Plastic packaging film and preparation method thereof

Through the composite material of graphene, modified resin and modified filler, the problem of insufficient mechanical strength and barrier performance of polyethylene plastic packaging film is solved, the preparation of high-performance plastic packaging film is realized, and the mechanical performance and barrier effect are improved.

CN118745261AActive Publication Date: 2024-10-08DONGGUAN YONGFEI IND CO LTD

Patent Information

Application Number
CN202411060814.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-08
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Polyethylene plastic packaging film has low mechanical strength and poor barrier properties, making it difficult to meet the needs of sealed packaging.

Method used

A composite material of graphene, modified resin and modified filler is used. The reinforced resin and modified filler are prepared through specific chemical reactions and processing methods, and then combined with dicumyl peroxide for melt blending to form a high-performance plastic packaging film. .

Benefits of technology

The mechanical properties and barrier effect of the plastic packaging film are significantly improved, allowing it to achieve good physical performance indicators while reducing the thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a plastic packaging film and a preparation method thereof. The plastic packaging film comprises the following raw materials in parts by weight: 80-100 parts of polyethylene master batch, 30-50 parts of reinforced resin and 0.5-2 parts of dicumyl peroxide. In the melt blending process of the raw materials, reinforced resin is grafted with polyethylene molecular chains under the action of dicumyl peroxide, then chain molecules are converted into dendritic molecules, graphene and montmorillonite are of a two-dimensional layered structure, the barrier effect of the plastic packaging film can be greatly improved by compounding with modified resin, meanwhile, a core-shell structure is formed with the modified resin, and the barrier effect of the plastic packaging film is greatly improved. A polyhedral oligomeric silsesquioxane structure is embedded between the modified graphene and the modified filler, so that the mechanical property of the plastic packaging film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic packaging film preparation, and in particular to a plastic packaging film and a preparation method thereof. Background Art

[0002] Polyethylene film is widely used in general moisture-proof packaging of food, medicine, daily necessities and metal products and packaging of frozen food due to its good water resistance, moisture resistance, drought resistance, chemical stability, hot viscosity and heat sealing performance. Due to the fast crystallization rate and high crystallinity of polyethylene, it is currently mainly produced by blow molding or cast film process, but the mechanical properties of polyethylene film produced by these two processes are poor, and the thickness of the film needs to be increased to meet the application requirements. Biaxially oriented polyethylene film is made of linear low-density polyethylene, which is stretched longitudinally and then transversely. Compared with polyethylene film produced by blow molding or cast film process, it has great improvements in physical properties, with high transparency, good heat sealing and moisture resistance, good longitudinal and transverse tensile strength, and foldability. Even when the thickness is reduced by 50%, its key performance can still reach good indicators. However, the barrier property of polyethylene film to gas is poor, and it is still difficult to meet the needs of sealed packaging. Summary of the invention

[0003] The object of the present invention is to provide a plastic packaging film and a preparation method thereof, which solves the problem that the mechanical strength of the polyethylene plastic packaging film at present is low and the barrier property is poor.

[0004] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a plastic packaging film comprises the following steps: The graphene is dispersed in ethanol, stirred and KH550 and deionized water are added at a speed of 150-200 r / min and a temperature of 40-50°C, and the reaction is carried out for 3-5 hours to obtain modified graphene. The modified resin, modified filler, modified graphene and DMF are evenly mixed, and the reaction is carried out for 4-6 hours at a speed of 120-150 r / min, a temperature of 20-25°C and a pH value of 10-11 to obtain a reinforced resin. The following raw materials are weighed in parts by weight: 80-100 parts of polyethylene masterbatch, 30-50 parts of reinforcing resin and 0.5-2 parts of diisopropylbenzene peroxide, the raw materials are melt-blended, and then blown into a film to obtain a plastic packaging film.

[0005] Furthermore, the amount of KH550 used is 5% of the mass of graphene, the mass ratio of modified resin, modified filler and modified graphene is 20:5:2, and the model of polyethylene masterbatch is HDPE6070.

