] Wherein x=12-28; wherein the wavy lines represent repeated segments.

[0008] Preferably, the polymer has a topological network structure polymer of four-arm dynamic cross-linking points of adjacent dynamic bonds, with dynamic amidine-urea bonds and oxime-carbamate bonds coupling locking units.

[0009] The present invention provides a method for preparing the polymer, comprising:

[0010] The alcohol and diisocyanate are mixed and reacted under protective gas conditions to obtain a prepolymer, and then a tetrafunctional crosslinking agent and a solvent are added and reacted to obtain a polymer.

[0011] The alcohol is alcohol after drying.

[0012] Preferably, the alcohol is a diol; the diol is polytetrahydrofuran; the M of the diol is n =1000-2000gmol -1 ; The diisocyanate is isophorone diisocyanate IPDI; the solvent is tetrahydrofuran or N,N-dimethylformamide;

[0013] Preferably, the tetrafunctional crosslinking agent contains two oximes and two amines.

[0014] More preferably, the tetrafunctional cross-linking agent is diaminoglyoxime DAG.

[0015] Preferably, the reaction temperature under the protective gas is 80-110° C. and the reaction time is 2-4 hours; wherein the protective gas is at least one of nitrogen and argon.

[0016] Preferably, the tetrafunctional crosslinking agent and solvent are added to react, wherein the reaction temperature is 40-60° C. and the reaction time is 24-48 hours.

[0017] Preferably, the molar ratio of the alcohol to the diisocyanate is (1-5):(1-3); and the molar ratio of the prepolymer to the tetrafunctional crosslinking agent is (1-9):(1-6).

[0018] More preferably, the molar ratio of the prepolymer to the tetrafunctional crosslinking agent is 4:3 to 2:1.

[0019] The invention provides an application of the polymer in the field of remodelable processing.

[0020] A new strategy for constructing polymer topological networks, namely, dynamic cross-linking coupled locking units, rather than the usual independent dynamic covalent cross-linking or supramolecular cross-linking, is proposed in this paper to improve mechanical properties at ambient temperature while inducing a rare melting point reduction - a phenomenon rarely seen in previous polymer chemistry studies. The key to the topological structure design is the tetrafunctional cross-linker diaminoglyoxime (DAG), in which two oximes and two amines can react with isocyanate to generate dynamic covalent oxime-carbamate bonds and hydrogen-bonded dynamic covalent amine-urea bonds, thereby constructing a cross-linked network with triple dynamic bonds. At room temperature, the dynamic bonds are in a frozen state, which is conducive to significantly improving the mechanical properties of DAG-PU elastomers by increasing the cross-linking density. As the temperature increases, the integrated dynamic bond density at the cross-linking point is higher and more likely to induce dissociation, resulting in the rapid disintegration of the network into a prepolymer, which is easy to flow. Overall, the design of locking units with synergistic multiple dynamic covalent and non-covalent bonds eliminates the contradiction between the mechanical strength and reprocessing performance of the polymer. Furthermore, networks with higher crosslink density exhibited significant enhancements in tensile strength and shock absorption compared to networks with lower density connections. Furthermore, these networks possessed superior toughness and resistance to deformation creep under sustained loading before significant bond dissociation.

[0021] Beneficial Effects

[0022] The present invention successfully prepared a self-healing elastomer, decoupling the contradiction between processing performance and mechanical properties. A new dynamic amidine-urea bond and oxime-carbamate bond coupling locking unit was designed to construct a high-performance elastomer with good processing performance.

