Piperazine phosphate-melamine phosphate copolymerized flame retardant, preparation method thereof and application of flame retardant in polyolefin material
Through the polymerization reaction of piperazine phosphate-melamine phosphate copolymer flame retardant, an intumescent flame retardant with carbon source, acid source and gas source is formed, which solves the safety problem of polyolefin materials when burning and the ease of traditional flame retardants. Eliminates the precipitation problem and achieves efficient V-0 flame retardant performance and environmentally friendly polyolefin material preparation.
Patent Information
- Application Number
- CN202411113287.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-08
AI Technical Summary
Existing polyolefin materials easily release a large amount of heat, smoke and toxic gases when burning, and traditional flame retardants such as halogen flame retardants are toxic. The large amount of hydroxide flame retardant added affects the material performance. Intumescent flame retardants The agent needs to be compounded, and it is easy to precipitate, causing flame retardant failure.
Develop a piperazine phosphate-melamine phosphate copolymer flame retardant. Through the polymerization reaction of piperazine diphosphate and melamine phosphate, an intumescent flame retardant with carbon source, acid source and gas source is formed, solving the traditional flame retardant problem. The problem of easy precipitation and hydrolysis of the agent is eliminated, the preparation method is simple, and it is suitable for polyolefin materials.
This copolymerized flame retardant has hydrolysis resistance and low precipitation properties. It can maintain V-0 flame retardant properties after boiling for 168 hours without affecting the material surface, providing an environmentally friendly flame retardant solution.
Smart Images

Figure CN118745249A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardant preparation, and relates to a piperazine phosphate-melamine phosphate copolymer flame retardant and a preparation method thereof and application thereof in polyolefin materials. Background Art
[0002] Polyolefins have the characteristics of low relative density, good chemical and water resistance, good mechanical strength and electrical insulation. They can be used for films, pipes, plates, various molded products, wires and cables, etc. They are widely used in agriculture, packaging, electronics, electrical, automobiles, machinery, daily necessities, etc. The chemical structure of polyolefins is mainly composed of carbon and hydrogen elements. This structure makes polyolefins easy to burn when encountering a fire source, and a large amount of heat, smoke and toxic gases may be released during the combustion process, posing a threat to people's lives and property safety, and also seriously restricting the application field of polyolefins. Therefore, improving the flame retardant properties of polyolefins has become a necessary way to expand their application.
[0003] Common flame retardants for polyolefins include halogen flame retardants, phosphorus-nitrogen intumescent flame retardants, and hydroxide flame retardants. Halogen flame retardants release toxic gases when burned, causing serious harm to humans and the environment when a fire occurs, while the high addition of hydroxide flame retardants has a great impact on the physical and mechanical properties of the material, which seriously restricts its application field. Intumescent flame retardants do not contain halogens, have excellent flame retardant properties, and produce low smoke, low toxicity, and no corrosive gases, which is in line with the research and development direction of flame retardants in the future. Intumescent flame retardants require the use of a variety of phosphorus-nitrogen flame retardants in combination, including ammonium polyphosphate (APP), triazine system, piperazine pyrophosphate, melamine polyphosphate system, ammonium polyphosphate (APP), pentaerythritol (PER), melamine (MEL) system, etc. APP is easy to precipitate and decompose, resulting in frost on the product surface and flame retardant failure.
[0004] Intumescent flame retardants require a combination of multiple phosphorus and nitrogen flame retardants, and existing technologies rarely use a single flame retardant. Therefore, it is necessary to develop a new intumescent flame retardant that has acid source, gas source and carbon source functions and is resistant to hydrolysis, thereby providing a new idea for the preparation of environmentally friendly flame-retardant polyolefins. Summary of the invention
[0005] In view of this, one of the objects of the present invention is to provide a piperazine phosphate-melamine phosphate copolymer flame retardant; the second object of the present invention is to provide a method for preparing the piperazine phosphate-melamine phosphate copolymer flame retardant; the third object of the present invention is to provide an application of the piperazine phosphate-melamine phosphate copolymer flame retardant in the preparation of polyolefin materials.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] 1. A method for preparing a piperazine phosphate-melamine phosphate copolymer flame retardant, the preparation method comprising the following steps:
[0008] The piperazine diphosphate and melamine phosphate are ground into powder and then mixed evenly, placed in an oven for polymerization reaction, and ground after cooling to obtain the piperazine phosphate-melamine phosphate copolymer flame retardant.