[0006] Further, the modified resin is prepared by the following steps: Step A1: polyvinyl alcohol, p-nitrobenzaldehyde, p-toluenesulfonic acid and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 5-7 hours at a speed of 120-150 r / min and a temperature of 110-120°C to obtain pretreated polyvinyl alcohol; the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are mixed evenly, and the reaction is carried out for 1-1.5 hours at a speed of 120-150 r / min and a temperature of 90-95°C, and ammonia water is added to the pH value to 8 to obtain functionalized polyvinyl alcohol.

[0007] Step A2: functionalized polyvinyl alcohol, maleic anhydride and DMF are mixed evenly, reacted at a speed of 120-150r / min and a temperature of 55-60°C for 30-40min, triethylamine, acetic anhydride and nickel acetate are added, reacted for 2-3h to obtain modified polyvinyl alcohol, modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and DMF are mixed evenly, reacted at a speed of 120-150r / min and a temperature of 65-70°C for 2-3h, sodium hydroxide solution is added, the temperature is raised to 75-80°C, and the reaction is carried out for 3-5h to obtain a modified resin.

[0008] Furthermore, the dosage ratio of polyvinyl alcohol, p-nitrobenzaldehyde and p-toluenesulfonic acid described in step A1 is 10g:30mmol:1mmol, the mass fraction of polyvinyl alcohol is 2000, the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are 2g:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0009] Furthermore, the amount ratio of the amino group, maleic anhydride, triethylamine, acetic anhydride and nickel acetate on the functionalized polyvinyl alcohol described in step A2 is 10mmol:10mmol:4mL:10mL:2.5g, the amount ratio of modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 5g:1g:0.9g:20mL, and the mass fraction of the sodium hydroxide solution is 20%.

[0010] Further, the modified filler is prepared by the following steps: Step B1: KH570, sodium hydroxide, isopropanol and deionized water are mixed evenly, reacted at a speed of 120-150r / min and a temperature of 60-70°C for 3-5h, cooled to 20-25°C, reacted for 10-15h to obtain sodium tetrasiliconate, sodium tetrasiliconate, triethylamine and tetrahydrofuran are mixed evenly, nitrogen is introduced for protection, stirred and methyl dichloroethane is added at a speed of 200-300r / min and a temperature of 0°C, reacted for 3-5h, heated to 20-25°C, and continued to react for 20-25h to obtain dihydrogen cage-type silsesquioxane; Step B2: Dihydrogen cage silsesquioxane, 3-mercaptopropyltrimethoxysilane, benzophenone and DMF are mixed evenly, and reacted for 30-40 minutes at a speed of 150-200 r / min, a temperature of 20-25° C. and ultraviolet irradiation to obtain modified silsesquioxane; the modified silsesquioxane, allyl alcohol glycidyl ether, Custer catalyst and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 10-15 hours at a speed of 120-150 r / min and a temperature of 80-85° C. to obtain functionalized silsesquioxane; Step B3: Mix the functionalized silsesquioxane, DMF, ethanol and deionized water evenly, stir and add hydrochloric acid solution to a pH value of 2-5 at a speed of 150-200 r / min and a temperature of 25-30°C, stir for 20-30 minutes to obtain a modified solution, mix sodium montmorillonite, ethanol and deionized water evenly, stir and add the modified solution at a speed of 300-500 r / min and a temperature of 80-85°C, react for 7-9 hours to obtain modified montmorillonite.

[0011] Furthermore, the dosage ratio of KH570, sodium hydroxide, isopropanol and deionized water in step B1 is 20g:3g:100mL:5mL, and the mass ratio of sodium tetrasiliconate, triethylamine and methyldichloroethane is 11:4:3.

[0012] Furthermore, the molar ratio of the double bond on the dihydrogen cage-type silsesquioxane described in step B2 to 3-mercaptopropyltrimethoxysilane is 1:1, the amount of benzophenone used is 1% by mass of 3-mercaptopropyltrimethoxysilane, the molar ratio of Si-H on the modified silsesquioxane to allyl alcohol glycidyl ether is 1:1, and the amount of Custer catalyst used is 1.5‰ of the mass of allyl alcohol glycidyl ether.

[0013] Furthermore, the amount ratio of the functionalized silsesquioxane, DMF, ethanol and deionized water in step B3 is 2g:20mL:15mL:5mL, and the amount ratio of sodium montmorillonite, ethanol, deionized water and modified liquid is 1g:75mL:25mL:20mL.