[0023] DAG concentrates triple dynamic bonds in one locking unit, instead of forming covalent or non-covalent cross-linking bonds that are usually independent of each other, to avoid the formation of too many obvious cross-linking sites, thereby ensuring high fluidity of the polymer chain. At the same time, the adjacent dynamic bonds trigger the neighboring group effect, catalyzing the dynamic dissociation of oxime-carbamate, and the unit exhibits high mechanical properties and reversibility. This new molecular design of the locking unit with coupled multiple bonds and multiple cross-linking site topologies can effectively solve the long-standing contradiction between the high tensile strength and processability of the material. Therefore, the present invention proposes a unique molecular design that couples multiple dynamic bonds in one locking unit to simultaneously regulate the chemical and topological structures of the polymer, which provides a new and powerful principle for regulating material properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1Design of topological structure of DAG-PU elastomer for decoupling processability and mechanical properties; including chemical structures and cartoon representations of prepolymer monomer A and crosslinker monomer B as well as hydrogen bonding units; schematic diagrams of dynamic oxime-carbamate bond and dynamic amine-urea bond mechanisms; schematic diagrams of robust mechanical properties of polymer networks at room temperature and dynamic properties at high temperatures;

[0025] Figure 2 Basic performance characteristics of DAG-PU elastomers; (a) Fourier transform infrared absorption spectra of DAG-PU-1, DAG-PU-2 and DAG-PU-3; (b) Temperature-dependent infrared spectroscopy to explore the effect of temperature on the dissociation of dynamic covalent bonds in DAG-PU-3; (c) Swelling ratio curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 in THF; (d) Stress-strain curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 recorded at a deformation rate of 50 mm / min; (e) The stress-strain curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 calculated based on the stress-strain curves Toughness and Young's modulus of DAG-PU-3; (f) Storage modulus and loss modulus of DAG-PU-1, DAG-PU-2 and DAG-PU-3 recorded by frequency sweep at 30 °C; (g) Cyclic tensile test of DAG-PU-1, DAG-PU-2 and DAG-PU-3, with a maximum applied strain of 100%; (h) Calculation of the dissipated toughness ratio of DAG-PU-1, DAG-PU-2 and DAG-PU-3 in five consecutive loading-unloading tensile tests; (i) Calculation of the damping capacity of DAG-PU-1, DAG-PU-2 and DAG-PU-3 based on the cyclic tensile test;

[0026] Figure 3 Thermal properties of DAG-PU elastomers; (a) Tanδ curves of temperature sweeps of DAG-PU-1, DAG-PU-2 and DAG-PU-3 using rheological tests; solid-liquid transition occurs at temperatures of approximately 150 to 130°C; (b) Summary of glass transition temperature and solid-liquid transition temperature data of DAG-PU-1, DAG-PU-2 and DAG-PU-3; (c) Viscosity-temperature curves of DAG-PU-1 and DAG-PU-3; (d) Comparison of mechanical properties and processing properties of DAG-PU-1, DAG-PU-2 and DAG-PU-3;

[0027] Figure 4 To gain a deeper understanding of the structure-property relationship of DAG-PU elastomers; (a) The conversion rate of compound b when reaching equilibrium with or without amidine-urea bonds (conversion rate = ([b]0-[b] t ) / ([b]0-[b] eq ), [b]0: the concentration of the initial concentration b, [b]t : The concentration of b at time t, [b] eq : equilibrium concentration of b); (b) normalized stress relaxation curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 measured at 60°C; (c) normalized stress relaxation curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 measured at 130°C; (d) fitting of relaxation time to Arrhenius equation; (e) strain scanning curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 at 130°C; (f) creep recovery curves of DAG-PU-1, DAG-PU-2 and DAG-PU-3 with the same stress level at 100°C;

[0028] Figure 5 is the molecular formula of DAG-PU, and the value of x is about 12 to 28;

[0029] Figure 6 (a) Schematic diagram of the DAG-PU reprocessing process and the mechanism of dynamic oxime-carbamate and amidine-urea bonds. (b) FTIR spectra, (c) stress-strain curves, and (d) temperature sweep rheological analysis of pristine and reprocessed DAG-PU-3 samples, indicating that the chemical and mechanical integrity is retained. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0031] Unless otherwise stated, all tests were performed at room temperature. Nuclear magnetic resonance (NMR) spectra were recorded with a Bruker Avance 600 spectrophotometer using deuterated solvents as lock substances and residual solvent or TMS as internal reference.