[0009] Preferably, the molar ratio of piperazine diphosphate to melamine phosphate is 1.2 to 2.0:1;
[0010] The polymerization temperature of the polymerization reaction is 250-270°C.
[0011] Further preferably, the molar ratio of piperazine diphosphate to melamine phosphate is 1.5:1;
[0012] The polymerization temperature of the polymerization reaction is 260°C.
[0013] Preferably, the polymerization time of the polymerization reaction is 1 to 3 hours;
[0014] The polymerization time of the polymerization reaction is 2 h.
[0015] 2. The piperazine phosphate-melamine phosphate copolymer flame retardant prepared according to the above preparation method.
[0016] 3. Application of the piperazine phosphate-melamine phosphate copolymer flame retardant in the preparation of flame-retardant polyolefin materials.
[0017] 4. Flame-retardant polyolefin material, which comprises the following components in parts by weight: 70 to 77 parts of polyolefin, 23 to 30 parts of the piperazine phosphate-melamine phosphate copolymer flame retardant according to claim 5, 0.5 to 0.8 parts of antioxidant, and 0.3 to 0.5 parts of processing lubricant.
[0018] Preferably, the polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber;
[0019] The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076;
[0020] The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
[0021] 5. A method for preparing the flame-retardant polyolefin material, which is as follows: polyolefin, the piperazine phosphate-melamine phosphate copolymer flame retardant, antioxidant and processing lubricant are uniformly mixed and placed in an extruder, and the flame-retardant polyolefin material is obtained by melting, blending, extruding, drawing, pelletizing and drying.
[0022] Preferably, the temperature of each section of the extruder from the main feeding port to the die head is: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C;
[0023] The rotation speed of the extruder is 300-350 r / min.
[0024] The beneficial effects of the present invention are as follows: the present invention provides a piperazine phosphate-melamine phosphate copolymer flame retardant, the structural formula of the copolymer flame retardant contains both a piperazine phosphate structure and a melamine phosphate structure, and is mainly obtained by polymerization of piperazine diphosphate and melamine phosphate, forming an intumescent flame retardant having a carbon source, an acid source, and a gas source, and solving the problems of easy precipitation and easy hydrolysis of traditional ammonium polyphosphate. The piperazine phosphate-melamine phosphate copolymer flame retardant of the present invention has the performance of hydrolysis resistance and low precipitation, and the preparation method is simple and easy to operate, and can be applied to the preparation of polyolefin materials. The flame retardant performance of the prepared polyolefin material still remains at V-0 level after boiling in water for 168 hours, and there is no precipitation on the surface.
[0025] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. DETAILED DESCRIPTION
[0026] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the experimental methods provided in the following examples are the basic concepts of the present invention, and the following examples and features in the examples can be combined with each other without conflict. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0028] Figure 1 The infrared spectrum analysis results of the piperazine phosphate-melamine phosphate copolymer flame retardant, piperazine diphosphate and melamine phosphate prepared in Example 1;
[0029] Figure 2 The results of nuclear magnetic resonance phosphorus spectrum analysis of the piperazine phosphate-melamine phosphate copolymer flame retardant prepared in Example 1.
[0030] Examples 1 to 7
[0031] A piperazine phosphate-melamine phosphate copolymer flame retardant, the specific preparation method is as follows:
[0032] Piperazine diphosphate and melamine phosphate (the molar numbers of piperazine diphosphate and melamine phosphate in each embodiment are as shown in Table 1) are ground into powder and mixed evenly, placed in an oven for polymerization reaction (the temperature and time of the polymerization reaction in each embodiment are as shown in Table 1), and then ground after cooling to obtain a piperazine phosphate-melamine phosphate copolymer flame retardant.