[0014] Beneficial effects of the present invention: A plastic packaging film prepared by the present invention comprises the following raw materials: polyethylene masterbatch, reinforcing resin and diisopropylbenzene peroxide; the reinforcing resin is treated with KH550 using graphene as raw material so that amino groups are grafted on the surface to obtain modified graphene; the modified resin, modified filler and modified graphene are reacted so that the epoxy groups on the modified resin and the epoxy groups on the modified filler react with the amino groups on the surface of the modified graphene to obtain the reinforcing resin.

[0015] The modified resin uses polyvinyl alcohol and p-nitrobenzaldehyde as raw materials, undergoes acetal reaction under the action of p-toluenesulfonic acid, so that adjacent alcohol hydroxyl groups of polyvinyl alcohol react with aldehyde groups of p-nitrobenzaldehyde to obtain pretreated polyvinyl alcohol, reduces the pretreated polyvinyl alcohol with tin powder, converts the nitro groups of the side chains into amino groups to obtain functionalized polyvinyl alcohol, reacts the functionalized polyvinyl alcohol with maleic anhydride, so that the amino groups on the functionalized polyvinyl alcohol react with maleic anhydride and close the ring to obtain modified polyvinyl alcohol, reacts the modified polyvinyl alcohol with epichlorohydrin, so that the hydroxyl groups on the modified polyvinyl alcohol react with the epoxy groups on the epichlorohydrin, and then closes the ring under the action of sodium hydroxide solution to obtain the modified resin.

[0016] The modified filler is hydrolyzed and condensed with KH570 as a raw material to form a sodium tetrasilanol structure containing a double bond to obtain sodium tetrasilanol. The sodium tetrasilanol is reacted with methyl dichloroethane to make the sodium alcohol structure on the sodium tetrasilanol react with the chlorine atom site on the methyl dichloroethane to obtain dihydrogen cage silsesquioxane. The dihydrogen cage silsesquioxane and 3-mercaptopropyltrimethoxysilane are irradiated with ultraviolet light to make the mercapto group on the mercaptopropyltrimethoxysilane and the dihydrogen cage The double bond on the modified silsesquioxane is grafted to obtain a modified silsesquioxane, the modified silsesquioxane and allyl alcohol glycidyl ether are treated with a Custer catalyst to graft the Si-H bond on the modified silsesquioxane with the double bond on the allyl alcohol glycidyl ether to obtain a functionalized silsesquioxane, the functionalized silsesquioxane is hydrolyzed to form a silanol bond, and then the functionalized silsesquioxane is grafted with the active groups on the surface and between layers of montmorillonite, and then the functionalized silsesquioxane and montmorillonite are composited to obtain a modified filler.

[0017] During the melt blending process of the raw materials, the reinforcing resin is grafted with the polyethylene molecular chains under the action of diisopropylbenzene peroxide, thereby converting the chain molecules into branched molecules. Graphene and montmorillonite are two-dimensional layered structures. When compounded with the modified resin, they can greatly enhance the barrier effect of the plastic packaging film and form a core-shell structure with the modified resin. A cage-type silsesquioxane structure is embedded between the modified graphene and the modified filler, thereby enhancing the mechanical properties of the plastic packaging film. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0019] A method for preparing a plastic packaging film comprises the following steps: Graphene was dispersed in ethanol, stirred and KH550 and deionized water were added at a speed of 150 r / min and a temperature of 40°C, and the mixture was reacted for 3 hours to obtain modified graphene. The modified resin, modified filler, modified graphene and DMF were evenly mixed, and the mixture was reacted for 4 hours at a speed of 120 r / min, a temperature of 20°C and a pH value of 10 to obtain reinforced resin. The following raw materials were weighed in parts by weight: 80 parts of polyethylene masterbatch, 30 parts of reinforcing resin and 0.5 parts of diisopropylbenzene peroxide, the raw materials were melt-blended, and then blown into a film to obtain a plastic packaging film.

[0020] The amount of KH550 used is 5% of the mass of graphene, the mass ratio of modified resin, modified filler and modified graphene is 20:5:2, and the model of polyethylene masterbatch is HDPE6070.