[0032] FTIR spectra were recorded on a Nicolet 8700 spectrometer. Attenuated total reflectance Fourier transform infrared (ATR-FTIR) spectra were recorded on a Thermo Fisher Scientific Nicolet iS50 spectrometer with an ATR accessory.

[0033] The surface morphology of the samples was studied using a * / Dimension FastScan / lcon atomic force microscope (AFM) with an aluminum reflective-coated silicon cantilever probe (HQ:NSC19 / Al BS).

[0034] The glass transition temperature was obtained by dynamic thermomechanical analysis on a DMA1 (Mettler-Toledo). Dynamic mechanical analyzer. Rectangular samples (approximately 1 mm (T) × 5 mm (W) × 10 mm (L)) were tested at a frequency of 1 Hz and a strain of 0.1%. The temperature was adjusted from -120 °C to 80 °C with a 5 °C min -1 The heating rate is calculated from the maximum value of tanδ. g value.

[0035] Thermogravimetric analysis (TGA) was used to study the dynamic thermal stability using a thermogravimetric analyzer (Libra / 209F1). -1 The synthesized copolymers were evaluated at 600 °C with a heating rate of .

[0036] Rheological experiments were performed using an Anton Paar MCR702 stress-controlled rheometer with an 8 mm parallel plate attachment. Normalized stress relaxation experiments were performed in strain-controlled (10% strain) mode. The relaxation modulus (G) was normalized by the initial value (G0). a represents the activation energy, τ0 represents the characteristic relaxation time at 1 / e, R is the gas constant, T is the temperature relaxation time, and τ(T) corresponds to the time it takes for the modulus to relax to 1 / e. a It can be calculated by multiplying the slope obtained by plotting ln(τ)-1000 / T by the constant R. The characteristic relaxation time (τ*) is defined as the time required for G / G0=1 / e, with an exponential decay function: G(t)=G0 exp(-t / τ*).

[0037] The mechanical properties of the samples were evaluated using an MTS E42 tensile machine equipped with a 100 N load cell. -1 When the film is cut from a large film, a uniaxial tensile test is performed. A rectangular tensile bar (1 mm (T) × 3 mm (W) × 20 mm (L)) cut from a large film is used. The deflection rate for uniaxial tensile measurements is 50 mm / min. At least three samples are tested for each sample and the average value is taken. If not specified, the cyclic tensile test is performed at a deflection rate of 50 mm / min. -1 The tensile rate is 50 mm min. -1 The energy dissipation is calculated by integrating the area enclosed by the cyclic stretch curve. The damping capacity is defined as the ratio of the dissipated energy (the area enclosed by the loading and unloading curves) to the loaded energy (the area enclosed by the loading curve).

[0038] Example 1

[0039] Polytetrahydrofuran (M n=1000) (PTMEG, 24 g, 24 mmol) was added to a glass reactor equipped with a magnetic stirrer and dried at 110 ° C for 2 hours under vacuum. After cooling to 70 ° C, isophorone diisocyanate (IPDI, 10.68 g, 48 mmol) was added dropwise to the reactor and heated to 110 ° C for 2 hours under a nitrogen atmosphere. After cooling to 60 ° C, diaminoglyoxime (DAG, 1.42 g, 12 mmol) and THF (265 mL) were added and reacted for 24 hours, and the ratio corresponded to A: B = 2: 1. The solution after the above reaction was poured into a tetrafluoroethylene mold and dried to obtain DAG-PU-1.

[0040] The preparation method of DAG-PU-2 is the same as that of DAG-PU-1, except that 54 mmol, 12.00 g of isophorone diisocyanate and 15 mmol, 1.77 g of diaminoglyoxime are added, and the corresponding ratio is A:B=8:5.

[0041] The preparation method of DAG-PU-3 is the same as that of DAG-PU-1, except that 60 mmol, 13.34 g, of isophorone diisocyanate and 18 mmol, 2.13 g, of diaminoglyoxime are added, and the corresponding ratio is A:B=4:3.

[0042] Design, synthesis, structural characterization and mechanical properties of DAG-PU.

