Efficient permanent antistatic polypropylene material and preparation method thereof
By using polyether-acrylic acid-methacrylic acid β-hydroxyethyl ester phosphate polymer, sodium hydroxide complex and other additives, a highly efficient and permanent antistatic polypropylene material is prepared, which solves the electrostatic problem of polypropylene materials and achieves antistatic Durability of performance and cost reduction, while improving material compatibility and mechanical properties.
Patent Information
- Application Number
- CN202410846984.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
AI Technical Summary
Polypropylene materials are prone to generate static electricity, leading to electrostatic discharge and fire and explosion risks. Existing antistatic modified materials are costly, difficult to process, and the antistatic effect is greatly affected by environmental humidity.
The antistatic agent is polyether-acrylic acid-methacrylic acid β-hydroxyethyl ester phosphate polymer and sodium hydroxide compound, combined with polyacrylamide, polypropylene grafted maleic anhydride and talc powder, and is manufactured through blending and extrusion. High-efficiency permanent antistatic polypropylene materials are prepared by granulation process.
It achieves the durability of antistatic properties and reduces costs, improves the compatibility and mechanical properties of materials, improves the dispersion and charge transfer capabilities of antistatic agents, and reduces the risk of electrostatic discharge.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polypropylene composite materials, and in particular to a high-efficiency permanent antistatic polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene is widely used in agriculture, industry, construction and other fields due to its advantages of low cost, easy processing, light weight, non-toxicity and stable performance. It ranks second in the world in global plastic production. However, polypropylene is an insulating material and is very easy to generate static electricity due to mechanical effects such as friction. The generated static electricity cannot be effectively transferred and often causes static discharge. In severe cases, it even causes fire and explosion, which greatly restricts the further development and application of polypropylene. Therefore, the development of antistatic polypropylene materials with excellent performance is of great significance to broaden its application fields.
[0003] At present, adding antistatic agents to the material is the mainstream method for antistatic modification of polypropylene. The modified fillers are mainly divided into small molecule type, polymer type, and conductive filler type. Among them, small molecule antistatic agents mainly absorb moisture in the air to form a conductive layer to eliminate static electricity. Its antistatic effect is greatly affected by environmental humidity and is not resistant to water washing. At the same time, the addition of low molecular weight antistatic agents objectively plasticizes polypropylene and has a great impact on the mechanical properties of composite materials. Conductive fillers conduct charges by forming a conductive network in the polypropylene matrix. The antistatic effect is obvious and is not affected by environmental humidity. However, due to poor dispersibility, poor compatibility with polypropylene, and high price, the modified material is difficult to process and the cost is increased. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a high-efficiency permanent antistatic polypropylene material with good performance.
[0005] Another technical problem to be solved by the present invention is to provide a method for preparing the high-efficiency permanent antistatic polypropylene material.
[0006] In order to solve the above problems, the present invention discloses a high-efficiency permanent antistatic polypropylene material, characterized in that the material is composed of the following components in parts by weight: 50-77 parts of polypropylene, 3.75-22.5 parts of antistatic agent, 0.1-3 parts of polyacrylamide, 10 parts of polypropylene grafted maleic anhydride, 0.1-10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 parts of antioxidant 1010 and 0.2 parts of antioxidant 168.