[0021] The modified resin is prepared by the following steps: Step A1: Evenly mix polyvinyl alcohol, p-nitrobenzaldehyde, p-toluenesulfonic acid and toluene, introduce nitrogen protection, react for 5 hours at a speed of 120 r / min and a temperature of 110°C to obtain pretreated polyvinyl alcohol; evenly mix the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid, react for 1 hour at a speed of 120 r / min and a temperature of 90°C, add ammonia water to a pH value of 8, and obtain functionalized polyvinyl alcohol.

[0022] Step A2: functionalized polyvinyl alcohol, maleic anhydride and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 55°C for 30 minutes, triethylamine, acetic anhydride and nickel acetate are added, and reacted for 2 hours to obtain modified polyvinyl alcohol; modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 65°C for 2 hours, sodium hydroxide solution is added, the temperature is raised to 75°C, and the reaction is carried out for 3 hours to obtain a modified resin.

[0023] The amount ratio of polyvinyl alcohol, p-nitrobenzaldehyde and p-toluenesulfonic acid described in step A1 is 10g:30mmol:1mmol, the mass fraction of polyvinyl alcohol is 2000, the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are 2g:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0024] The amount ratio of amino group, maleic anhydride, triethylamine, acetic anhydride and nickel acetate on the functionalized polyvinyl alcohol described in step A2 is 10mmol:10mmol:4mL:10mL:2.5g, the amount ratio of modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 5g:1g:0.9g:20mL, and the mass fraction of sodium hydroxide solution is 20%.

[0025] The modified filler is prepared by the following steps: Step B1: KH570, sodium hydroxide, isopropanol and deionized water are mixed evenly, reacted at a speed of 120 r / min and a temperature of 60°C for 3 hours, cooled to 20°C, reacted for 10 hours to obtain sodium tetrasiliconate, sodium tetrasiliconate, triethylamine and tetrahydrofuran are mixed evenly, nitrogen is introduced for protection, stirred and methyl dichloroethane is added at a speed of 200 r / min and a temperature of 0°C, reacted for 3 hours, heated to 20°C, and continued to react for 20 hours to obtain dihydrogen cage-type silsesquioxane; Step B2: Dihydrogen cage silsesquioxane, 3-mercaptopropyltrimethoxysilane, benzophenone and DMF are mixed evenly, and reacted for 30 minutes at a speed of 150 r / min, a temperature of 20° C. and ultraviolet light irradiation to obtain modified silsesquioxane; modified silsesquioxane, allyl alcohol glycidyl ether, Custer catalyst and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 10 hours at a speed of 120 r / min and a temperature of 80° C. to obtain functionalized silsesquioxane; Step B3: Mix the functionalized silsesquioxane, DMF, ethanol and deionized water evenly, stir and add hydrochloric acid solution to a pH value of 2 at a speed of 150 r / min and a temperature of 25°C, stir for 20 minutes to obtain a modified solution, mix sodium montmorillonite, ethanol and deionized water evenly, stir and add the modified solution at a speed of 300 r / min and a temperature of 80°C, react for 7 hours to obtain modified montmorillonite.

[0026] The amount ratio of KH570, sodium hydroxide, isopropanol and deionized water in step B1 is 20g:3g:100mL:5mL, and the mass ratio of sodium tetrasiliconate, triethylamine and methyl dichloroethane is 11:4:3.

[0027] The molar ratio of the double bond on the dihydrogen cage silsesquioxane described in step B2 to 3-mercaptopropyltrimethoxysilane is 1:1, the amount of benzophenone used is 1% by mass of 3-mercaptopropyltrimethoxysilane, the molar ratio of Si-H on the modified silsesquioxane to allyl alcohol glycidyl ether is 1:1, and the amount of Custer catalyst used is 1.5‰ of the mass of allyl alcohol glycidyl ether.