[0043] Polyurethane is widely used in the preparation of elastomeric materials due to its mechanical properties. For this reason, the present invention selects PU as the polymer component. Commercially available polytetramethylene glycol (PTMEG), isophorone diisocyanate (IPDI) and diaminoglyoxime (DAG) are used to synthesize the DAG-PU network by one-pot polycondensation. PTMEG is selected as the soft segment because its flexible chain is conducive to chain movement, thereby achieving better self-repair. IPDI is selected as the hard segment because its bulky structure can inhibit crystallization and increase the mobility of the chain to achieve better self-repair. Due to the spatial influence of the cyclohexyl ring, the IPDI-derived carbamate has relatively high dynamics, which further promotes the reorganization of the covalent network. DAG is crucial in the design of DAG-PU. Its two oxime groups can form reversible dynamic bonds with isocyanate, while its two amino groups can form dynamic amidine-urea bonds, providing many hydrogen bonds, dissipating energy during mechanical deformation and resulting in high toughness. The simultaneous presence of multiple dynamic bonds gives it processability, while the relatively strong chemical crosslinking ensures its stable mechanical properties and structural stability (such as Figure 1 shown).

[0044] The structure of the polymer network was first investigated by Fourier transform infrared spectroscopy (FTIR) in attenuated total reflectance (ATR) mode. Figure 2As shown in a, -N=C=O group corresponds to 2275 cm -1 The peaks near 3329 cm completely disappeared in the polymer network, indicating that IPDI and the formed monomer with -N=C=O group had reacted completely. -1 and 1717cm -1 The peaks at 1533 cm-1 were assigned to the stretching vibrations of NH and C=O, respectively, which is consistent with the formation of carbamate groups. -1 and 954cm -1 peaks, indicating the presence of DAG in the polymer network. To elucidate the dynamic properties of DAG-PU, temperature-dependent Fourier transform infrared (FTIR) spectroscopy was performed. The FTIR results at different temperatures revealed the integrity of the oxime-carbamate bonds in DAG-PU at room temperature. In addition, a small portion of free isocyanate (2275 cm -1 ) will separate from the oxime-carbamate bond ( Figure 2 b) Above 130°C, the oxime-carbamate bond in DAG-PU dissociates significantly. Then, the sample is subjected to a swelling test in THF to confirm the formed network structure. The results show that the sample exhibits significant swelling behavior in THF. Figure 2 As shown in Fig. c, after immersion in THF for 30 minutes, the size of the sample increased significantly. In this case, the high cross-linked network in DAG-PU-3 will limit the expansion of the network, which is the reason for its low swelling rate. In contrast, DAG-PU-1 with low cross-linking density has a higher swelling rate, which also proves the design of the present invention.

[0045] The mechanical properties of the three polymers were investigated by tensile tests to reveal the differences caused by the increase in their degree of cross-linking. Figure 2 As shown in Figure d, the stress-strain curves of all samples exhibit typical rubber-like tensile behavior. DAG-PU-3 has the highest modulus and strength due to its highest crosslinker content and highest hydrogen bond density. The Young's modulus of DAG-PU-1, DAG-PU-2 and DAG-PU-3 are 3.8±1.0, 12.3±2.0 and 29.7±0.9MPa, respectively, and the maximum stresses are 19.5±1.6, 28.6±8.1 and 45.0±1.7MPa, respectively. The elongation at break decreases with the increase of crosslinking points, which are 1039.7±32.8%, 717.3±23.3% and 567.3±37.8%, respectively. It is worth noting that due to its good strength and elongation, it is comparable to DAG-PU-2 (94.9±15.6MJ / m 3 ) and DAG-PU-1 (51.7±18.2MJ / m 3), DAG-PU-3 has the highest toughness, which is 105.5±12.9MJ / m 3 ( Figure 2 e). These results indicate that the material has a higher toughness due to the increase in cross-linking. The frequency sweep results are consistent with the tensile test results ( Figure 2 f). The storage modulus of DAG-PU-3 is higher than that of DAG-PU-1 and DAG-PU-2, indicating that the network with higher cross-linking density has a stiffer characteristic.

