EPDM (Ethylene-Propylene-Diene Monomer) thermal insulation material with foam structure regulated and controlled by carbon nanomaterial and
By using carbon nanomaterials to regulate the cell structure in EPDM insulation materials, the problem of ablation resistance and density reduction of existing materials is solved, the material's ablation resistance is improved and the cell structure is uniform, ensuring Product quality consistency.
Patent Information
- Application Number
- CN202410737433.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
AI Technical Summary
While the density of existing EPDM insulation materials is reduced, the ablation resistance is reduced and the cell structure is uneven, which makes it difficult to meet the requirements for product quality consistency, affecting its application in solid rocket motors.
The preparation method of using carbon nanomaterials to control the cell structure, by adding carbon nanotubes, graphene or graphene oxide, and combining specific process steps such as pre-sulfurization and positive sulfurization to control the cell structure and improve the ablation resistance of the material and density.
It significantly enhances the ablation resistance of EPDM insulation materials, while achieving uniformity of cell structure and reduction in density, ensuring the quality consistency of the material.
Smart Images

Figure BDA0004882205170000061 
Figure BDA0004882205170000071 
Figure HDA0004882205190000011
Abstract
Description
Technical Field
[0001] The invention relates to a solid rocket engine and a heat protection material, and in particular to an EPDM heat insulation material with a pore structure regulated by a carbon nanometer material and a preparation method thereof. Background Art
[0002] Laying an insulation layer inside the combustion chamber shell is the main means of thermal protection for solid rocket engines. However, the insulation layer is an inert mass, which reduces the thrust-to-mass ratio of the engine to a certain extent. Therefore, reducing the density of insulation materials is an important issue in the field of rocket engines. At present, researchers mainly use the characteristics of foaming agents that produce gas by pyrolysis at high temperatures to introduce gas into the insulation material to reduce the density of the material.
[0003] At present, the most widely used insulation material is ethylene propylene diene monomer (EPDM) rubber-based composite material, and the foaming agents that match its processing technology are mainly AC and OBSH. Studies have found that adding the above-mentioned foaming agents can achieve a maximum reduction of about 40% in material density, greatly reducing the density of the material and achieving lightweight. However, it also brings about the problem of a sharp decline in the ablation resistance of EPDM insulation materials, as well as defects such as uneven pore structure and large dispersion of pore sizes in different batches of products. This neither meets the product's requirements for ablation resistance nor the requirements for product quality consistency, making it difficult for the product to be applied and promoted. Summary of the invention
[0004] In view of the defects and shortcomings of the prior art, the present invention provides an EPDM thermal insulation material with a pore structure regulated by carbon nanomaterials.
[0005] To this end, the raw materials for preparing the EPDM thermal insulation material with carbon nanomaterials regulating the pore structure provided by the present invention include: EPDM rubber, aramid fiber, carbon fiber, phenolic resin, white carbon black, zinc oxide, paraffin oil, sulfur, OBSH (4,4'-oxybisbenzenesulfonyl hydrazide) and carbon nanomaterial; the particle size of the OBSH is 5-50um; the carbon nanomaterial is selected from carbon nanotubes (CNTs), graphene (G) or graphene oxide (GO); the mass ratio of the EPDM rubber, aramid fiber, carbon fiber, phenolic resin, white carbon black, zinc oxide, paraffin oil, sulfur, OBSH and carbon nanomaterial is 100: (5-20): (5-20): (5-20): (5-30): (1-20): (1-15): (0.5-5): (1-20): (1-20).
[0006] An optional solution is that the aramid fibers are short-cut aramid fibers with a length of 5 to 8 mm.
[0007] An optional solution is that the carbon fiber is chopped carbon fiber with a length of 2 to 5 mm.
[0008] An optional solution is that the length of the CNTs is between 10 and 200 um.
