Permanent amphoteric antistatic compound and preparation method thereof

By using a specific ratio of anionic and cationic antistatic agents, compatibilizers and talc in polyolefin plastics, a permanent amphoteric antistatic compound is formed, which solves the static problem of polyolefin plastics and achieves high-efficiency antistatic performance and low The combination of cost broadens its application fields.

CN118745271APending Publication Date: 2024-10-08LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410846987.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing polyolefin plastic materials are prone to generate static electricity due to friction, leading to electrostatic induction or fire and explosion, which limits their application fields. Moreover, existing antistatic agents are expensive and have poor compatibility, making it difficult to meet performance and safety requirements.

Method used

Using a permanent amphoteric antistatic compound composed of polypropylene, anionic antistatic agent, cationic antistatic agent, compatibilizer polypropylene grafted with maleic anhydride, talc and sodium hydroxide, through specific preparation methods and proportions , forming a polymeric antistatic agent with good compatibility with the polymer matrix and long-lasting antistatic properties.

Benefits of technology

It achieves long-lasting antistatic properties of the material, improves the compatibility between polar groups and the plastic matrix, improves the mechanical properties and antistatic durability of the material, reduces costs, and has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a permanent amphoteric antistatic compound, which is prepared from the following components in parts by mass: 45 to 60 parts of polypropylene, 2.5 to 15 parts of anionic antistatic agent, 2.5 to 15 parts of cationic antistatic agent, 10 parts of compatilizer polypropylene grafted maleic anhydride, 10.5 parts of talcum powder, 3.5 parts of sodium hydroxide, 0.1 part of antioxidant 1010 and 0.2 part of antioxidant 168. Meanwhile, the invention also discloses a preparation method of the compound. The antistatic plastic has excellent antistatic property and mechanical property, high durability and low cost, and has a good industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material modification, in particular to a permanent amphoteric antistatic composite and a preparation method thereof. Background Art

[0002] Polyolefin plastics are made of one or more olefins homopolymerized or copolymerized. They are widely used in agriculture, industry, construction and other fields due to their low cost, easy processing, light weight, non-toxicity and stable performance. However, most polyolefin plastics are insulating materials, which are very easy to generate static electricity due to mechanical effects such as friction, which may cause static induction or static discharge of materials, or cause fire and explosion, which greatly restricts the further development and application of such materials. Therefore, the development of antistatic polymer materials with excellent performance is of great significance to broaden their application fields.

[0003] Polymer antistatic agents are widely used in the field of polymer antistatic due to their excellent antistatic performance, long-lasting effect, and unaffected by environmental factors. According to the type of ionized groups, they can be divided into anionic, cationic, and amphoteric types. Among them, anionic antistatic agents have relatively good compatibility with polymer matrices, but their antistatic effect is weak; although cationic antistatic agents have significant effects, their high price, poor compatibility with polymers, and easy leakage from the inside of products still limit their application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a permanent amphoteric antistatic composite with good performance.

[0005] Another technical problem to be solved by the present invention is to provide a method for preparing the permanent amphoteric antistatic composite.

[0006] In order to solve the above problems, the present invention discloses a permanent amphoteric antistatic composite, characterized in that the composite is composed of the following components in parts by mass: 45-60 parts of polypropylene, 2.5-15 parts of anionic antistatic agent, 2.5-15 parts of cationic antistatic agent, 10 parts of compatibilizer polypropylene grafted maleic anhydride, 10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 parts of antioxidant 1010 and 0.2 parts of antioxidant 168.

[0007] The anionic antistatic agent is prepared as follows: ① Preparation of functional phosphates: Add β-hydroxyethyl methacrylate (HEMA) to a container A equipped with a thermometer and a stirring rod, add P2O5 in batches at a temperature of 25-35°C, and continue stirring. After the raw materials are completely dissolved, control the temperature to 78°C and react for 4 hours; after the esterification reaction is completed, add deionized water, continue to heat to 90°C, hydrolyze for 2 hours, and obtain functional phosphate; the molar ratio of the β-hydroxyethyl methacrylate (HEMA) to the P2O5 is 3:1; the molar ratio of the β-hydroxyethyl methacrylate (HEMA) to the deionized water is 1:0.48; ② Preparation of HPEG-AA aqueous solution: The unsaturated polyether monomer was added into the container B containing deionized water in batches and stirred until dissolved, acrylic acid and hydrogen peroxide were added, N2 was passed for 15 min to drive out oxygen, and then ferrous chloride aqueous solution was added dropwise, and the reaction was placed in a 70°C water bath pot and continued for 3 h to obtain HPEG-AA aqueous solution; the mass ratio of the unsaturated polyether monomer to the deionized water was 45:50; the molar ratio of the unsaturated polyether monomer to the acrylic acid was 1:2; the molar ratio of the unsaturated polyether monomer to the hydrogen peroxide was 1:0.3; ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1:2:4, and the mixture was reacted at 70°C for 24 hours to obtain a phosphate copolymer aqueous solution. ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h, then take out the mixture and grind it into powder.