[0028] The amount ratio of the functionalized silsesquioxane, DMF, ethanol and deionized water described in step B3 is 2g:20mL:15mL:5mL, and the amount ratio of sodium montmorillonite, ethanol, deionized water and modified liquid is 1g:75mL:25mL:20mL. Example

[0029] A method for preparing a plastic packaging film comprises the following steps: Graphene was dispersed in ethanol, stirred and KH550 and deionized water were added at a speed of 150 r / min and a temperature of 45°C, and the reaction was carried out for 4 hours to obtain modified graphene. The modified resin, modified filler, modified graphene and DMF were evenly mixed, and the reaction was carried out for 5 hours at a speed of 120 r / min, a temperature of 25°C and a pH value of 10 to obtain a reinforced resin. The following raw materials were weighed in parts by weight: 90 parts of polyethylene masterbatch, 40 parts of reinforcing resin and 1.2 parts of diisopropylbenzene peroxide, the raw materials were melt-blended, and then blown into a film to obtain a plastic packaging film.

[0030] The amount of KH550 used is 5% of the mass of graphene, the mass ratio of modified resin, modified filler and modified graphene is 20:5:2, and the model of polyethylene masterbatch is HDPE6070.

[0031] The modified resin is prepared by the following steps: Step A1: Evenly mix polyvinyl alcohol, p-nitrobenzaldehyde, p-toluenesulfonic acid and toluene, introduce nitrogen protection, react for 6 hours at a speed of 120 r / min and a temperature of 115°C to obtain pretreated polyvinyl alcohol; evenly mix the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid, react for 1.3 hours at a speed of 120 r / min and a temperature of 95°C, add ammonia water to a pH value of 8, and obtain functionalized polyvinyl alcohol.

[0032] Step A2: functionalized polyvinyl alcohol, maleic anhydride and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 58°C for 35 minutes, triethylamine, acetic anhydride and nickel acetate are added, and reacted for 3 hours to obtain modified polyvinyl alcohol; modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and DMF are mixed evenly, reacted at a speed of 120 r / min and a temperature of 68°C for 3 hours, and then sodium hydroxide solution is added, the temperature is raised to 78°C, and the reaction is carried out for 4 hours to obtain a modified resin.

[0033] The amount ratio of polyvinyl alcohol, p-nitrobenzaldehyde and p-toluenesulfonic acid described in step A1 is 10g:30mmol:1mmol, the mass fraction of polyvinyl alcohol is 2000, the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are 2g:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0034] The amount ratio of amino group, maleic anhydride, triethylamine, acetic anhydride and nickel acetate on the functionalized polyvinyl alcohol described in step A2 is 10mmol:10mmol:4mL:10mL:2.5g, the amount ratio of modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 5g:1g:0.9g:20mL, and the mass fraction of sodium hydroxide solution is 20%.

[0035] The modified filler is prepared by the following steps: Step B1: KH570, sodium hydroxide, isopropanol and deionized water are mixed evenly, reacted at a speed of 120 r / min and a temperature of 65°C for 4 hours, cooled to 25°C, reacted for 10 hours to obtain sodium tetrasiliconate, sodium tetrasiliconate, triethylamine and tetrahydrofuran are mixed evenly, nitrogen is introduced for protection, stirred at a speed of 300 r / min and a temperature of 0°C, methyl dichloroethane is added, reacted for 4 hours, heated to 25°C, and reacted for 20 hours to obtain dihydrogen cage-type silsesquioxane; Step B2: Dihydrogen cage silsesquioxane, 3-mercaptopropyltrimethoxysilane, benzophenone and DMF were mixed evenly, and reacted for 35 minutes at a speed of 200 r / min, a temperature of 20° C. and ultraviolet light irradiation to obtain modified silsesquioxane; modified silsesquioxane, allyl alcohol glycidyl ether, Custer catalyst and toluene were mixed evenly, nitrogen was introduced for protection, and the reaction was carried out for 15 hours at a speed of 150 r / min and a temperature of 80° C. to obtain functionalized silsesquioxane; Step B3: Mix the functionalized silsesquioxane, DMF, ethanol and deionized water evenly, stir and add hydrochloric acid solution to pH 5 at a speed of 150 r / min and a temperature of 28°C, stir for 25 minutes to obtain a modified solution, mix sodium montmorillonite, ethanol and deionized water evenly, stir and add the modified solution at a speed of 500 r / min and a temperature of 80°C, react for 8 hours to obtain modified montmorillonite.

[0036] The amount ratio of KH570, sodium hydroxide, isopropanol and deionized water in step B1 is 20g:3g:100mL:5mL, and the mass ratio of sodium tetrasiliconate, triethylamine and methyl dichloroethane is 11:4:3.