[0033] Table 1 Molar ratio of reaction materials and polymerization conditions in Examples 1 to 7 and Comparative Examples 1 to 6
[0034]
[0035]
[0036] Comparative Examples 1 to 6
[0037] A piperazine phosphate-melamine phosphate copolymer flame retardant, the specific preparation method is as follows:
[0038] Piperazine diphosphate and melamine phosphate (the molar numbers of piperazine diphosphate and melamine phosphate in each comparative example are as shown in Table 1) are ground into powder and mixed evenly, placed in an oven for polymerization reaction (the temperature and time of the polymerization reaction in each comparative example are as shown in Table 1), and then ground after cooling to obtain a piperazine phosphate-melamine phosphate copolymer flame retardant.
[0039] Embodiments 8 to 16
[0040] A flame retardant polyolefin material, the specific preparation method is as follows:
[0041] Polyolefin (HDPE 5000S, melt index 3g / 10min, Daqing Petrochemical), piperazine phosphate-melamine phosphate copolymer flame retardant, antioxidant (anti-1076) and processing lubricant (silicone wax, grade E525) are mixed (the number of different reaction materials added in each embodiment is as shown in Table 2) and evenly placed in an extruder (wherein the temperatures of each section of the extruder from the main feed port to the die head in each embodiment are: 180°C, 190°C, 200°C, 200°C, 210°C, 210°C, 200°C, 200°C, 200°C, and the speed of the extruder is 350r / min), and the flame retardant polyolefin material can be obtained by melting, blending, extruding, drawing, pelletizing and drying.
[0042] Table 2 Number of reactants of flame retardant polyolefin materials in Examples 8 to 16 and Comparative Examples 7 to 11
[0043]
[0044]
[0045] Example 17 to Example 22
[0046] A flame retardant polyolefin material, the specific preparation method is as follows:
[0047] 750 parts of polyolefin (the specific polyolefin type in each embodiment is shown in Table 3), 250 parts of piperazine phosphate-melamine phosphate copolymer flame retardant (using the piperazine phosphate-melamine phosphate copolymer flame retardant prepared in Example 1), 6.0 parts of antioxidant (the specific polyolefin type in each embodiment is shown in Table 3) and 4.0 parts of processing lubricant (the specific polyolefin type in each embodiment is shown in Table 3) are mixed evenly and placed in an extruder (the parameters and speed of the extruder in each embodiment are respectively shown in Table 3), and a flame-retardant polyolefin material can be obtained by melting, blending, extruding, pulling, pelletizing and drying.
[0048] Table 3 Different reaction materials in the preparation of flame retardant polyolefin materials in Examples 17 to 22
[0049]
[0050]
[0051] Performance Testing
[0052] The piperazine phosphate-melamine phosphate copolymer flame retardant, piperazine diphosphate and melamine phosphate prepared in Example 1 were subjected to infrared spectroscopy analysis, and the results are as follows: Figure 1 As shown. Figure 1It can be seen from the infrared spectrum analysis results that the infrared spectrum peak of the piperazine phosphate-melamine phosphate copolymer flame retardant prepared in Example 1 is obviously different from that of melamine phosphate and piperazine diphosphate. -1 The peak is the characteristic peak of the stretching vibration absorption of POP, indicating that a polycondensation reaction occurred during the preparation process of Example 1, proving that a product with a structure of piperazine phosphate-melamine phosphate copolymer flame retardant was prepared in Example 1.
[0053] The piperazine phosphate-melamine phosphate copolymer flame retardant prepared in Example 1 was subjected to nuclear magnetic resonance phosphorus spectrum analysis, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the NMR phosphorus spectrum of the piperazine phosphate-melamine phosphate copolymer flame retardant prepared in Example 1 simultaneously shows a free phosphorus peak with a chemical shift of -0.47, a terminal phosphorus peak with a chemical shift of -10.45, and an intermediate phosphorus peak with a chemical shift of -23.67. The presence of the terminal and intermediate phosphorus peaks indicates that the piperazine phosphate-melamine phosphate copolymer flame retardant structure is indeed present in the product prepared by the preparation method of Example 1.