[0008] The cationic antistatic agent is a polyether-quaternary ammonium salt copolymer.

[0009] The talcum powder is of pharmaceutical grade, wherein the effective content of the talcum powder is greater than 96%, and the average particle size is ≥325 meshes.

[0010] The method for preparing a permanent amphoteric antistatic composite as described above is characterized in that: first, the weights are weighed according to the ratio; then, polypropylene, anionic antistatic agent, cationic antistatic agent, compatibilizer polypropylene grafted maleic anhydride, talcum powder, sodium hydroxide, antioxidant 1010 and antioxidant 168 are placed in a high-speed blender, stirred at a speed of 3 r / s for 5 minutes, extruded and granulated by a twin-screw extruder, and injection molded by an injection molding machine to obtain the permanent amphoteric antistatic composite.

[0011] The temperature of each zone of the twin-screw extruder is 200°C in zone 1, 200°C in zone 2, and 210°C in zone 3. The speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min.

[0012] The injection molding machine has an injection pressure of 0.22 MPa, an injection pressure of 0.20 MPa, a template zone temperature of 80°C, an injection zone temperature of 170°C, an injection time of 3 s, and a mold closing time of 10 s.

[0013] Compared with the prior art, the present invention has the following advantages: 1. The anionic antistatic agent in the present invention is a complex of polyether-acrylic acid-methacrylate β-hydroxyethyl phosphate polymer and sodium hydroxide. Different from small molecule antistatic agents, it has a longer service life, permanent antistatic performance and low cost.

[0014] 2. The cationic antistatic agent in the present invention is a polyether-quaternary ammonium salt copolymer, which has permanent antistatic properties and good compatibility with polymer materials.

[0015] 3. The antistatic agents added in the present invention are all polymer antistatic agents with long-lasting antistatic effect; at the same time, the polyether groups contained in the anionic and cationic antistatic agents can effectively improve the poor compatibility between the polar groups and the plastic matrix, and improve the mechanical properties of the material.

[0016] 4. In the present invention, polypropylene grafted maleic anhydride is a compatibilizer, which can improve the compatibility between the antistatic agent and the polymer matrix, thereby improving the antistatic durability of the material.

[0017] 5. The addition of talc in the present invention can give the material good processing properties and mechanical properties, and its excellent lubricity can also improve the dispersion of the antistatic agent in the polypropylene matrix.

[0018] 6. Adding sodium hydroxide in the present invention can enhance the material's ability to transfer charge and improve its antistatic properties.

[0019] 7. The raw materials of the present invention are widely available and low in cost, and the obtained composite has good industrial application prospects. DETAILED DESCRIPTION

[0020] A permanent amphoteric antistatic composite comprises the following components in parts by mass (g): 45-60 parts of polypropylene, 2.5-15 parts of anionic antistatic agent, 2.5-15 parts of cationic antistatic agent, 10 parts of polypropylene grafted maleic anhydride as a compatibilizer, 10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 parts of antioxidant 1010 and 0.2 parts of antioxidant 168.

[0021] Wherein: the anionic antistatic agent is prepared by the following method: ① Preparation of functional phosphates: Add β-hydroxyethyl methacrylate (HEMA) to container A equipped with a thermometer and a stirring rod, add P2O5 in batches at a temperature of 25-35°C, the molar ratio of β-hydroxyethyl methacrylate (HEMA) to P2O5 is 3:1, and continue stirring. After the raw materials are completely dissolved, control the temperature to 78°C and react for 4 hours; after the esterification reaction is completed, add deionized water at a molar ratio of β-hydroxyethyl methacrylate (HEMA) to deionized water of 1:0.48, continue to heat to 90°C, hydrolyze for 2 hours, and obtain functional phosphate.

[0022] ② Preparation of HPEG-AA aqueous solution: 45 g of unsaturated polyether monomer was added in batches to container B containing 50 g of deionized water and stirred until dissolved, acrylic acid and hydrogen peroxide were added, N2 was passed for 15 min to drive out oxygen, and then ferrous chloride aqueous solution was added dropwise, and the reaction was placed in a 70 ℃ water bath for 3 h to obtain HPEG-AA aqueous solution. The molar ratio of unsaturated polyether monomer to acrylic acid was 1:2; the molar ratio of unsaturated polyether monomer to hydrogen peroxide was 1:0.3.

