Polymer catalyst for efficiently catalyzing hydrogenation of alpha, beta-unsaturated carbonyl derivative to prepare alpha, beta-unsaturated alcohol in water phase as well as preparation method and application of polymer catalyst
By developing an efficient polymer catalyst in the aqueous phase, the balance problem between conversion rate and selectivity in the catalytic hydrogenation reaction of α,β-unsaturated carbonyl derivatives was solved, and the catalyst was recyclable, overcoming the The reaction liquid in the prior art is difficult to separate.
Patent Information
- Application Number
- CN202410729381.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
It is difficult for existing catalysts to achieve a balance between conversion rate and selectivity when catalyzing the hydrogenation reaction of α,β-unsaturated carbonyl derivatives, and it is difficult to directly separate from the reaction solution after the reaction and cannot be recycled.
Develop a polymer catalyst that efficiently catalyzes the hydrogenation of α,β-unsaturated carbonyl derivatives in the aqueous phase. Its structure includes stable metal complexes, combined with ligands through covalent bonds or coordination bonds, and adopts specific synthesis methods. Prepared by a method, it can show high activity under mild conditions and is easy to separate and recover.
It achieves highly selective catalytic production of α,β-unsaturated alcohols under mild conditions, and the catalyst can be directly separated and reused after the reaction, solving the problem of difficulty in separating the reaction liquid.
Smart Images

Figure CN118745252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic catalysts, and in particular to a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to prepare α,β-unsaturated alcohols in an aqueous phase, and a preparation method and application thereof. Background Art
[0002] Biomass is the only renewable carbon-based resource in nature, and it has the advantages of abundant sources and low cost. Converting biomass into fine chemicals and fuels has important practical significance for meeting the needs of economic and social development and alleviating the shortage of fossil resources. With the development and utilization of biomass resources, carbonyl derivatives such as α,β-unsaturated aldehydes made from biomass are widely used in the preparation of high value-added fine chemical intermediates or products.
[0003] For example, cinnamaldehyde, which is commonly found in plants such as cinnamon, contains conjugated C=C and C=O double bonds in its structure and is a typical α,β-unsaturated aldehyde. Cinnamyl alcohol is the product of carbonyl hydrogenation of cinnamaldehyde and is widely used in the synthesis of flavors, fragrances, cosmetics, medicines, and fungicides. However, from a thermodynamic point of view, the bond energy of C=C in the cinnamaldehyde structure (615KJ·mol -1 ) is relatively C=O bond energy (715KJ·mol -1 ) is low, which makes it difficult to selectively catalyze the hydrogenation of C=O without destroying C=C. Therefore, most catalysts are difficult to achieve a good balance between conversion rate and cinnamyl alcohol selectivity in the catalytic hydrogenation reaction of cinnamaldehyde.
[0004] At present, there are mainly chemical methods and catalytic hydrogenation methods for reducing α,β-unsaturated aldehydes (ketones). The chemical method uses a metered amount of reducing reagents such as sodium borohydride to react with α,β-unsaturated aldehydes (ketones), and the main product is α,β-unsaturated alcohols. However, due to the high price of reducing agents and the complex post-reaction treatment process, this method is only suitable for small-scale laboratory use. In contrast, the catalytic hydrogenation method has the advantages of high efficiency and green environmental protection. However, the catalytic hydrogenation of α,β-unsaturated aldehydes (ketones) can produce a variety of products such as saturated aldehydes (ketones), unsaturated alcohols, and saturated alcohols, which is relatively complicated. It is crucial to develop a catalyst that can highly selectively catalyze the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols.
[0005] Since the new century, the research and development of hydrogenation catalysts has made significant progress. At present, hydrogenation catalysts mainly include two categories: supported metal catalysts and homogeneous metal complex catalysts. Supported metal catalysts often require relatively harsh reaction conditions, which makes it difficult for the catalytic system to obtain α, β-unsaturated alcohol products with high selectivity in the hydrogenation reaction of α, β-unsaturated carbonyl derivatives. It is well known that homogeneous metal complex catalysts have clear structural characteristics and often show excellent catalytic activity under mild conditions. They have inherent advantages in catalyzing the hydrogenation of α, β-unsaturated aldehydes (ketones) to α, β-unsaturated alcohols. So far, researchers have developed a series of homogeneous metal complex catalysts that can effectively catalyze the highly selective hydrogenation of α, β-unsaturated carbonyl derivatives to α, β-unsaturated alcohols. However, it has been reported that metal complexes mostly require organic solvents such as isopropanol and tetrahydrofuran as reaction media (existing literature, Chem. Eur. J. 2017, 23, 8473-8481, J. Catal. 2023, 417, 109-115, CN 202211418869), and it is difficult to separate directly from the reaction solution after the reaction and cannot be recycled. Therefore, it is urgent to develop a new catalyst system that has the characteristics of high reaction activity and good selectivity of homogeneous metal complex catalysts and easy separation, recovery and reuse of supported catalysts. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present invention is to provide a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase, and a preparation method and application thereof, which solves the problems of being difficult to directly separate from the reaction liquid after the reaction and being unable to be recycled.