[0046] Subsequently, cyclic stress-strain tests with maximum strains ranging from 100% to 500% were performed on three different samples, and the quantitative analysis of energy dissipation is summarized in Figure 2 h. It is noteworthy that all three networks exhibit considerable hysteresis, with the amplitude of the hysteresis loop increasing with increasing crosslinking levels. This enhancement is mainly attributed to the dissociation of hydrogen bonds prevalent in the polyurethane segments. The damping capacity is defined as the ratio of energy dissipated to input energy and is summarized in the calculation results based on cyclic tensile tests. Figure 2 i. The change in damping capacity may be related to the effect of cross-linking on the energy dissipation mechanism. The results show that the damping capacity decreases with increasing strain levels applied to samples with different cross-linking densities, which may originate from the tendency of the chemically cross-linked network to recover its original size mainly through elastic deformation under high strain.

[0047] Thermal properties, self-healing and reprocessability of DAG-PU

[0048] So far, the advantages of tetrafunctional crosslinking in ensuring the mechanical properties of materials have been confirmed, and a series of explorations have been carried out to enhance its processing properties. DMA studies have shown that all DAG-PU-1 to 3 have two different glass transition temperatures (T g The transition observed in DAG-PU at about -60 °C is attributed to the relaxation of the soft polytetrahydrofuran segments, which is independent of the content of rigid crosslinks in the network. It is worth noting that DAG-PU-1~3 also exhibit a second T g , the measurement range is -15.2 to 33.8℃. g The value shows an upward trend, which is due to the fact that as more hard segments are added, the network becomes denser, making it more difficult for the polymer segments to move. In order to better understand the temperature dependence of the viscoelasticity of DAG-PU, G' and G". were studied in an extended temperature scan. The temperature corresponding to the point where the loss tangent (tanδ) equals 1 represents the transition temperature (T) where the material changes from the rubbery state to the viscous state. f ), which can be generally approximated as the lower limit of the material reprocessing temperature range. When the viscous response dominates the viscoelastic behavior, T fThe corresponding values ​​recorded for DAG-PU-1, DAG-PU-2 and DAG-PU-3 were 153.8℃, 147.7℃ and 131.3℃ ( Figure 3 a), indicating that the relaxation is accelerated with the increase of the dynamic bond concentration in DAG-PU. f Below, the elastic platform of DAG-PU-3 is not obvious, but the elastic platform of DAG-PU-1 is obvious, which means that DAG-PU-3 has a more dynamic network than the control group. f As shown above, G' and G" of all three samples decrease with increasing temperature, indicating final relaxation. The glass transition temperatures (T g ) and solid-liquid transition temperature (T f ) has been summarized in Figure 3 b. Figure 3 c clearly illustrates the alternating viscosity variation trends of DAG-PU-1 and DAG-PU-3. A significant transition in complex viscosity occurs near the solid-liquid transition point of the material. DAG-PU-3 exhibits higher crosslinking density and complex viscosity at low temperatures. However, when heated to the dissociation temperature, the higher content of dynamic bonds in DAG-PU-3 causes the polymer network to collapse rapidly through dissociation, decomposing into small molecular chains that are easy to move, resulting in a significant decrease in the complex viscosity of DAG-PU-3. This result provides intuitive evidence for the performance of highly crosslinked materials that are easier to process.

[0049] Structure-property relationships of DAG-PU.

[0050] Increasing the degree of crosslinking significantly improves the mechanical and reprocessing thermal properties of DAG-PU, as demonstrated by tensile and thermal analysis. However, there is still interest in understanding how highly crosslinked polymers affect the mechanical behavior and how they can reduce the thermally treated solid-liquid transition temperature while still improving the mechanical properties of DAG-PU. To address these questions, rheological experiments and 1 HNMR spectroscopy was performed to fully understand the structure-property relationship of DAG-PU. To investigate the reversibility of the DAG unit, a small molecule model containing an amidine-urea bond and an oxime-carbamate bond was synthesized and mixed with benzyl isocyanate in deuterated DMSO-d6. The exchange reaction was monitored by HNMR and its equilibrium rate was calculated. It took nearly 36 hours to reach equilibrium at 25°C ( Figure 4 a), while the exchange reaction without amino groups reached equilibrium only after 50 hours. Therefore, it can be inferred that the neighboring group effect in the DAG group leads to a higher reversibility of the oxime-carbamate bond compared to the oxime without amino groups. This experiment clearly demonstrates the reversibility of the amidine-urea bond, thereby promoting the dynamic reorganization of the DAG-PU chain.