[0009] The present invention also provides a method for preparing the EPDM thermal insulation material with a pore structure controlled by the carbon nanomaterial, the preparation method comprising the following steps:
[0010] Step 1: Prepare the first substrate
[0011] The formulated EPDM rubber is kneaded on a double-roll mill to obtain a first matrix;
[0012] Step 2: Prepare the second substrate
[0013] Adding a formulated amount of aramid fiber into the first matrix and kneading until uniform to obtain a second matrix;
[0014] Step 3: Prepare the third substrate
[0015] Adding a formulated amount of carbon nanomaterial into the second matrix and mixing until uniform, to obtain a third matrix;
[0016] Step 4: Prepare the fourth substrate
[0017] Adding the formulated amount of OBSH into the third matrix and mixing until uniform, to obtain a fourth matrix;
[0018] Step 5: Prepare the fifth substrate
[0019] Adding a formula amount of paraffin oil, phenolic resin, white carbon black and zinc oxide into the fourth matrix and mixing evenly to obtain a fifth matrix;
[0020] Step 6: Prepare the sixth substrate
[0021] Adding a formula amount of sulfur and carbon fiber into the fifth matrix and mixing until uniform, to obtain a sixth matrix;
[0022] Step 7: Prepare the seventh substrate
[0023] The sixth base body is kneaded and pressed into a sheet shape on an open mill to obtain a seventh base body;
[0024] Step 8: Pre-vulcanization
[0025] Pre-curing the seventh substrate at 110-150° C. to obtain an eighth substrate;
[0026] Step 9: Vulcanization
[0027] After the pre-vulcanization is completed, the temperature is raised to 160-180°C for vulcanization, and after the vulcanization is completed, it is naturally cooled to obtain the insulation material.
[0028] An optional solution is to add a portion of the paraffin oil in the above step five to the fourth matrix; then add the formulated amount of phenolic resin, white carbon black and zinc oxide, and add the remaining paraffin oil during the addition process; after all are added, mix evenly to obtain the fifth matrix.
[0029] An optional solution is that in the above step eight, the seventh substrate is placed in a mold and pre-cured at a high temperature of 110 to 150° C. to obtain an eighth substrate.
[0030] An optional solution is that the pre-vulcanization time is 10 to 20 minutes.
[0031] An optional solution is that the vulcanization time is 30 to 60 minutes.
[0032] The foamed EPDM thermal insulation material of the present invention regulates the pore structure and enhances the ablation resistance of the material through carbon nanomaterials, so that the ablation resistance of the material is enhanced, the material performance can be adjusted by controlling the pore structure, and the quality consistency of the thermal insulation material can be guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart for preparing the carbon nanomaterial reinforced foamed EPDM thermal insulation material of the present invention.
[0034] Figure 2 It is a comparison chart of thermal conductivity of the embodiment and the comparative example.
[0035] Figure 3 It is a density comparison diagram of the embodiment and the comparative example.
[0036] Figure 4 This is a SEM photograph of the foam cells of the material prepared in Example 1.
[0037] Figure 5 This is a SEM photograph of the pores of the material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0038] Unless otherwise specified, the scientific and technical terms in this article are understood according to the knowledge of ordinary technicians in the relevant fields. It should be noted that the following are specific embodiments of the present invention. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0039] All raw materials and testing methods used in the present invention, unless otherwise specified, are those known in the art. For example:
[0040] Ethylene propylene diene monomer rubber EPDM is a conventional material known in the prior art. The following examples use Japanese Mitsui 4045 EPDM rubber. Phenolic resin uses conventional phenolic resin products known in the prior art. The phenolic resins in the following examples come from Shaanxi Taihang Fire Retardant Polymer Co., Ltd. Paraffin oil uses conventional analytical pure paraffin oil known in the prior art. The paraffin oil in the following examples is produced by Chengdu Kelong Chemical Reagent Factory. The aramid fiber used in the following examples is chopped aramid fiber with a length of 5 to 8 mm. Carbon fiber is chopped carbon fiber with a length of 2 to 5 mm. CNTs have a length between 10 and 200 um.
[0041] The thermal conductivity test adopts the oxyacetylene ablation test device known in the prior art, and the test process refers to GJB-323A-1996 in the "National Military Standard".