[0037] The molar ratio of the double bond on the dihydrogen cage silsesquioxane described in step B2 to 3-mercaptopropyltrimethoxysilane is 1:1, the amount of benzophenone used is 1% by mass of 3-mercaptopropyltrimethoxysilane, the molar ratio of Si-H on the modified silsesquioxane to allyl alcohol glycidyl ether is 1:1, and the amount of Custer catalyst used is 1.5‰ of the mass of allyl alcohol glycidyl ether.

[0038] The amount ratio of the functionalized silsesquioxane, DMF, ethanol and deionized water described in step B3 is 2g:20mL:15mL:5mL, and the amount ratio of sodium montmorillonite, ethanol, deionized water and modified liquid is 1g:75mL:25mL:20mL. Example

[0039] A method for preparing a plastic packaging film comprises the following steps: Graphene was dispersed in ethanol, stirred and KH550 and deionized water were added at a speed of 200 r / min and a temperature of 50°C, and the reaction was carried out for 5 hours to obtain modified graphene. The modified resin, modified filler, modified graphene and DMF were evenly mixed, and the reaction was carried out for 6 hours at a speed of 150 r / min, a temperature of 25°C and a pH value of 11 to obtain a reinforced resin. The following raw materials were weighed in parts by weight: 100 parts of polyethylene masterbatch, 50 parts of reinforcing resin and 2 parts of diisopropylbenzene peroxide, the raw materials were melt-blended, and then blown into a film to obtain a plastic packaging film.

[0040] The amount of KH550 used is 5% of the mass of graphene, the mass ratio of modified resin, modified filler and modified graphene is 20:5:2, and the model of polyethylene masterbatch is HDPE6070.

[0041] The modified resin is prepared by the following steps: Step A1: Evenly mix polyvinyl alcohol, p-nitrobenzaldehyde, p-toluenesulfonic acid and toluene, introduce nitrogen protection, react for 7 hours at a speed of 150 r / min and a temperature of 120°C to obtain pretreated polyvinyl alcohol; evenly mix the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid, react for 1.5 hours at a speed of 150 r / min and a temperature of 95°C, add ammonia water to a pH value of 8, and obtain functionalized polyvinyl alcohol.

[0042] Step A2: functionalized polyvinyl alcohol, maleic anhydride and DMF are mixed evenly, reacted at a speed of 150 r / min and a temperature of 60°C for 40 minutes, triethylamine, acetic anhydride and nickel acetate are added, and reacted for 3 hours to obtain modified polyvinyl alcohol; modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and DMF are mixed evenly, reacted at a speed of 150 r / min and a temperature of 70°C for 3 hours, and then sodium hydroxide solution is added, the temperature is raised to 80°C, and the reaction is carried out for 5 hours to obtain a modified resin.

[0043] The amount ratio of polyvinyl alcohol, p-nitrobenzaldehyde and p-toluenesulfonic acid described in step A1 is 10g:30mmol:1mmol, the mass fraction of polyvinyl alcohol is 2000, the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are 2g:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0044] The amount ratio of amino group, maleic anhydride, triethylamine, acetic anhydride and nickel acetate on the functionalized polyvinyl alcohol described in step A2 is 10mmol:10mmol:4mL:10mL:2.5g, the amount ratio of modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 5g:1g:0.9g:20mL, and the mass fraction of sodium hydroxide solution is 20%.