[0023] ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1:2:4, and the mixture was reacted at 70°C for 24 hours to obtain a phosphate copolymer aqueous solution.

[0024] ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h to remove excess moisture. Then take out the mixture and grind it into powder.

[0025] The cationic antistatic agent is a polyether-quaternary ammonium salt copolymer, and its preparation reference patent is a polymer permanent cationic antistatic agent for polymer materials and its preparation method, patent number is ZL202210295133.0.

[0026] The talc is of pharmaceutical grade, with the effective content of talc greater than 96% and the average particle size ≥ 325 mesh.

[0027] A method for preparing a permanent amphoteric antistatic composite: First, the mixture is weighed according to the ratio; then polypropylene, anionic antistatic agent, cationic antistatic agent, compatibilizer polypropylene grafted maleic anhydride, talcum powder, sodium hydroxide, antioxidant 1010 and antioxidant 168 are placed in a high-speed blender, stirred at a speed of 3 r / s for 5 minutes, and extruded into granules by a twin-screw extruder. The temperature of each zone of the twin-screw extruder is 200°C in zone 1, 200°C in zone 2, and 210°C in zone 3. The speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min. After granulation, the injection molding machine is used for injection molding. The injection pressure of the injection molding machine is 0.22 MPa, the injection pressure of the injection molding machine is 0.20 MPa, the temperature of the template zone is 80°C, the temperature of the injection zone is 170°C, the injection time is 3 s, and the mold closing time is 10 s. After molding, a permanent amphoteric antistatic composite is obtained.

[0028] Example 1 Prepare 60.7 g of polypropylene, 12.5 g of anionic antistatic agent, 2.5 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0029] Preparation method: After weighing the above materials, place them in a high-speed blender, stir them at a speed of 3 r / s for 5 minutes, and extrude and granulate them by a twin-screw extruder. The temperature of each zone of the twin-screw extruder is 200°C in zone 1, 200°C in zone 2, and 210°C in zone 3. The speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min. After granulation, the injection molding machine is used for injection molding. The injection pressure of the injection molding machine is 0.22 MPa, the injection pressure of the injection molding machine is 0.20 MPa, the temperature of the template zone is 80°C, the temperature of the injection zone is 170°C, the injection time is 3 s, and the mold closing time is 10 s. After molding, a permanent amphoteric antistatic composite is obtained.

[0030] Example 2 Prepare 60.7 g of polypropylene, 10 g of anionic antistatic agent, 5 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0031] The preparation method is the same as that of Example 1.

[0032] Example 3 Prepare 60.7 g of polypropylene, 7.5 g of anionic antistatic agent, 7.5 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0033] The preparation method is the same as that of Example 1.

[0034] Example 4 Prepare 60.7 g of polypropylene, 5 g of anionic antistatic agent, 10 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0035] The preparation method is the same as that of Example 1.

[0036] Example 5 Prepare 60.7 g of polypropylene, 2.5 g of anionic antistatic agent, 12.5 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0037] The preparation method is the same as that of Example 1.

[0038] Comparative Example 1 Prepare 60.7 g of polypropylene, 15 g of anionic antistatic agent, 0 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0039] The preparation method is the same as that of Example 1.

[0040] Comparative Example 2 Prepare 60.7 g of polypropylene, 0 g of anionic antistatic agent, 15 g of cationic antistatic agent, 10 g of compatibilizer polypropylene grafted maleic anhydride, 10.5 g of talc, 3.5 g of sodium hydroxide, 0.1 g of antioxidant 1010, and 0.2 g of antioxidant 168.

[0041] The preparation method is the same as that of Example 1.

[0042] The materials obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were tested, and the tensile properties were tested according to GB / T1040.1-2006, the impact properties were tested according to GB / T 1843-2008, the melting properties were tested according to GB / T3682-2000, and the surface resistivity was tested according to GB / T1410-2006. After each sample was stored for 90 days, the surface resistivity was tested again according to GB / T1410-2006. The results are shown in Table 1.

[0043] Table 1 Test results As can be seen from Table 1, the antistatic performance of Example 1 is significantly lower than that of Examples 2, 3, 4, and 5, and the antistatic performance and impact strength of each embodiment are gradually improved, which shows that the comprehensive effect of the cationic antistatic agent is better than that of the anionic antistatic agent. As time goes by, the antistatic performance of each embodiment does not change much, which shows that the antistatic agent has excellent durability. In Example 5, the antistatic performance rises significantly, and the impact strength rises significantly. By comparing the experimental results of Example 5 with Comparative Examples 1 and 2, the synergistic effect of anionic and cationic antistatic agents significantly improves the antistatic performance and impact properties of the material. Therefore, the present invention has excellent antistatic performance and mechanical properties, high durability and low cost, and has good industrial application prospects.