[0054] Similarly, the piperazine phosphate-melamine phosphate copolymer flame retardant prepared in the other embodiments above was subjected to infrared spectrum and nuclear magnetic resonance phosphorus spectrum analysis, and the results were basically the same as those in the above embodiment 1, which shows that the preparation method of the present invention can indeed prepare piperazine phosphate-melamine phosphate copolymer flame retardant. The piperazine phosphate-melamine phosphate copolymer flame retardant of the present invention contains both piperazine phosphate structure and melamine phosphate structure, and the following situations may exist during the polymerization process: (1) the piperazine phosphate structure and the melamine phosphate structure are randomly copolymerized; (2) the piperazine phosphate structure and the melamine phosphate structure are alternately copolymerized; (3) the piperazine phosphate structure and the melamine phosphate structure are block copolymerized.
[0055] In order to verify the performance and polymerization process of the piperazine phosphate-melamine phosphate copolymer flame retardant prepared by the present invention, the yield, TG (1% thermal weight loss) and flame retardant color tests were performed on the corresponding flame retardants prepared in Examples 1 to 7 and Comparative Examples 1 to 6. The test results are shown in Table 4. The specific test method is as follows:
[0056] (1) Yield test: the total weight of the mixture of piperazine diphosphate and melamine phosphate before high-temperature polymerization is m1, the weight of the piperazine phosphate-melamine phosphate copolymer flame retardant after high-temperature polymerization is m2, and the flame retardant yield = m1÷m2*100%;
[0057] (2) TG (1% thermal weight loss): carried out in accordance with the latest standard of ASTM E2550;
[0058] (3) Flame retardant color: judged by the eyes as white, gray, or black.
[0059] Table 4 Comparison of yield, TG (1% thermal weight loss), and color performance of the flame retardants prepared in Examples 1 to 7 and Comparative Examples 1 to 6
[0060] Flame retardants Flame retardant yield% TG (1% thermal weight loss)℃ Flame retardant color Example 1 75.53 284.13 White Example 2 91.69 284.92 White Example 3 91.07 283.18 White Example 4 91.98 283.97 White Example 5 91.07 284.21 Light Gray Example 6 91.88 283.87 White Example 7 91.12 284.24 Light Gray Comparative Example 1 92.05 281.39 White Comparative Example 2 90.89 284.22 black Comparative Example 3 92.11 282.85 White Comparative Example 4 91.57 284.31 black Comparative Example 5 90.32 283.94 White Comparative Example 6 92.01 284.35 White
[0061] As can be seen from Table 4, the polymerization temperature and time in the polymerization reaction have a crucial influence on the performance of the prepared piperazine phosphate-melamine phosphate copolymer flame retardant, as shown below: When the polymerization temperature is 250-270°C and the polymerization time is 1-3h, the yield, TG (1% thermal weight loss) and color performance of the piperazine phosphate-melamine phosphate copolymer flame retardant are optimal. By comparing Example 1, Examples 4-7 and Comparative Examples 1-4, it can be found that when the polymerization temperature exceeds 270°C or the polymerization time exceeds 3h, the color of the prepared copolymer flame retardant turns black, indicating that the polymerization temperature is too high and the polymerization time is too long, resulting in carbonization of the copolymer flame retardant; when the polymerization temperature is lower than 250°C or the polymerization time is less than 1h, the yield of the prepared copolymer flame retardant is too large, and the TG (1% thermal weight loss) temperature is low, indicating that the polymerization temperature is too low and the polymerization time is too short, resulting in incomplete polymerization of the copolymer flame retardant.
[0062] In order to verify the performance of the flame-retardant polyolefin material obtained by using the piperazine phosphate-melamine phosphate copolymer flame retardant prepared by the present invention to prepare the flame-retardant polyolefin material, the flame-retardant properties, the flame-retardant properties after boiling and the precipitates on the surface of the sample strips of the corresponding flame-retardant polyolefin materials prepared in Examples 8 to 16, Examples 17 to 22 and Comparative Examples 7 to 11 were tested. The test results are shown in Table 5. The specific test method is as follows:
[0063] (1) Flame retardant properties: According to the latest UL94 standard, the corresponding polyolefin materials in Examples 8 to 16 and Comparative Examples 7 to 11 were placed in an oven and dried at 100° C. for 3 h, and then each material was injection molded into UL94 standard specimens using an injection molding machine;
[0064] (2) Boiling test: carried out in accordance with the latest UL746C standard, with a boiling temperature of 85°C and a boiling time of 168 hours;
[0065] (3) Spline surface precipitate test: The spline surface is judged visually.