[0045] The modified filler is prepared by the following steps: Step B1: KH570, sodium hydroxide, isopropanol and deionized water are mixed evenly, reacted at a speed of 150 r / min and a temperature of 70°C for 5 hours, cooled to 25°C, reacted for 15 hours to obtain sodium tetrasiliconate, sodium tetrasiliconate, triethylamine and tetrahydrofuran are mixed evenly, nitrogen is introduced for protection, stirred and methyl dichloroethane is added at a speed of 300 r / min and a temperature of 0°C, reacted for 5 hours, heated to 25°C, and continued to react for 25 hours to obtain dihydrogen cage-type silsesquioxane; Step B2: Dihydrogen cage silsesquioxane, 3-mercaptopropyltrimethoxysilane, benzophenone and DMF are mixed evenly, and reacted for 40 minutes at a speed of 200 r / min, a temperature of 25° C. and ultraviolet light irradiation to obtain modified silsesquioxane; modified silsesquioxane, allyl alcohol glycidyl ether, Custer catalyst and toluene are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 15 hours at a speed of 150 r / min and a temperature of 85° C. to obtain functionalized silsesquioxane; Step B3: Mix the functionalized silsesquioxane, DMF, ethanol and deionized water evenly, stir and add hydrochloric acid solution to a pH value of 2 at a speed of 150 r / min and a temperature of 25°C, stir for 20 minutes to obtain a modified solution, mix sodium montmorillonite, ethanol and deionized water evenly, stir and add the modified solution at a speed of 300 r / min and a temperature of 80°C, react for 7 hours to obtain modified montmorillonite.

[0046] The amount ratio of KH570, sodium hydroxide, isopropanol and deionized water in step B1 is 20g:3g:100mL:5mL, and the mass ratio of sodium tetrasiliconate, triethylamine and methyl dichloroethane is 11:4:3.

[0047] The molar ratio of the double bond on the dihydrogen cage silsesquioxane described in step B2 to 3-mercaptopropyltrimethoxysilane is 1:1, the amount of benzophenone used is 1% by mass of 3-mercaptopropyltrimethoxysilane, the molar ratio of Si-H on the modified silsesquioxane to allyl alcohol glycidyl ether is 1:1, and the amount of Custer catalyst used is 1.5‰ of the mass of allyl alcohol glycidyl ether.

[0048] The amount ratio of the functionalized silsesquioxane, DMF, ethanol and deionized water described in step B3 is 2g:20mL:15mL:5mL, and the amount ratio of sodium montmorillonite, ethanol, deionized water and modified liquid is 1g:75mL:25mL:20mL.

[0049] Comparative Example 1 Compared with Example 1, this comparative example uses ethylenediamine instead of modified graphene, and the remaining steps are the same.

[0050] Comparative Example 2 Compared with Example 1, no modified resin was added in this comparative example, and the remaining steps were the same.

[0051] Comparative Example 3 Compared with Example 1, this comparative example uses modified polyvinyl alcohol instead of modified resin, and the remaining steps are the same.

[0052] Comparative Example 4 Compared with Example 1, this comparative example uses graphene instead of the modified filler, and the remaining steps are the same.

[0053] Comparative Example 5 Compared with Example 1, this comparative example uses KH560 instead of functionalized silsesquioxane, and the remaining steps are the same.

[0054] The plastic films prepared in Examples 1-3 and Comparative Examples 1-5 were made into samples with a thickness of 0.05 mm. The longitudinal tensile strength and transverse tensile strength of the samples were tested in accordance with GB / T6672-2001, and the puncture resistance was tested in accordance with the standard of GB / T9639.1-2008. The dart mass was 80 g. The barrier effect was tested in accordance with the standard of GB / T1037-2021. The test results are shown in the following table.

[0055]

[0056] It can be seen from the above table that the present application has good barrier effect and mechanical properties.

[0057] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a plastic packaging film, characterized in that: The specific steps include: The graphene is dispersed in ethanol, stirred and KH550 and deionized water are added at a speed of 150-200 r / min and a temperature of 40-50°C, and the reaction is carried out for 3-5 hours to obtain modified graphene. The modified resin, modified filler, modified graphene and DMF are evenly mixed, and the reaction is carried out for 4-6 hours at a speed of 120-150 r / min, a temperature of 20-25°C and a pH value of 10-11 to obtain a reinforced resin. The following raw materials are weighed in parts by weight: 80-100 parts of polyethylene masterbatch, 30-50 parts of reinforcing resin and 0.5-2 parts of diisopropylbenzene peroxide, the raw materials are melt-blended, and then blown into a film to obtain a plastic packaging film.

2. The method for preparing a plastic packaging film according to claim 1, characterized in that: The amount of KH550 used is 5% of the mass of graphene, and the mass ratio of the modified resin, the modified filler and the modified graphene is 20:5:

2.