[0007] According to the present invention, a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase has the following structural formula:
[0008]
[0009] Wherein, M is selected from one of Ru, Os, Rh, Ir, Mn, Fe or Co;
[0010] D1, D2, D3, and D4 are donor atoms coordinated to the metal center, each independently selected from N and P;
[0011] R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from hydrogen, a linear or branched C1-C 10 Alkyl, C3-C 10 Cycloalkyl, C4-C 24 Aryl or heteroaryl, R9, R 10Each independently selected from: hydrogen, a straight chain or branched C1-C 10 Alkyl, C3-C 10 Cycloalkyl, C4-C 24 Aryl or heteroaryl, R9 and R 10 Can be connected to form C3-C 10 Cycloalkyl, C4-C 24 aryl or heteroaryl;
[0012] X is selected from one of CO, halogen anion, hydride anion, borohydride ion, hydroxide ion, sulfonate ion, nitrile ion or sulfonitrile ion;
[0013] The coupling group between the complexes is selected from C1-C 10 Alkylene or C3-C 10 Cycloalkylene;
[0014] k, m, and n are each independently selected from integers between 0 and 3.
[0015] In some embodiments of the present invention, the M and the D1, D2, D3, D4 ligands are combined in the form of covalent bonds or coordination bonds, and this interaction can exist in the solid state or in solution.
[0016] A method for preparing a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to prepare α,β-unsaturated alcohols in an aqueous phase, comprising the following two raw materials of molecular structure formula:
[0017]
[0018] The specific steps are as follows:
[0019] S1: In the absence of oxygen and water, in the range of room temperature to reflux temperature, the ligand L1 and the metal precursor containing MXn are sealed and heated to 40-150°C in an organic solvent at a ratio of 1:0.5-1, and the heating is maintained for 2-100 hours, and the intermediate i is obtained through reduced pressure concentration, filtration, weak polar solvent washing, and vacuum drying;
[0020] S2: In the absence of oxygen and water, in the range of room temperature to reflux temperature, the ligand L2 and the intermediate i obtained in step S1 are sealed and heated to 40-150° C. in an organic solvent at a ratio of 1:0.5-5, and the heating is maintained for 2-100 hours, and a metal complex is obtained by concentrating under reduced pressure, filtering, washing with a weak polar solvent, and vacuum drying.
[0021] S3: Under the condition of no water and no oxygen, weigh the metal complex obtained in step S2, the metal halide and the dihalide according to the molar ratio of 1:10-30:100-10000, add 2-100 ml of solvent and place in a 200 ml Schlenk bottle; under an inert atmosphere, react the reaction solution in the temperature range of 0-100° C. by programmed temperature control for 48-96 hours to obtain a final reaction solution;
[0022] S4: Add 30-60 mL of aqueous hydrochloric acid to the final reaction solution obtained in step S3, stir for 0.5-2 hours, filter and collect the solid product, wash it with ethanol, water, and ethanol in sequence, and dry it under reduced pressure to obtain a polymer catalyst.
[0023] In other embodiments of the present invention, the organic solvent is selected from toluene, tetrahydrofuran, 1,4-dioxane or diethyl ether;
[0024] The weakly polar solvent is selected from one of n-hexane, n-heptane or cyclohexane;
[0025] The metal halide is selected from one of AlCl3, FeCl3 or ZnCl2;
[0026] The dihalide is selected from chain C1-C 10 Dihalogen compounds or cyclic C3-C 10 Dihalogen compounds;
[0027] The anhydrous solvent is selected from carbon disulfide, nitrobenzene or petroleum ether.
[0028] The invention discloses an application of the polymer catalyst which can efficiently catalyze the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in a water phase to the application of the polymer catalyst which can efficiently catalyze the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in a water phase.
[0029] In other embodiments of the present invention, the α,β-unsaturated carbonyl derivative is an α,β-unsaturated aldehyde or an α,β-unsaturated ketone.
[0030] In other embodiments of the present invention, the steps of efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase are as follows: under a hydrogen atmosphere, the initial hydrogen pressure is in the range of 1-70 bar, at a temperature of room temperature to 110°C, a polymer catalyst and an α,β-unsaturated carbonyl derivative are added to a solvent in a mass ratio of 1:100-100000 to react, the reaction time is 0.1-200 hours, and an α,β-unsaturated alcohol as a hydrogenation reaction product is obtained.