[0007] The antistatic agent is prepared as follows: ① Preparation of functional phosphates: Add β-hydroxyethyl methacrylate (HEMA) to container A equipped with a thermometer and a stirring rod, and stir P at a temperature of 25-35°C. 2O 5 Add in batches and continue stirring. After the raw materials are completely dissolved, control the temperature to 78 °C and react for 4 h. After the esterification reaction is completed, add deionized water, continue to raise the temperature to 90 °C, hydrolyze for 2 h, and then obtain functional phosphate. The β-hydroxyethyl methacrylate (HEMA) and the P 2 O 5 The molar ratio of the β-hydroxyethyl methacrylate (HEMA) to the deionized water is 1:0.48; ② Preparation of HPEG-AA aqueous solution: The unsaturated polyether monomer was added in batches into a container B filled with deionized water and stirred until dissolved. Acrylic acid and hydrogen peroxide were added and the mixture was stirred for 2 hours. 2 The mixture was stirred for 15 min to drive out oxygen, and then an aqueous solution of ferrous chloride was added dropwise. The reaction was placed in a 70°C water bath and continued for 3 h to obtain an HPEG-AA aqueous solution. The mass ratio of the unsaturated polyether monomer to the deionized water was 45:50; the molar ratio of the unsaturated polyether monomer to the acrylic acid was 1:2; and the molar ratio of the unsaturated polyether monomer to the hydrogen peroxide was 1:0.3. ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1:2:4, and the mixture was reacted at 70°C for 24 h to obtain a phosphate copolymer aqueous solution. ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h, then take out the mixture and grind it into powder.
[0008] The polyacrylamide is a cationic polyacrylamide, the polymerization monomer of which is a quaternary ammonium salt, and the molecular weight of which is 100,000.
[0009] The talcum powder is of pharmaceutical grade, wherein the effective content of the talcum powder is greater than 96%, and the average particle size is ≥325 meshes.
[0010] The method for preparing the above-mentioned high-efficiency permanent antistatic polypropylene material comprises the following steps: ⑴Weigh according to the ratio; (2) Add polyacrylamide and talcum powder to distilled water, stir evenly, vacuum dry and grind to obtain mixed powder; the mass ratio of the distilled water, the polyacrylamide and the talcum powder is 20:3:10.5; ⑶ Place the mixed powder obtained in step ⑵, polypropylene, antistatic agent, polypropylene grafted maleic anhydride, sodium hydroxide, antioxidant 1010 and antioxidant 168 in a high-speed blender, stir at a speed of 3 r / s for 5 minutes, extrude and granulate by a twin-screw extruder, and injection mold by an injection molding machine to obtain a high-efficiency permanent antistatic polypropylene material.
[0011] The vacuum drying conditions in step (2) are a temperature of 90° C. and a time of 48 h.
[0012] In step (3), the temperature of each zone of the twin-screw extruder is 200° C. in zone 1, 200° C. in zone 2, and 210° C. in zone 3; the feeder speed is 50 r / min; and the screw speed is 50 r / min.
[0013] In step (3), the injection molding machine has an injection pressure of 0.22 MPa, an injection pressure of 0.20 MPa, a template zone temperature of 80°C, an injection zone temperature of 170°C, an injection time of 3 s, and a mold closing time of 10 s.
[0014] Compared with the prior art, the present invention has the following advantages: 1. The antistatic agent in the present invention is a complex of polyether-acrylic acid-methacrylate β-hydroxyethyl phosphate polymer and sodium hydroxide. Different from small molecule antistatic agents, it has a longer service life, permanent antistatic performance and low cost.
[0015] 2. The antistatic agent added in the present invention is a polymer permanent antistatic agent with a long-lasting antistatic effect; it also contains a polyether group, a phosphate group, and an acrylic acid group, wherein the polyether group improves the poor compatibility of the polar group with the polymer.
[0016] 3. The polyacrylamide and the antistatic agent in the present invention have a synergistic antistatic effect, which can give the material good antistatic properties.
[0017] 4. The addition of maleic anhydride grafted to polypropylene in the present invention can improve the compatibility between polar groups and polypropylene and enhance the antistatic durability of the material.
[0018] 5. The addition of talcum powder in the present invention can give the material good processing performance and mechanical properties, and its excellent lubricity can also improve the dispersion of the antistatic agent in the polypropylene matrix.
[0019] 6. In the present invention, sodium hydroxide is added to neutralize the phosphate group and the acrylic acid group to improve their charge transfer ability, thereby improving their antistatic property.