[0066] Table 5 Comparison of flame retardancy, flame retardancy after boiling and surface precipitates of the flame retardant polyolefin materials prepared in Examples 8 to 16 and Comparative Examples 7 to 11
[0067] performance Flame retardant properties Flame retardant performance after boiling Sedimentation of the specimen after boiling Example 8 V-0 V-0 No precipitates on the surface of the spline Example 9 V-0 V-0 No precipitates on the surface of the spline Example 10 V-0 V-0 No precipitates on the surface of the spline Embodiment 11 V-0 V-0 No precipitates on the surface of the spline Example 12 V-0 V-0 No precipitates on the surface of the spline Embodiment 13 V-0 V-0 No precipitates on the surface of the spline Embodiment 14 V-0 V-0 No precipitates on the surface of the spline Embodiment 15 V-0 V-0 No precipitates on the surface of the spline Example 16 V-0 V-0 No precipitates on the surface of the spline Comparative Example 7 Not flame retardant Not flame retardant No precipitates on the surface of the spline Comparative Example 8 Not flame retardant Not flame retardant No precipitates on the surface of the spline Comparative Example 9 V-0 Flame retardant failure There are precipitates on the surface of the spline Comparative Example 10 V-0 Flame retardant failure There are precipitates on the surface of the spline Comparative Example 11 V-0 Flame retardant failure There are precipitates on the surface of the spline Embodiment 17 V-0 V-0 No precipitates on the surface of the spline Embodiment 18 V-0 V-0 No precipitates on the surface of the spline Embodiment 19 V-0 V-0 No precipitates on the surface of the spline Embodiment 20 V-0 V-0 No precipitates on the surface of the spline Embodiment 21 V-0 V-0 No precipitates on the surface of the spline Embodiment 22 V-0 V-0 No precipitates on the surface of the spline
[0068] As can be seen from Tables 4 and 5, the piperazine phosphate-melamine phosphate copolymer flame retardant of the present invention is applied to the preparation of flame-retardant polyolefin materials. The molar ratio of piperazine diphosphate and melamine phosphate used in the preparation process of piperazine phosphate-melamine phosphate copolymer flame retardant has a crucial influence on the flame retardant properties of the flame-retardant polyolefin material finally prepared, which is specifically manifested as follows: piperazine phosphate is used as a carbon source and an acid source in the copolymer flame retardant, and melamine phosphate is used as a gas source and an acid source. By comparing Examples 1 to 3, Examples 8 to 10 and Comparative Examples 5 to 8, it can be found that when the molar ratio of piperazine diphosphate to melamine phosphate is too much piperazine diphosphate (Comparative Example 5), it leads to too much carbon source and too little gas source, and when the piperazine diphosphate is too little (Comparative Example 6), it leads to too little carbon source, and too much gas source, all of which affect the flame retardant efficiency of the copolymer flame retardant. When applied to polyolefin materials, the flame retardant polyolefin material obtained is not flame retardant (Comparative Examples 7 to 8). Therefore, the ratio of piperazine diphosphate and melamine phosphate affects the proportion of carbon source, gas source and acid source in the copolymer. Only a suitable ratio can achieve the optimal flame retardant efficiency. When applied to polyolefin materials, the materials can reach V-0 flame retardancy.
[0069] At the same time, by comparing Examples 8 to 16 and Comparative Examples 9 to 11, it can be found that when the piperazine phosphate-melamine phosphate copolymer flame retardant is applied to flame-retardant polyolefin materials (polypropylene, polyethylene, vinyl elastomer), the flame retardant performance of the polyolefin material reaches V-0 level, and the material remains flame retardant at V-0 level after boiling, and there is no precipitate on the surface of the spline; while using the ammonium polyphosphate (APP) system flame retardant, the flame retardant performance of the polyolefin material reaches V-0 level, but the flame retardant of the material fails after boiling, is not flame retardant, and there are precipitates on the surface of the spline.