[0031] In some other embodiments of the present invention, the operation steps of the reactor are as follows:
[0032] S1: In an inert atmosphere glove box, weigh the polymer catalyst, base, and α,β-unsaturated carbonyl derivative into a high-pressure reactor, assemble the reactor body, and transfer it out of the glove box;
[0033] S2: After cooling the kettle to 0-10°C with ice water, add 2-200 ml of solvent under N2 protection, replace the gas in the kettle with hydrogen and then fill it with hydrogen;
[0034] S3: placing the kettle body in a heating device for heating and reaction;
[0035] S4: After the reaction is completed, the temperature of the kettle is quickly reduced to 0-10°C, and the remaining hydrogen in the kettle is discharged. The reaction liquid is filtered through a silica gel short column to obtain the hydrogenation reaction product α, β-unsaturated alcohol.
[0036] In other embodiments of the present invention, the solvent is one of water, methanol, ethanol, n-propanol, isopropanol, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, toluene or acetonitrile; the base is one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, cesium carbonate, sodium bicarbonate, potassium bicarbonate, sodium alkoxide or potassium alkoxide.
[0037] In the present invention, the active center of this type of catalyst is a metal complex stabilized by phosphine ligands and amine ligands. This type of catalyst has the advantages of mild reaction conditions and high activity of homogeneous metal complex catalysts in the catalytic hydrogenation reaction, and easy separation, recovery and reuse of heterogeneous catalysts after the reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0039] Figure 1 The results of recycling the polymer catalyst 1c in Example 9 and Example 23 to Example 27 of the present invention to catalyze the hydrogenation of cinnamaldehyde to cinnamyl alcohol in water solvent DETAILED DESCRIPTION
[0040] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0041] The present invention proposes a metal complex-based polymer catalyst whose active center is stabilized by phosphine ligands and amine ligands, and the structural formula is shown in the figure below:
[0042]
[0043] Two kinds of raw materials with molecular structure:
[0044]
[0045] In the present invention, the synthesis of the polymer catalyst is completed under anhydrous and oxygen-free conditions using standard Schlenk operation techniques, and the method is as follows:
[0046] (1) In the temperature range of 40-150°C, the ligand L1 and the metal precursor are reacted in an organic solvent at a ratio of 1:0.5-1 for 2-100 hours. After the reaction is completed, the intermediate i is obtained by vacuum concentration, adding a weak polar solvent to precipitate a solid, filtering and collecting the precipitate, washing the precipitate with a weak polar solvent, and vacuum drying. In this synthesis method, the organic solvent can be selected from toluene, xylene, tetrahydrofuran, 1,4-dioxane, 2-methyltetrahydrofuran, ethanol, n-propanol, isopropanol, etc., and the weak polar solvent can be selected from n-hexane, cyclohexane, n-heptane, etc.
[0047] (2) In the temperature range of 40-150° C., the ligand L2 and the intermediate i obtained in step (1) are reacted in an organic solvent at a ratio of 1:0.5-5 for 2-100 hours. After the reaction is completed, the metal complex is obtained by concentrating under reduced pressure, adding a weak polar solvent to precipitate a solid, filtering and collecting the precipitate, washing with a weak polar solvent, and drying under reduced pressure. In this synthesis method, the organic solvent can be selected from toluene, xylene, tetrahydrofuran, 1,4-dioxane, 2-methyltetrahydrofuran, ethanol, n-propanol, isopropanol, etc., and the weak polar solvent can be selected from n-hexane, cyclohexane, n-heptane, etc.
[0048] (3) In the temperature range of 0-100°C, the metal complex obtained in step (2) is reacted with a metal halide and a dihalide in a molar ratio of 1:10-30:100-10000 in an anhydrous solvent by a programmed temperature control method for 48-96 hours. After the reaction is completed, 30-60 mL of a hydrochloric acid aqueous solution (v / v=1:1) is added, stirred for 0.5-2 hours, and the solid is collected by filtration, washed with ethanol and water in turn, and dried under reduced pressure. In this synthesis method, the metal halide can be selected from AlCl3, FeCl3, ZnCl2, and the dihalide can be selected from a chain C1-C 10 Dihalogen compounds, cyclic C3-C 10 Dihalogen compounds and anhydrous solvents may be carbon disulfide, nitrobenzene, petroleum ether, etc.
[0049] The activity evaluation of the above polymer catalyst for catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to α,β-unsaturated alcohols is carried out in a high-pressure reactor with magnetic stirring or mechanical stirring. The operation method is as follows:
[0050] In the temperature range of room temperature to 110° C., the initial hydrogen pressure is 1-70 bar, the mass ratio of the polymer catalyst to the α,β-unsaturated carbonyl derivative molecules is 1:100-100000 (the ratio is adjustable), and the reaction is carried out in a solvent for 0.1-200 hours to obtain a carbonyl selective hydrogenation product; the solvent is selected from water, methanol, ethanol, n-propanol, isopropanol, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, toluene, acetonitrile, etc., preferably water and isopropanol; a certain amount of base needs to be added in the reaction, such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, cesium carbonate, sodium bicarbonate, potassium bicarbonate, sodium alkoxide, potassium alkoxide, etc., preferably sodium hydroxide and sodium alkoxide; the substrate conversion rate and product yield are detected and analyzed by a gas chromatograph equipped with a hydrogen ion flame detector or a liquid nuclear magnetic hydrogen spectrum.