[0020] 7. The raw materials of the present invention are widely available and low in cost, and the obtained composite has good industrial application prospects. DETAILED DESCRIPTION
[0021] A high-efficiency permanent antistatic polypropylene material is composed of the following components in parts by mass (g): 50-77 parts of polypropylene, 3.75-22.5 parts of antistatic agent, 0.1-3 parts of polyacrylamide, 10 parts of polypropylene grafted maleic anhydride, 0.1-10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 part of antioxidant 1010 and 0.2 part of antioxidant 168.
[0022] Wherein: the antistatic agent is prepared by the following method: ① Preparation of functional phosphates: Add β-hydroxyethyl methacrylate (HEMA) to container A equipped with a thermometer and a stirring rod, and stir P at a temperature of 25-35°C. 2 O 5 Add in batches, β-hydroxyethyl methacrylate (HEMA) and P 2 O 5 The molar ratio of HEMA to deionized water is 3:1, and stirring is continued. After the raw materials are completely dissolved, the temperature is controlled to 78 °C and the reaction is carried out for 4 h. After the esterification reaction is completed, deionized water is added at a molar ratio of β-hydroxyethyl methacrylate (HEMA) to deionized water of 1:0.48, and the temperature is continued to rise to 90 °C. The material is hydrolyzed for 2 h to obtain the functional phosphate.
[0023] ② Preparation of HPEG-AA aqueous solution: 45 g of unsaturated polyether monomer was added in batches into container B containing 50 g of deionized water and stirred until dissolved. Acrylic acid and hydrogen peroxide were added and the mixture was stirred for 2 h. 2 The mixture was deoxygenated for 15 min, and then an aqueous solution of ferrous chloride was added dropwise. The reaction was placed in a 70 °C water bath and continued for 3 h to obtain an aqueous solution of HPEG-AA. The molar ratio of the unsaturated polyether monomer to acrylic acid was 1:2; the molar ratio of the unsaturated polyether monomer to hydrogen peroxide was 1:0.3.
[0024] ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1: 2: 4, and the mixture was reacted at 70° C. for 24 h to obtain a phosphate copolymer aqueous solution.
[0025] ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h to remove excess moisture. Then take out the mixture and grind it into powder.
[0026] Polyacrylamide is a cationic polyacrylamide, its polymerization monomer is a quaternary ammonium salt, and its molecular weight is 100,000.
[0027] The talc is of pharmaceutical grade, with the effective content of talc greater than 96% and the average particle size ≥ 325 mesh.
[0028] A method for preparing a high-efficiency permanent antistatic polypropylene material comprises the following steps: ⑴Weigh according to the ratio; (2) Compatibility treatment of polyacrylamide and talc: Add polyacrylamide and talc into distilled water, stir evenly, vacuum dry and grind to obtain mixed powder; the mass ratio (g / g) of distilled water, polyacrylamide and talc is 20:3:10.5; ⑶ Place the mixed powder obtained in step ⑵, polypropylene, antistatic agent, polypropylene grafted maleic anhydride, sodium hydroxide, antioxidant 1010 and antioxidant 168 in a high-speed blender, stir at a speed of 3 r / s for 5 minutes, and extrude granulate by a twin-screw extruder. The temperature of each zone of the twin-screw extruder is 200°C in zone 1, 200°C in zone 2, and 210°C in zone 3. The speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min. After granulation, the injection molding machine is used for injection molding. The injection pressure of the injection molding machine is 0.22 MPa, the injection pressure of the injection molding machine is 0.20 MPa, the temperature of the template zone is 80°C, the temperature of the injection zone is 170°C, the injection time is 3s, and the mold closing time is 10 s. After molding, a high-efficiency permanent antistatic polypropylene material is obtained.
[0029] The polypropylene in the following examples and comparative examples is polypropylene T30S produced by PetroChina Lanzhou Petrochemical Company.