[0051] Stress relaxation and creep experiments can also yield valuable structural information about the network. Bond dissociation in the CAN leads to significant stress relaxation, and the scaling of the characteristic relaxation time (τ*) with temperature is an important aspect in describing its rheological behavior. Figure 4 As shown in Fig. 2b, the smallest relaxation was observed among the three sample groups. It is worth noting that DAG-PU-3 did not relax after 3000 s at 60 °C, while DAG-PU-1 and DAG-PU-2 experienced slightly faster stress relaxation behavior. Subsequently, the same stress was applied to all three samples at 130 °C, and obvious changes were observed ( Figure 4 c). The results show that DAG-PU-3 relaxes rapidly within 100 s, which is in stark contrast to the results obtained at 60 °C. Given the dependence of the relaxation behavior of the polymer network on its individual crosslinks, the findings reinforce the view that DAG-PU-3 has a higher density of dynamic crosslinks compared to DAG-PU-1 and DAG-PU-2. As mentioned earlier, at 60 °C, stress maintenance is commendable until the bonds begin to dissociate extensively, and then stress relaxation accelerates at increasing temperatures. It is assumed that dynamic crosslink activation occurs around 130 °C, but it is speculated that stress release is not complete even after extensive bond dissociation, which may be attributed to the presence of partial crosslinks. The traditional 1 / e method for stress relaxation experiments was first used to determine τ as the time when the normalized stress drops to 36.8% (1 / e) of the initial value. ln(τ) shows a good linear relationship with 1000 / T ( Figure 4 e), the apparent activation energies calculated from their slopes were 97.42 kJ / mol, 87.72 kJ / mol, and 76.98 kJ / mol (for DAG-PU-1, DAG-PU-2, and DAG-PU-3, respectively). Increasing the number of oxime carbamate bonds enhances the sensitivity of dynamic exchange to temperature. Similarly, increasing the number of crosslinking points reduces the temperature sensitivity of CAN. In the present study, both the number of dynamic bonds and the number of crosslinks were increased, combined with the catalysis of the neighboring group effect, suggesting that the synergistic effect of these two factors led to a decrease in activation energy with increasing DAG. Since this activation energy is related to the dissociation of dynamic crosslinks in DAG-PU, the lower activation energy of DAG-PU-3 indicates that its dynamic crosslinks can be more easily broken with increasing temperature, thereby improving its processing properties. The viscoelastic behavior of the three samples was studied using strain sweep tests. The changes in G' and G" with increasing oscillation amplitude reflect the integrity of the network. As Figure 4As shown in Figure 5e, under an oscillatory strain of 5.25%, the G' and G" of DAG-PU-3 first intersect, indicating that the DAG-PU-3 network is damaged due to a large amount of dynamic bond dissociation. On the other hand, under the same strain conditions, the G' and G" of DAG-PU-1 show smaller changes at larger oscillation amplitudes because it has a lower dynamic bond density and can maintain the network. Rheological experiments show that at temperatures below the temperature at which dynamic crosslinks are extensively dissociated, the network remains elastic even under large applied strains. In contrast, once significant bond dissociation occurs, smaller strains can easily damage the network. In order to verify the stability of the polymer before network dissociation, creep and recovery experiments were carried out on DAG-PU-1, DAG-PU-2, and DAG-PU-3 at 50°C and 100°C under an applied load of 800Pa, respectively. DAG-PU-3 also maintains its excellent creep resistance at 100°C, and the creep strain of this network is only 0.15%. These creep strain values ​​are almost comparable to those exhibited by the static network. It is noted that the oxime-carbamate and amidine-urea bonds in DAG-PU have been shown to undergo significant dissociation reactions at 100 °C ( Figure 4 f). Therefore, the DAG-PU dynamic chemistry is expected to be active but at a very low level during creep testing at 100 °C. This is also confirmed by the creep recovery behavior of the network at 100 °C, as the strain is not fully recovered 300 s after stress relief. However, considering the negligible creep strain and low residual strain, the triple dynamic bond dissociation rate is believed to be low enough to almost prevent creep at 100 °C. This study provides a comparative investigation of the decoupling of mechanical properties and thermal processing characteristics of dynamic polymer networks through topological design. It is expected that the fundamental insights gained from the study will guide the development of high-performance, easy-to-process elastomers through topological network design strategies.