[0051] Embodiment 1:
[0052] Preparation of polymer catalyst 1a:
[0053] Step (1): Under an inert atmosphere, 1.92 g of RuCl2(DMSO)4 (4.0 mmol) and 1.16 g of o-PPh2C6H4NHMe (4.0 mmol) were weighed into a Schlenk bottle (200 mL) containing about 60 mL of tetrahydrofuran, and the bottle was sealed and heated to 60° C. After reacting for 2 days, the reaction solution was cooled to room temperature, filtered and collected, and the brick-red precipitate was washed with n-hexane, dried under reduced pressure, and weighed to 1.61 g (yield 64%), to obtain the intermediate ia(o-Ph2PC6H4NHMe)RuCl2(DMSO)2;
[0054] Step (2): Under an inert atmosphere, 0.95 g (1.5 mmol) of the intermediate ia obtained in step (1) and 0.12 g NH2(CH2)2NH2 (2.0 mmol) were placed in a Schlenk bottle (200 mL) containing about 50 mL of 1,4-dioxane, and the mixture was sealed and heated to 110° C. After six days of reaction, the generated off-white solid precipitate was collected by filtration and washed with n-hexane, dried under reduced pressure, and weighed 0.72 g (yield 90%) to obtain the complex iaa (o-Ph2PC6H4NHMe) [(CH2NH2)2]RuCl2;
[0055] Step (3): Under an inert atmosphere, weigh 0.51 g (1.0 mmol) of the complex iaa obtained in step (2) and 2.67 g of AlCl3 (20.0 mmol) into a Schlenk bottle (200 mL) containing 38 mL of CH2Cl2 (600 mmol) and 30 mL of carbon disulfide. Under stirring conditions, react at 0°C for 4 hours, 20°C for 8 hours, 40°C for 12 hours, 60°C for 24 hours, and 80°C for 48 hours. After the reaction is completed, add 40 mL of hydrochloric acid aqueous solution (v / v=1:1) to the reaction solution, stir for 1 hour, filter and collect the solid, wash with ethanol (50 mL×3), water (50 mL×3), and ethanol (50 mL×3) in sequence, and dry under reduced pressure. The weight is 0.62 g to obtain polymer catalyst 1a.
[0056] 31 P NMR (162MHz, in solid, 298k, ppm): δ = 66.41 (br).
[0057]
[0058] Embodiment 2:
[0059] Preparation of polymer catalyst 1b:
[0060] Step (1): Under an inert atmosphere, 0.95 g of the intermediate ia (1.5 mmol) obtained in step (1) of Example 1 and 176.7 mg (CH2NHMe)2 (2.0 mmol) were weighed into a Schlenk bottle (200 mL) containing about 60 mL of toluene, and the mixture was sealed and heated to 70°C. After four days of reaction, the mixture was cooled to room temperature, the reaction solution was concentrated under reduced pressure to about 5 mL, and then 5 mL of n-hexane was added. The precipitate was collected by filtration, dried under reduced pressure, and weighed to 0.455 g (yield 55%) to obtain complex iab;
[0061] Step (2): Under an inert atmosphere, weigh 0.55 g (1.0 mmol) of the complex iab obtained in step (1) and 2.67 g of AlCl3 (20.0 mmol) into a Schlenk bottle (200 mL) containing 38 mL of CH2Cl2 (600 mmol) and 30 mL of carbon disulfide. Under stirring conditions, react at 0°C for 4 hours, 20°C for 8 hours, 40°C for 12 hours, 60°C for 24 hours, and 80°C for 48 hours. After the reaction is completed, add 40 mL of hydrochloric acid aqueous solution (v / v=1:1) to the reaction solution, stir for 1 hour, filter and collect the solid, wash with ethanol (50 mL×3), water (50 mL×3), and ethanol (50 mL×3) in sequence, and dry under reduced pressure. The weight is 0.64 g to obtain polymer catalyst 1b.
[0062] 31 P NMR (162MHz, in solid, 298k, ppm): δ = 63.41 (br).