[0030] Example 1 Prepare 68.95 g of polypropylene, 3.75 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0031] Preparation method: Add polyacrylamide and talcum powder to distilled water, stir evenly, vacuum dry and grind to obtain mixed powder; place the obtained mixed powder, polypropylene, antistatic agent, polypropylene grafted maleic anhydride, sodium hydroxide, antioxidant 1010 and antioxidant 168 in a high-speed blender, stir at a speed of 3 r / s for 5 minutes, and extrude granulation by a twin-screw extruder. The temperature of each zone of the twin-screw extruder is 200 ℃ in zone 1, 200 ℃ in zone 2, and 210 ℃ in zone 3. The speed of the feeder is 50 r / min and the speed of the screw is 50 r / min. After granulation, the injection molding machine is used for injection molding. The injection pressure of the injection molding machine is 0.22 MPa, the injection pressure of the injection molding machine is 0.20 MPa, the temperature of the template zone is 80 ℃, the temperature of the injection zone is 170 ℃, the injection time is 3 s, and the mold closing time is 10 s. After molding, a high-efficiency permanent antistatic polypropylene material is obtained.
[0032] Example 2 Prepare 65.2 g of polypropylene, 7.5 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0033] The preparation method is the same as that of Example 1.
[0034] Example 3 Prepare 61.45 g of polypropylene, 11.25 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0035] The preparation method is the same as that of Example 1.
[0036] Example 4 Prepare 57.7 g of polypropylene, 15 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0037] The preparation method is the same as that of Example 1.
[0038] Example 5 Prepare 53.95 g of polypropylene, 18.75 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0039] The preparation method is the same as that of Example 1.
[0040] Example 6 Prepare 50.2 g of polypropylene, 22.5 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, 0.2 g of antioxidant 168, and 20 g of deionized water.
[0041] The preparation method is the same as that of Example 1.
[0042] Comparative Example 1 Prepare 72.7 g of polypropylene, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.
[0043] The preparation method is the same as that of Example 1.
[0044] Comparative Example 2 Prepare 60.7 g of polypropylene, 15 g of antistatic agent, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.
[0045] The preparation method is the same as that of Example 1.
[0046] Comparative Example 3 Prepare 68.2 g of polypropylene, 15 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.
[0047] The preparation method is the same as that of Example 1.
[0048] Comparative Example 4 Prepare 61.2 g of polypropylene, 15 g of antistatic agent, 3 g of polyacrylamide, 10 g of polypropylene grafted maleic anhydride, 10.5 g of talc, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.
[0049] The preparation method is the same as that of Example 1.
[0050] The materials obtained in Examples 1 to 6 and Comparative Examples 1 to 4 were tested, and the tensile properties were tested according to GB / T1040.1-2006, the impact properties were tested according to GB / T 1843-2008, the melting properties were tested according to GB / T3682-2000, and the surface resistivity was tested according to GB / T1410-2006. After each sample was stored for 90 days, the surface resistivity was tested again according to GB / T1410-2006. The results are shown in Table 1.
[0051] Table 1 Test results As can be seen from Table 1, the antistatic performance of Example 1 is significantly lower than that of Examples 2, 3, 4, and 5, and the antistatic performance of each example is gradually improved, which shows that the antistatic agent has a better effect, but the mechanical properties are gradually reduced, which shows that the antistatic agent has a certain negative impact on the mechanical properties of polypropylene. As time goes by, the antistatic performance of each example does not change much, which shows that the antistatic agent has excellent durability. The antistatic performance in Example 4 decreases significantly, and the mechanical properties are balanced. By comparing the experimental results of Example 4 with those of Comparative Examples 1, 2, and 4, the addition of antistatic agent, polyacrylamide and NaOH significantly improves the antistatic performance of polypropylene materials; compared with Comparative Example 3, the addition of talcum powder in Example 4 significantly improves the impact performance of polypropylene materials. Therefore, the polypropylene material prepared by the present invention has excellent antistatic performance, long-lasting performance, low cost, and great practical advantages.