[0070] In addition, from the performance of the flame-retardant polyolefin materials prepared from different types of materials in Examples 17 to 22, it can be seen that in the process of preparing the flame-retardant polyolefin materials, after adding the piperazine phosphate-melamine phosphate copolymer flame retardant prepared by the present invention, any one or more of polyethylene, polypropylene, polybutene, vinyl elastomer, propylene-based elastomer or EPDM rubber in the remaining materials can be used as polyolefin, any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076 can be used as antioxidants, and any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate can be used as processing lubricants. The prepared flame-retardant polyolefin materials all have V-0 grade flame retardancy, are still V-0 grade flame retardant after boiling in water, and the flame retardant does not precipitate.
[0071] In summary, the present invention provides a piperazine phosphate-melamine phosphate copolymer flame retardant, the structural formula of the copolymer flame retardant contains both a piperazine phosphate structure and a melamine phosphate structure, and is mainly obtained by the polymerization reaction of piperazine diphosphate and melamine phosphate, forming an intumescent flame retardant having a carbon source, an acid source, and a gas source, and solves the problems of easy precipitation and easy hydrolysis of traditional ammonium polyphosphate. The piperazine phosphate-melamine phosphate copolymer flame retardant of the present invention has the performance of hydrolysis resistance and low precipitation, and the preparation method is simple and easy to operate, and can be applied to the preparation of polyolefin materials. The flame retardant performance of the prepared polyolefin material still remains V-0 level after boiling in water for 168 hours, and there is no precipitate on the surface.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a piperazine phosphate-melamine phosphate copolymer flame retardant, characterized in that: The preparation method comprises the following steps: The piperazine diphosphate and melamine phosphate are ground into powder and then mixed evenly, placed in an oven for polymerization reaction, and ground after cooling to obtain the piperazine phosphate-melamine phosphate copolymer flame retardant.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the piperazine diphosphate to melamine phosphate is 1.2 to 2.0:1; The polymerization temperature of the polymerization reaction is 250-270°C.
3. The preparation method according to claim 2, characterized in that: The molar ratio of piperazine diphosphate to melamine phosphate is 1.5:1; The polymerization temperature of the polymerization reaction is 260°C.
4. The preparation method according to claim 1, characterized in that: The polymerization time of the polymerization reaction is 1 to 3 hours; The polymerization time of the polymerization reaction is 2 h.
5. The piperazine phosphate-melamine phosphate copolymer flame retardant prepared according to the preparation method according to any one of claims 1 to 4.
6. Use of the piperazine phosphate-melamine phosphate copolymer flame retardant according to claim 5 in the preparation of flame-retardant polyolefin materials.
7. Flame retardant polyolefin material, characterized in that: In terms of weight parts, the flame retardant polyolefin material comprises the following components: 70-77 parts of polyolefin, 23-30 parts of the piperazine phosphate-melamine phosphate copolymer flame retardant according to claim 5, 0.5-0.8 parts of antioxidant, and 0.3-0.5 parts of processing lubricant.
8. The flame retardant polyolefin material according to claim 7, characterized in that: The polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber; The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076; The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
9. The method for preparing the flame retardant polyolefin material according to any one of claims 7 to 8, characterized in that: The preparation method is as follows: polyolefin, the piperazine phosphate-melamine phosphate copolymer flame retardant according to claim 5, an antioxidant and a processing lubricant are uniformly mixed and placed in an extruder, and the flame-retardant polyolefin material can be obtained by melting, blending, extruding, drawing, pelletizing and drying.
10. The preparation method according to claim 9, characterized in that: The temperatures of the extruder from the main feed port to the die are: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C; The rotation speed of the extruder is 300-350 r / min.
Citation Information
Cited By
Environment-friendly flame-retardant plastic as well as preparation method and application thereof