[0063]
[0064] Embodiment 4:
[0065] Preparation of polymer catalyst 2a:
[0066] Step (1): Under an inert atmosphere, weigh 1.16 g of RuCl2(PPh3)3 (1.2 mmol) and 0.36 go-Ph2PC6H4NMe2 (1.2 mmol) into a Schlenk bottle (100 mL) containing about 40 mL of toluene, and heat to 100°C in a sealed container. After reacting overnight, cool to room temperature, concentrate the reaction solution to about 3 mL under reduced pressure, add 5 mL of n-hexane, collect the precipitated green precipitate by filtration, dry under reduced pressure, and weigh 0.82 g (yield 92%) to obtain the intermediate ib(o-Ph2PC6H4NMe2)RuCl2(PPh3);
[0067] Step (2): Under an inert atmosphere, 0.60 g of the intermediate ib (0.8 mmol) obtained in step (1) and 186.0 mg (CH2NHEt)2 (1.6 mmol) were weighed into a Schlenk bottle (200 mL) containing about 60 mL of 1,4-dioxane, and the mixture was sealed and heated to 100°C. After two days of reaction, the mixture was cooled to room temperature, the reaction solution was concentrated under reduced pressure to about 5 mL, and then 5 mL of n-heptane was added. The precipitate was collected by filtration, dried under reduced pressure, and weighed to 0.36 g (yield 76%) to obtain the complex iba;
[0068] Step (3): Under an inert atmosphere, weigh 0.59 g (1.0 mmol) of the complex iba obtained in step (2) and 2.67 g AlCl3 (20.0 mmol) into a Schlenk bottle (200 mL) containing 38 mL CH2Cl2 (600 mmol) and 30 mL carbon disulfide. Under stirring conditions, react at 0°C for 4 hours, 20°C for 8 hours, 40°C for 12 hours, 60°C for 24 hours, and 80°C for 48 hours. After the reaction is completed, add 40 mL of hydrochloric acid aqueous solution (v / v=1:1) to the reaction solution, stir for 1 hour, filter and collect the solid, wash with ethanol (50 mL×3), water (50 mL×3), and ethanol (50 mL×3) in sequence, and dry under reduced pressure. The weight is 0.68 g to obtain polymer catalyst 2a.
[0069] 31P NMR (162MHz, in solid, 298k, ppm): δ = 64.32 (br).
[0070]
[0071] Example 5 to Example 22 are methods for selectively hydrogenating cinnamaldehyde molecules to produce cinnamyl alcohol using complex catalysts 1a-1c and 2a.
[0072] Example 5:
[0073] In an argon atmosphere glove box, polymer catalyst 1a (5.0 mg), sodium methoxide (50.0 mg), cinnamaldehyde (1.0 g, cinnamaldehyde and sodium methoxide, catalyst mass ratio is 200:10:1), isopropanol (4 mL) were weighed into a 25 mL reactor with a magnetic stirring device, and the reactor was assembled and transferred out of the glove box. Subsequently, the reactor was cooled to about 5 ° C with ice water, and the atmosphere in the reactor was replaced with hydrogen (1 bar) 3 times and then filled with hydrogen to 10 bar. The reactor was placed in a heating device and heated to 40 ° C and maintained at this temperature for 1 h. After the reaction was completed, the reactor was quickly cooled to about 5 ° C and the remaining hydrogen in the reactor was discharged. After the reaction liquid was filtered with a silica gel short column, it was analyzed by gas chromatography with a hydrogen ion flame detector (chromatographic column model HB-Wax, specification 30m×0.32mm×0.33μm), the conversion rate of cinnamaldehyde was 43%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 43%.
[0074] Embodiment six:
[0075] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1b (5.0 mg), the conversion rate of cinnamaldehyde was 76%, and the yield of cinnamyl alcohol, the hydrogenation product, was 75%.
[0076] Embodiment seven:
[0077] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the conversion rate of cinnamaldehyde was 99%, and the yield of cinnamyl alcohol, the hydrogenation product, was 98%.
[0078] Embodiment eight:
[0079] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 2a (5.0 mg), the conversion rate of cinnamaldehyde was 16%, and the yield of cinnamyl alcohol, the hydrogenation product, was 16%.
[0080] Table 1 Comprehensive results of hydrogenation of cinnamaldehyde to cinnamyl alcohol catalyzed by polymer catalysts of Examples 5 to 8
[0081]
[0082]
[0083] Embodiment nine:
[0084] The same experimental steps as in Example 5 were used, except that the polymer catalyst was changed to 1c (5.0 mg), the base was changed to sodium hydroxide (37.0 mg), and the solvent was changed to water (4 mL). The conversion rate of cinnamaldehyde was 98%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 97%.
[0085] Embodiment ten:
[0086] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to n-propanol (4 mL), the conversion rate of cinnamaldehyde was 97%, and the yield of cinnamyl alcohol, the hydrogenation product, was 95%.
[0087] Embodiment eleven:
[0088] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to ethanol (4 mL), the conversion rate of cinnamaldehyde was 70%, and the yield of cinnamyl alcohol, the hydrogenation product, was 67%.
[0089] Embodiment 12:
[0090] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to methanol (4 mL), the conversion rate of cinnamaldehyde was 95%, and the yield of cinnamyl alcohol, the hydrogenation product, was 94%.