Claims
1. A highly efficient and permanent antistatic polypropylene material, characterized by: The material consists of the following components in parts by weight: 50-77 parts of polypropylene, 3.75-22.5 parts of antistatic agent, 0.1-3 parts of polyacrylamide, 10 parts of polypropylene grafted maleic anhydride, 0.1-10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 part of antioxidant 1010 and 0.2 part of antioxidant 168.
2. A high-efficiency permanent antistatic polypropylene material as claimed in claim 1, characterized in that: The antistatic agent is prepared as follows: ① Preparation of functional phosphate esters: Add β-hydroxyethyl methacrylate to container A equipped with a thermometer and a stirring rod, add P2O5 in batches at a temperature of 25-35°C, and continue stirring. After the raw materials are completely dissolved, control the temperature to 78°C and react for 4 hours; after the esterification reaction is completed, add deionized water, continue to heat to 90°C, hydrolyze for 2 hours, and obtain functional phosphate; the molar ratio of the β-hydroxyethyl methacrylate to the P2O5 is 3:1; the molar ratio of the β-hydroxyethyl methacrylate to the deionized water is 1:0.48; ② Preparation of HPEG-AA aqueous solution: The unsaturated polyether monomer was added to the container B filled with deionized water in batches and stirred until dissolved, acrylic acid and hydrogen peroxide were added, N2 was passed for 15 min to drive out oxygen, and then ferrous chloride aqueous solution was added dropwise, and the reaction was placed in a 70°C water bath pot and continued for 3 hours to obtain HPEG-AA aqueous solution; the mass ratio of the unsaturated polyether monomer to the deionized water was 45:50; the molar ratio of the unsaturated polyether monomer to the acrylic acid was 1:2; the molar ratio of the unsaturated polyether monomer to the hydrogen peroxide was 1:0.3; ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1:2:4, and the mixture was reacted at 70°C for 24 h to obtain a phosphate copolymer aqueous solution. ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h, then take out the mixture and grind it into powder.
3. A high-efficiency permanent antistatic polypropylene material as claimed in claim 1, characterized in that: The polyacrylamide is a cationic polyacrylamide, the polymerization monomer of which is a quaternary ammonium salt, and the molecular weight of which is 100,000.
4. A highly efficient permanent antistatic polypropylene material as claimed in claim 1, characterized in that: The talcum powder is of pharmaceutical grade, wherein the effective content of the talcum powder is greater than 96%, and the average particle size is ≥325 meshes.
5. A method for preparing a high-efficiency permanent antistatic polypropylene material as claimed in any one of claims 1 to 4, comprising the following steps: ⑴Weigh according to the ratio; (2) Add polyacrylamide and talcum powder to distilled water, stir evenly, vacuum dry and grind to obtain mixed powder; the mass ratio of the distilled water, the polyacrylamide and the talcum powder is 20:3:10.5; ⑶ Place the mixed powder obtained in step ⑵, polypropylene, antistatic agent, polypropylene grafted maleic anhydride, sodium hydroxide, antioxidant 1010 and antioxidant 168 in a high-speed blender, stir at a speed of 3 r / s for 5 minutes, extrude and granulate by a twin-screw extruder, and injection mold by an injection molding machine to obtain a high-efficiency permanent antistatic polypropylene material.
6. The method for preparing a high-efficiency permanent antistatic polypropylene material according to claim 5, characterized in that: The vacuum drying conditions in step (2) are a temperature of 90° C. and a time of 48 h.
7. The method for preparing a high-efficiency permanent antistatic polypropylene material according to claim 5, characterized in that: In step (3), the temperature of each zone of the twin-screw extruder is 200° C. in zone 1, 200° C. in zone 2, and 210° C. in zone 3; the speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min.
8. The method for preparing a high-efficiency permanent antistatic polypropylene material according to claim 5, characterized in that: In step (3), the injection molding machine has an injection pressure of 0.22 MPa, an injection pressure of 0.20 MPa, a template zone temperature of 80°C, an injection zone temperature of 170°C, an injection time of 3 s, and a mold closing time of 10 s.