[0042] Embodiment 1:
[0043] The foamed EPDM insulation material of this embodiment is prepared from the following raw materials, by mass: 100 parts of EPDM rubber, 10 parts of aramid fiber, 5 parts of carbon fiber, 10 parts of phenolic resin, 15 parts of white carbon black, 5 parts of zinc oxide, 5 parts of paraffin oil, 1 part of sulfur, 5 parts of OBSH (OBSH particle size is 25-35um), and 5 parts of CNTs.
[0044] In this embodiment, Figure 1 As shown, the preparation method of the thermal insulation material specifically includes the following steps:
[0045] Step 1: preparing the first substrate:
[0046] Putting the formulated EPDM rubber into an XK-160 double-roll mill for mixing to obtain a first matrix;
[0047] Step 2: Prepare the second substrate
[0048] Putting the formulated amount of aramid fiber into the first matrix and mixing, and passing through 10 times until uniform, to obtain a second matrix;
[0049] Step 3: Prepare the third substrate
[0050] Putting the formulated amount of CNTs into the second matrix and kneading until uniform, to obtain a third matrix;
[0051] Step 4: Prepare the fourth substrate
[0052] Add the formulated amount of OBSH into the third matrix and mix until uniform to obtain a fourth matrix;
[0053] Step 5: Prepare the fifth substrate
[0054] Weigh the formula amount of phenolic resin, white carbon black, zinc oxide and paraffin oil; then add a part of the paraffin oil to the fourth matrix, and then add the phenolic resin, white carbon black and zinc oxide, and gradually add the remaining paraffin oil during the adding process; after all the additions are completed, mix and knead evenly to obtain the fifth matrix;
[0055] Step 6: Prepare the sixth substrate
[0056] Sequentially adding the formulated amount of sulfur and carbon fiber into the fifth matrix and kneading until uniform, thereby obtaining a sixth matrix;
[0057] Step 7: Prepare the seventh substrate
[0058] The sixth substrate is prepared into a 2 mm thin sheet on an open mill, and cut according to the specifications of the vulcanization mold to obtain the seventh substrate;
[0059] Step 8: Pre-vulcanization
[0060] The seventh substrate is placed in a mold and pre-cured at 120° C. for 15 minutes to obtain an eighth substrate;
[0061] Step 9: Vulcanization
[0062] After the pre-vulcanization is completed, the temperature is directly raised to 160°C for vulcanization for 30 minutes. After the vulcanization is completed, it is naturally cooled and demolded to obtain the final carbon nanomaterial-reinforced EPDM insulation material.
[0063] Comparative Example 1:
[0064] The difference between this comparative example and Example 1 is that no foamed CNTs are added and there is no pre-sulfurization step. During the preparation, step 9 is directly performed after step 7 is completed.
[0065] Comparative Example 2:
[0066] The difference between this comparative example and Example 1 is that no CNTs are added, and step 4 is directly performed after step 2 is completed during preparation.
[0067] Comparative Example 3:
[0068] The difference between this comparative example and Example 1 is that the particle size distribution of OBSH is: 1-200 um.
[0069] Comparative Example 4:
[0070] The difference between this comparative example and Example 1 is that there is no pre-sulfurization step eight, that is, step nine is directly carried out after step seven is completed.
[0071] Embodiment 2:
[0072] The difference between this embodiment and embodiment 1 is that the amount of the foaming agent OBSH added is 2 parts.
[0073] Embodiment 3:
[0074] The difference between this embodiment and embodiment 1 is that the added amount of the blowing agent OBSH is 10 parts.
[0075] Embodiment 4:
[0076] This embodiment is different from embodiment 1 in that the amount of CNTs added is 2 parts.
[0077] Embodiment 5:
[0078] The difference between this embodiment and embodiment 1 is that the amount of CNTs added is 10 parts.
[0079] Embodiment 6:
[0080] The carbon nanotubes CNTs in the example are replaced with an equal amount of graphene G.
[0081] Embodiment 7:
[0082] The carbon nanotubes CNTs in the example are replaced with an equal amount of graphene oxide GO.
[0083] The thermal insulation materials prepared in the above examples and comparative examples were tested for density, thermal conductivity and microscopic morphology. The test results are shown in Tables 1 and Figure 1-2 shown.