[0091] Embodiment 13:
[0092] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to 1,4-dioxane (4 mL), the conversion rate of cinnamaldehyde was 73%, and the yield of cinnamyl alcohol, the hydrogenation product, was 72%.
[0093] Embodiment 14:
[0094] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to tetrahydrofuran (4 mL), the conversion rate of cinnamaldehyde was 61%, and the yield of cinnamyl alcohol, the hydrogenation product, was 61%.
[0095] Embodiment 15:
[0096] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to toluene (4 mL), the conversion rate of cinnamaldehyde was 7%, and the yield of cinnamyl alcohol, the hydrogenation product, was 7%.
[0097] Embodiment 16:
[0098] The experimental steps were the same as those in Example 5, except that the polymer catalyst was changed to 1c (5.0 mg), the solvent was changed to acetonitrile (4 mL), the conversion rate of cinnamaldehyde was 2%, and the yield of cinnamyl alcohol, the hydrogenation product, was 2%.
[0099] Table 2. Comprehensive results of cinnamaldehyde hydrogenation to cinnamyl alcohol catalyzed by polymer catalyst 1c in different solvents in Examples 9 to 16
[0100]
[0101] Embodiment 17:
[0102] The same experimental steps as in Example 9 were used, except that the reaction temperature was lowered to room temperature (25° C.), the reaction time was extended to 3 h, the conversion rate of cinnamaldehyde was 95%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 94%.
[0103] Embodiment 18:
[0104] The same experimental steps as in Example 9 were used, except that the hydrogen pressure was reduced to 1 bar, the reaction time was extended to 2 h, the conversion rate of cinnamaldehyde was 97%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 95%.
[0105] Embodiment 19:
[0106] The same experimental steps as in Example 9 were used, except that the hydrogen pressure was reduced to 1 bar, the reaction temperature was reduced to room temperature (25° C.), the reaction time was extended to 6 h, the cinnamaldehyde conversion rate was 92%, and the yield of the hydrogenation reaction product, cinnamyl alcohol, was 91%.
[0107] Embodiment 20:
[0108] The same experimental steps as in Example 9 were used, except that the amount of cinnamaldehyde was increased to 2.0 g (the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of cinnamaldehyde was 96%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 94%.
[0109] Embodiment 21:
[0110] The same experimental steps as in Example 9 were used, except that a 50 mL magnetic stirring reactor was used, the amount of sodium hydroxide was increased to 74.0 mg, the amount of cinnamaldehyde was increased to 10.0 g (the mass ratio of substrate to sodium hydroxide and catalyst was 2000:14.8:1), the water volume was increased to 10 mL, the hydrogen pressure was increased to 30 bar, the reaction temperature was increased to 60 ° C, the reaction time was extended to 4 h, the cinnamaldehyde conversion rate was 99%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 97%.
[0111] Embodiment 22:
[0112] The same experimental steps as in Example 5 were used, except that a 250 mL mechanically stirred reactor was used, the amount of sodium hydroxide was increased to 370.0 mg, the amount of cinnamaldehyde was increased to 100.0 g (the mass ratio of substrate to sodium hydroxide and catalyst was 20000:74:1), the water volume was increased to 100 mL, the hydrogen pressure was increased to 70 bar, the reaction temperature was increased to 110 ° C, the reaction time was extended to 48 h, the cinnamaldehyde conversion was 98%, and the yield of hydrogenation reaction product cinnamyl alcohol was 95%.
[0113] Table 3. Comprehensive results of catalytic hydrogenation of cinnamaldehyde to cinnamyl alcohol by polymer catalyst 1c in Example 17 to Example 22 under different conditions in water solvent
[0114]
[0115] Example 23 to Example 27 are methods for reusing polymer catalyst 1c to catalyze the selective hydrogenation of cinnamaldehyde molecules to produce cinnamyl alcohol.
[0116] Embodiment 23:
[0117] The reaction solution obtained in Example 9 was centrifuged (2000 rpm, 3 molecules) to collect the solid matter. The same experimental steps as in Example 9, the catalyst was replaced with the solid matter obtained by centrifugation, the conversion rate of cinnamaldehyde was 98%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 96%.
[0118] Embodiment 24:
[0119] The reaction solution obtained in Example 23 was centrifuged (2000 rpm, 3 molecules) to collect the solid matter. The same experimental steps as in Example 9, the catalyst was replaced with the solid matter obtained by centrifugation, the conversion rate of cinnamaldehyde was 97%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 95%.
[0120] Embodiment 25:
[0121] The reaction solution obtained in Example 24 was centrifuged (2000 rpm, 3 molecules) to collect the solid matter. The same experimental steps as in Example 9, the catalyst was replaced with the solid matter obtained by centrifugation, the conversion rate of cinnamaldehyde was 97%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 95%.