Claims

1. A permanent amphoteric antistatic composite, characterized in that: The compound is composed of the following components in parts by weight: 45-60 parts of polypropylene, 2.5-15 parts of anionic antistatic agent, 2.5-15 parts of cationic antistatic agent, 10 parts of polypropylene grafted maleic anhydride as a compatibilizer, 10.5 parts of talc, 3.5 parts of sodium hydroxide, 0.1 parts of antioxidant 1010 and 0.2 parts of antioxidant 168.

2. A permanent amphoteric antistatic composite as claimed in claim 1, characterized in that: The anionic antistatic agent is prepared as follows: ① Preparation of functional phosphate esters: Add β-hydroxyethyl methacrylate to container A equipped with a thermometer and a stirring rod, add P2O5 in batches at a temperature of 25-35°C, and continue stirring. After the raw materials are completely dissolved, control the temperature to 78°C and react for 4 hours; after the esterification reaction is completed, add deionized water, continue to heat to 90°C, hydrolyze for 2 hours, and obtain functional phosphate; the molar ratio of the β-hydroxyethyl methacrylate to the P2O5 is 3:1; the molar ratio of the β-hydroxyethyl methacrylate to the deionized water is 1:0.48; ② Preparation of HPEG-AA aqueous solution: The unsaturated polyether monomer was added to the container B filled with deionized water in batches and stirred until dissolved, acrylic acid and hydrogen peroxide were added, N2 was passed for 15 min to drive out oxygen, and then ferrous chloride aqueous solution was added dropwise, and the reaction was placed in a 70°C water bath pot and continued for 3 hours to obtain HPEG-AA aqueous solution; the mass ratio of the unsaturated polyether monomer to the deionized water was 45:50; the molar ratio of the unsaturated polyether monomer to the acrylic acid was 1:2; the molar ratio of the unsaturated polyether monomer to the hydrogen peroxide was 1:0.3; ③ Preparation of phosphate copolymer aqueous solution: The HPEG-AA aqueous solution, the catalyst p-toluenesulfonic acid hydrate, and the functional phosphate were mixed in a molar ratio of 1:2:4, and the mixture was reacted at 70°C for 24 h to obtain a phosphate copolymer aqueous solution. ④ Test the pH value of the phosphate copolymer aqueous solution. When the pH value is 2, add 22.5% NaOH solution dropwise into the phosphate copolymer aqueous solution until the pH value of the solution is 12. Dry the phosphate copolymer mixed solution in a 90 °C vacuum drying oven for 48 h, then take out the mixture and grind it into powder.

3. A permanent amphoteric antistatic composite as claimed in claim 1, characterized in that: The cationic antistatic agent is a polyether-quaternary ammonium salt copolymer.

4. A permanent amphoteric antistatic composite as claimed in claim 1, characterized in that: The talcum powder is of pharmaceutical grade, wherein the effective content of the talcum powder is greater than 96%, and the average particle size is ≥325 meshes.

5. A method for preparing a permanent amphoteric antistatic composite according to any one of claims 1 to 4, characterized in that: First, weigh according to the ratio; then put polypropylene, anionic antistatic agent, cationic antistatic agent, compatibilizer polypropylene grafted maleic anhydride, talcum powder, sodium hydroxide, antioxidant 1010 and antioxidant 168 in a high-speed blender, stir at a speed of 3 r / s for 5 minutes, extrude and granulate by a twin-screw extruder, and injection mold by an injection molding machine to obtain a permanent amphoteric antistatic composite.

6. The method for preparing a permanent amphoteric antistatic composite according to claim 5, characterized in that: The temperature of each zone of the twin-screw extruder is 200°C in zone 1, 200°C in zone 2, and 210°C in zone 3. The speed of the feeder is 50 r / min, and the speed of the screw is 50 r / min.

7. The method for preparing a permanent amphoteric antistatic composite according to claim 5, characterized in that: The injection molding machine has an injection pressure of 0.22 MPa, an injection pressure of 0.20 MPa, a template zone temperature of 80°C, an injection zone temperature of 170°C, an injection time of 3 s, and a mold closing time of 10 s.

Citation Information

Patent Citations

  • Polymer permanent antistatic agent and preparation method thereof

    CN114539486A