[0084] Table 1 Material properties of examples and comparative examples
[0085]
[0086]
[0087] From Table 1, Figure 2 and Figure 3 It can be seen that adding carbon nanomaterials and adopting the preparation process of the present invention can not only promote the foaming of the foaming agent to reduce the density of the EPDM insulation material, but also enhance the ablation resistance of the insulation material.
[0088] from Figure 4-Figure 5 It can be seen that CNTs and the process of the present invention change the pore structure of the foamed EPDM, so that the pore diameter increases and the pore diameter distribution becomes more uniform, eliminating the existence of macropores.
Claims
1. An EPDM thermal insulation material with carbon nanomaterials regulating the pore structure, characterized in that: The raw materials for preparing the thermal insulation material include: EPDM rubber, aramid fiber, carbon fiber, phenolic resin, white carbon black, zinc oxide, paraffin oil, sulfur, OBSH and carbon nanomaterials; the particle size of the OBSH is 5-50um; the carbon nanomaterial is selected from carbon nanotubes, graphene or graphene oxide; the mass ratio of the EPDM rubber, aramid fiber, carbon fiber, phenolic resin, white carbon black, zinc oxide, paraffin oil, sulfur, OBSH and carbon nanomaterials is 100: (5-20): (5-20): (5-20): (5-30): (1-20): (1-15): (0.5-5): (1-20): (1-20).
2. The EPDM thermal insulation material with carbon nanomaterial-controlled pore structure according to claim 1, characterized in that: The aramid fiber is short-cut aramid fiber with a length of 5 to 8 mm.
3. The EPDM thermal insulation material with carbon nanomaterial-controlled pore structure according to claim 1, characterized in that: The carbon fiber is short-cut carbon fiber with a length of 2 to 5 mm.
4. The EPDM thermal insulation material with carbon nanomaterial-controlled pore structure according to claim 1, characterized in that: The length of the CNTs is between 10 and 200 um.
5. The method for preparing the EPDM thermal insulation material with carbon nanomaterial-controlled pore structure according to claim 1, characterized in that: The preparation method comprises the following steps: Step 1: Prepare the first substrate The formulated EPDM rubber is kneaded on a double-roll mill to obtain a first matrix; Step 2: Prepare the second substrate Adding a formulated amount of aramid fiber into the first matrix and kneading until uniform to obtain a second matrix; Step 3: Prepare the third substrate Adding a formulated amount of carbon nanomaterial into the second matrix and mixing until uniform, to obtain a third matrix; Step 4: Prepare the fourth substrate Adding the formulated amount of OBSH into the third matrix and mixing until uniform, to obtain a fourth matrix; Step 5: Prepare the fifth substrate Adding a formula amount of paraffin oil, phenolic resin, white carbon black and zinc oxide into the fourth matrix and mixing evenly to obtain a fifth matrix; Step 6: Prepare the sixth substrate Adding a formula amount of sulfur and carbon fiber into the fifth matrix and mixing until uniform, to obtain a sixth matrix; Step 7: Prepare the seventh substrate The sixth base body is kneaded and pressed into a sheet shape on an open mill to obtain a seventh base body; Step 8: Pre-vulcanization Pre-curing the seventh substrate at 110-150° C. to obtain an eighth substrate; Step 9: Vulcanization After the pre-vulcanization is completed, the temperature is raised to 160-180°C for vulcanization, and after the vulcanization is completed, it is naturally cooled to obtain the insulation material.
6. The preparation method according to claim 5, characterized in that: In step five, a part of paraffin oil is added to the fourth matrix; then a formula amount of phenolic resin, white carbon black and zinc oxide are added, and the remaining paraffin oil is added during the adding process; after all are added, they are mixed evenly to obtain the fifth matrix.
7. The preparation method according to claim 5, characterized in that: In step eight, the seventh substrate is placed in a mold and pre-cured at a high temperature of 110-150° C. to obtain the eighth substrate.
8. The preparation method according to claim 5, characterized in that: The pre-vulcanization time is 10 to 20 minutes.
9. The preparation method according to claim 5, characterized in that: The curing time is 30 to 60 minutes.