[0122] Embodiment 26:
[0123] The reaction solution obtained in Example 25 was centrifuged (2000 rpm, 3 molecules) to collect the solid matter. The same experimental steps as in Example 9, the catalyst was replaced with the solid matter obtained by centrifugation, the conversion rate of cinnamaldehyde was 96%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 95%.
[0124] Embodiment 27:
[0125] The reaction solution obtained in Example 26 was centrifuged (2000 rpm, 3 molecules) to collect the solid matter. The same experimental steps as in Example 9, the catalyst was replaced with the solid matter obtained by centrifugation, the conversion rate of cinnamaldehyde was 95%, and the yield of cinnamyl alcohol, the hydrogenation reaction product, was 94%.
[0126] From the experimental results in Tables 1 to 3, it can be seen that the polymer catalyst with a suitable precursor configuration invented in this patent can effectively catalyze the highly selective hydrogenation of cinnamaldehyde to cinnamyl alcohol in an aqueous phase under mild conditions. Figure 1 The results show that the polymer catalyst has excellent recycling performance. The above method effectively overcomes the defects of the current literature and patents that the reaction system for preparing α,β-unsaturated alcohol from α,β-unsaturated aldehyde is difficult to have both mild reaction conditions and water as the reaction medium.
[0127] Example 28 to Example 35 are methods for preparing unsaturated alcohols by selective hydrogenation of unsaturated aldehydes and ketones with different structures catalyzed by polymer catalyst 3c.
[0128] Embodiment 28:
[0129] The same experimental steps as in Example 9 were used, except that the substrate was changed to furfural (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the furfural conversion rate was 99%, and the yield of furfuryl alcohol, the hydrogenation reaction product, was 98%.
[0130] Embodiment 29:
[0131] The same experimental steps as in Example 9 were used, except that the substrate was changed to citral (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the reaction time was extended to 2 h, the citral conversion rate was 87%, and the yield of the hydrogenation reaction product geraniol was 86%.
[0132] Embodiment 30:
[0133] The experimental steps were the same as those in Example 9, except that the substrate was changed to crotonaldehyde (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of crotonaldehyde was 99%, and the yield of the hydrogenation reaction product 2-butenol was 98%.
[0134] Embodiment 31:
[0135] The same experimental steps as in Example 9 were used, except that the substrate was changed to 3-methyl-2-butenal (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of 3-methyl-2-butenal was 97%, and the yield of the hydrogenation reaction product 3-methyl-2-butene-1-ol was 97%.
[0136] Embodiment 32:
[0137] The same experimental steps as in Example 9 were used, except that the substrate was changed to 2-methylacrolein (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of 2-methylacrolein was 99%, and the yield of methylallyl alcohol, the hydrogenation product, was 97%.
[0138] Embodiment 33:
[0139] The same experimental steps as in Example 9 were used, except that the substrate was changed to 1-cyclohexene-1-carboxaldehyde (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of 1-cyclohexene-1-carboxaldehyde was 97%, and the yield of hydrogenation reaction product (cyclohexatriene-1-ene-1-yl) methanol was 95%.
[0140] Embodiment 34:
[0141] The same experimental steps as in Example 9 were used, except that the substrate was changed to 3-cyclohexene-1-carboxaldehyde (2.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 400:7.4:1), the conversion rate of 3-cyclohexene-1-carboxaldehyde was 96%, and the yield of the hydrogenation reaction product 3-cyclohexene-1-methanol was 95%.
[0142] Embodiment 35:
[0143] The same experimental steps as in Example 9 were used, except that the substrate was changed to benzylidene acetone (1.0 g, the mass ratio of substrate to sodium hydroxide and catalyst was 200:7.4:1), the conversion rate of benzylidene acetone was 99%, and the yield of the hydrogenation reaction product 4-phenyl-3-butene-2-ol was 97%.
[0144] Table 4. Comprehensive results of the hydrogenation of unsaturated aldehydes and ketones to unsaturated alcohols catalyzed by polymer catalyst 1c in Examples 28 to 35
[0145]
[0146] From the results in Table 4, it can be seen that under the implementation method, the polymer catalyst can effectively catalyze the highly selective hydrogenation of various α,β-unsaturated aldehydes (ketones) with different structures to produce α,β-unsaturated alcohols. In summary, it can be seen that under the implementation method, the reaction system has good substrate compatibility.
[0147] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to α,β-unsaturated alcohols in an aqueous phase. Features: Its structural formula is as follows: Wherein, M is selected from one of Ru, Os, Rh, Ir, Mn, Fe or Co; D 1 , D 2 , D 3 , D 4 are donor atoms coordinated to the metal center, each independently selected from N and P; R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 Each independently selected from hydrogen, a straight chain or branched chain C 1 -C 10 Alkyl, C 3 -C 10 Cycloalkyl, C 4 -C 24 Aryl or heteroaryl, R 9 , R 10 Each independently selected from: hydrogen, straight chain or branched chain C 1 -C 10 Alkyl, C 3 -C 10 Cycloalkyl, C 4 -C 24 Aryl or heteroaryl, R 9 and R 10 Can be connected to form C 3 -C 10 Cycloalkyl, C 4 -C 24 Aryl or heteroaryl; X is selected from one of CO, halogen anion, hydride anion, borohydride ion, hydroxide ion, sulfonate ion, nitrile ion or sulfonitrile ion; The coupling group between the complexes is selected from C 1 -C 10 Alkylene or C 3 -C 10 Cycloalkylene; k, m, and n are each independently selected from integers between 0 and 3.