[0052] DAG-PU reshaping application

[0053] The processability of DAG-PU-3 was studied through cyclic remodeling experiments, demonstrating its practical performance in the field of recycled elastomers. Figure 6In the paper, the reprocessing process of DAG-PU-3 samples is described, in which the mechanism of heating to activate dynamic bonds is also emphasized. The original sample of DAG-PU-3 was cut into small pieces and reprocessed by compression molding at 110°C and 5MPa pressure for 10 minutes to obtain the reshaped sample. Unlike self-healing properties, processability places more stringent requirements on the dynamic properties of crosslinking. This process was repeated three times, and as shown in the figure, the original and reshaped DAG-PU-3 showed almost identical FTIR spectra, indicating that the chemical integrity was maintained after three reprocessing. In addition, tensile tests and rheological temperature scans were performed on the reprocessed DAG-PU-3, and it was demonstrated that it has excellent reprocessability in terms of maintaining mechanical properties (including storage modulus and toughness). The good reprocessability of DAG-PU-3 means that the tetrafunctional crosslinker has good dynamic properties. It also shows good application prospects for it in the field of recyclable elastomers.

Claims

1. A polymer represented by the following general formula I, Where n=12-28.

2. The polymer according to claim 1, characterized in that The polymer has a topological network structure polymer with four-arm dynamic cross-linking points.

3. A method for preparing the polymer according to claim 1, comprising: The alcohol and diisocyanate are mixed and reacted under protective gas conditions to obtain a prepolymer, and then a tetrafunctional crosslinking agent and a solvent are added and reacted to obtain a polymer.

4. The preparation method according to claim 3, characterized in that: The alcohol is a diol; the diol is polytetrahydrofuran; the M of the diol n =1000~2000g mol -1 ; The diisocyanate is isophorone diisocyanate IPDI; the solvent is tetrahydrofuran or N,N-dimethylformamide.

5. The preparation method according to claim 3, characterized in that: The tetrafunctional crosslinking agent contains two oximes and two amines.

6. The preparation method according to claim 5, characterized in that: The tetrafunctional cross-linking agent is diaminoglyoxime DAG.

7. The preparation method according to claim 3, characterized in that: The reaction temperature under the protective gas is 80-110° C. and the reaction time is 2-4 hours; wherein the protective gas is at least one of argon and nitrogen.

8. The preparation method according to claim 3, characterized in that: The tetrafunctional crosslinking agent and solvent are added to react, wherein the reaction temperature is 40-60° C. and the reaction time is 24-48 hours.

9. The preparation method according to claim 3, characterized in that: The molar ratio of the alcohol and the diisocyanate is (1-5): (1-3); the molar ratio of the prepolymer and the tetrafunctional crosslinking agent is (1-9): (1-6).

10. Use of the polymer according to claim 1 in the field of remodeling.

Citation Information

Patent Citations

  • Acylamino-urea-bond-based novel high-performance reversible covalent cross-linked polymer and preparation method thereof

    CN109265636A

  • Adaptable thermoset polymers with internal dynamic bonds, and methods of making and using the same

    US11713370B1

  • Methods for making recyclable and depolymerizable polymer network materials via thiourethane dynamic chemistry

    US20200407482A1