3. The method for preparing a plastic packaging film according to claim 1, characterized in that: The modified resin is prepared by the following steps: Step A1: polyvinyl alcohol, p-nitrobenzaldehyde, p-toluenesulfonic acid and toluene are uniformly mixed, nitrogen is introduced for protection, and a reaction is carried out to obtain pretreated polyvinyl alcohol; the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are mixed for reaction, and ammonia water is added to obtain functionalized polyvinyl alcohol; Step A2: functionalized polyvinyl alcohol, maleic anhydride and DMF are mixed for reaction, triethylamine, acetic anhydride and nickel acetate are added for reaction to obtain modified polyvinyl alcohol; modified polyvinyl alcohol, epichlorohydrin, boron trifluoride ether and DMF are mixed for reaction, sodium hydroxide solution is added, and the temperature is increased for reaction to obtain modified resin.

4. The method for preparing a plastic packaging film according to claim 3, characterized in that: The amount ratio of polyvinyl alcohol, p-nitrobenzaldehyde and p-toluenesulfonic acid described in step A1 is 10g:30mmol:1mmol, the mass fraction of polyvinyl alcohol is 2000, and the pretreated polyvinyl alcohol, tin powder and concentrated hydrochloric acid are 2g:2g:5mL.

5. The method for preparing a plastic packaging film according to claim 3, characterized in that: The amount ratio of the amino group, maleic anhydride, triethylamine, acetic anhydride and nickel acetate on the functionalized polyvinyl alcohol described in step A2 is 10mmol:10mmol:4mL:10mL:2.5g, and the amount ratio of the modified polyvinyl alcohol, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution is 5g:1g:0.9g:20mL.

6. The method for preparing a plastic packaging film according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step B1: KH570, sodium hydroxide, isopropanol and deionized water are mixed to react to obtain sodium tetrasiliconate, sodium tetrasiliconate, triethylamine and tetrahydrofuran are mixed evenly, nitrogen is introduced for protection, methyl dichloroethane is added while stirring, and a reaction is carried out to obtain dihydrogen cage-type silsesquioxane; Step B2: dihydrogen cage silsesquioxane, 3-mercaptopropyltrimethoxysilane, benzophenone and DMF are mixed to react to obtain modified silsesquioxane, and the modified silsesquioxane, allyl alcohol glycidyl ether, Custer catalyst and toluene are mixed evenly, and nitrogen is introduced for protection to react to obtain functionalized silsesquioxane; Step B3: functionalized silsesquioxane, DMF, ethanol and deionized water are mixed and stirred, and hydrochloric acid solution is added, and stirred to obtain a modified solution; sodium montmorillonite, ethanol and deionized water are mixed and stirred, and the modified solution is added to react to obtain modified montmorillonite.

7. The method for preparing a plastic packaging film according to claim 6, characterized in that: The amount ratio of KH570, sodium hydroxide, isopropanol and deionized water in step B1 is 20g:3g:100mL:5mL, and the mass ratio of sodium tetrasiliconate, triethylamine and methyl dichloroethane is 11:4:

3.

8. The method for preparing a plastic packaging film according to claim 6, characterized in that: The molar ratio of the double bond on the dihydrogen cage silsesquioxane and 3-mercaptopropyltrimethoxysilane in step B2 is 1:1, and the molar ratio of Si-H on the modified silsesquioxane and allyl alcohol glycidyl ether is 1:

1.

9. The method for preparing a plastic packaging film according to claim 6, characterized in that: The amount ratio of the functionalized silsesquioxane, DMF, ethanol and deionized water described in step B3 is 2g:20mL:15mL:5mL, and the amount ratio of sodium montmorillonite, ethanol, deionized water and modified liquid is 1g:75mL:25mL:20mL.

10. A plastic packaging film, characterized in that: Prepared according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Anti-static degradable film and preparation method thereof

    CN112793274A

  • Modified polyvinyl alcohol film and preparation method thereof

    CN114957895A

  • Polymer composite decorative film and production method thereof

    CN115216097A

  • High barrier RGO-sio2 / pet protective film and preparation method therefor

    WO2021128808A1

Cited By

  • High-temperature-resistant and high-voltage-resistant power tube and preparation method thereof

    CN119307031A

  • Anti-static polyester fabric and preparation method thereof

    CN121700541A

  • An antistatic polyester fabric and its preparation method