2. A polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase according to claim 1, Features: The M and D 1 , D 2 , D 3 , D 4 The role of the ligand is to bind by covalent bond or coordination bond, and this role can exist in solid state or solution.
3. A method for preparing a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to α,β-unsaturated alcohols in an aqueous phase, Features: The raw materials include the following two molecular structures: The specific steps are as follows: S1: In the absence of oxygen and water, at room temperature-reflux temperature range, ligand L 1 The metal precursor containing MXn is sealed and heated to 40-150° C. in an organic solvent at a ratio of 1:0.5-1, and the heating is maintained for 2-100 hours, and the intermediate i is obtained through reduced pressure concentration, filtration, weak polar solvent washing, and vacuum drying. S2: In the absence of oxygen and water, in the range of room temperature to reflux temperature, the ligand L2 and the intermediate i obtained in step S1 are sealed and heated to 40-150° C. in an organic solvent at a ratio of 1:0.5-5, and the heating is maintained for 2-100 hours, and a metal complex is obtained by concentrating under reduced pressure, filtering, washing with a weak polar solvent, and vacuum drying. S3: Under the condition of no water and no oxygen, weigh the metal complex obtained in step S2, the metal halide and the dihalide according to the molar ratio of 1:10-30:100-10000, add 2-100 ml of solvent and place in a 200 ml Schlenk bottle; under an inert atmosphere, react the reaction solution in the temperature range of 0-100° C. by programmed temperature control for 48-96 hours to obtain a final reaction solution; S4: Add 30-60 mL of aqueous hydrochloric acid to the final reaction solution obtained in step S3, stir for 0.5-2 hours, filter and collect the solid product, wash it with ethanol, water, and ethanol in sequence, and dry it under reduced pressure to obtain a polymer catalyst.
4. A method for preparing a polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to α,β-unsaturated alcohols in an aqueous phase according to claim 3, Features: The organic solvent is selected from toluene, tetrahydrofuran, 1,4-dioxane or diethyl ether; The weakly polar solvent is selected from one of n-hexane, n-heptane or cyclohexane; The metal halide is selected from AlCl 3 、FeCl 3 or ZnCl 2 One of the following; The dihalide is selected from chain C 1 -C 10 Dihalogen compounds or cyclic C 3 -C 10 Dihalogen compounds; The anhydrous solvent is selected from carbon disulfide, nitrobenzene or petroleum ether.
5. Use of the polymer catalyst for efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase as described in any one of claims 1 or 2 in efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase.
6. The use according to claim 5, Features: The α,β-unsaturated carbonyl derivative is an α,β-unsaturated aldehyde or an α,β-unsaturated ketone.
7. The use according to claim 5, Features: The steps of efficiently catalyzing the hydrogenation of α,β-unsaturated carbonyl derivatives to produce α,β-unsaturated alcohols in an aqueous phase are as follows: under a hydrogen atmosphere, with an initial hydrogen pressure in the range of 1-70 bar, at a temperature of room temperature to 110° C., a polymer catalyst and an α,β-unsaturated carbonyl derivative are added to a solvent in a mass ratio of 1:100-100000 to react for a reaction time of 0.1-200 hours to obtain a hydrogenation reaction product, α,β-unsaturated alcohol.
8. The use according to claim 7, Features: The operation steps of the reactor are as follows: S1: In an inert atmosphere glove box, weigh the polymer catalyst, base, and α,β-unsaturated carbonyl derivative into a high-pressure reactor, assemble the reactor body, and transfer it out of the glove box; S2: Cool the kettle to 0-10°C with ice water and heat it under N 2 Add 2-200 ml of solvent under gas protection, replace the gas in the kettle with hydrogen and then fill it with hydrogen; S3: placing the kettle body in a heating device for heating and reaction; S4: After the reaction is completed, the temperature of the kettle is quickly reduced to 0-10°C, and the remaining hydrogen in the kettle is discharged. The reaction liquid is filtered through a silica gel short column to obtain the hydrogenation reaction product α, β-unsaturated alcohol.
9. The use according to claim 8, Features: The solvent is one of water, methanol, ethanol, n-propanol, isopropanol, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, toluene or acetonitrile; the base is one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, cesium carbonate, sodium bicarbonate, potassium bicarbonate, sodium alcoholate or potassium alcoholate.