Method for plasticizing PLA (Polylactic Acid) by using bio-based plasticizer, PLA plasticizing master batch and application of PLA plasticizing master batch
Through the grafting reaction of cardanol ethyl ester and epoxidized cardanol ethyl ester, combined with the twin-screw extrusion and mixing process, the problem of PLA plasticizer precipitation and migration is solved, and more efficient plasticizing effect and performance are achieved. promote.
Patent Information
- Application Number
- CN202410918234.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-08
AI Technical Summary
Existing PLA plasticizers are prone to precipitation and migration during the plasticization process, resulting in reduced performance, especially at high content, the elongation at break will be reduced.
Cardanol ethyl ester and epoxidized cardanol ethyl ester are used as plasticizers, and melt extrusion is carried out through a twin-screw extruder or a mixing torque rheometer, and additives such as free radical initiators or catalysts are added. Plasticizer molecules are grafted onto PLA chains to form PLA plasticizer masterbatch, which is used for self-plasticization to reduce migration and volatilization rates.
It improves the plasticizing effect, reduces the precipitation and migration rate of plasticizer, maintains good mechanical properties, and improves the utilization rate and processing convenience of PLA.
Smart Images

Figure BDA0004935815900000061 
Figure BDA0004935815900000071 
Figure BDA0004935815900000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biodegradable materials, and specifically relates to a method for plasticizing PLA with a bio-based plasticizer, a PLA plasticizing masterbatch and an application thereof in plasticizing PLA. Background Art
[0002] Due to the increasing shortage of petroleum resources and the aggravation of white pollution, polylactic acid (PLA) has become the most popular polymer in the market among biodegradable and bio-based polymers. It is made of 100% renewable resources and can be completely composted and degraded within one month. It has many advantages, such as high strength and high modulus, high optical properties, good barrier properties, biocompatibility, safety and non-toxicity, but the Tg of PLA is 55-60℃, it is hard and brittle at room temperature, and its mechanical properties are slightly poor (poor impact strength, low elongation at break, low heat deflection temperature), which limits its application. Therefore, the research on PLA is currently focused on plasticization, blending, copolymerization, surface modification and other aspects to improve processing properties or increase glassy flexibility and impact strength.
[0003] Among them, plasticization is the most effective way to improve the flexibility of polymers. By adding plasticizers, the PLA molecular chains are separated, making the movement between the chains easier, and the overall performance is soft and tough. However, the selection of plasticizers is affected by many factors, such as compatibility with PLA, thermal stability of plasticizers, safety and non-toxicity, etc. Currently, commonly used plasticizers for PLA include: citrate, polyethylene glycol (PEG), low molecular weight polyester, etc. Cardanol is a phenolic substance extracted from cashew nut shell oil, 100% natural, which can replace or partially replace phenol in the manufacture of epoxy curing agent, liquid phenolic resin, liquid or powdered thermosetting phenolic resin, and it can also be used as a plasticizer to plasticize brittle plastics such as PLA, and the plasticization effect is excellent. Because it comes from biomass, it is environmentally friendly and non-toxic. Once discovered, it has become a hot spot in current research.
[0004] Plasticizers all have the problem of precipitation and migration, which is caused by the incompatibility between the plasticizer molecules and the plastic matrix. The incompatibility of the system will also cause the agglomeration of the plasticizer molecules, resulting in phase separation and affecting the performance of the product.
[0005] Chinese patent CN117229233 discloses a cardanol-based plasticizer and its application and PLA film, wherein cardanol ethyl ester, acetylated cardanol ethyl ester and epoxidized cardanol ethyl ester are used to plasticize PLA. However, the plasticizing method is physical plasticizing, i.e., external plasticizing, and the plasticizer is simply added to PLA. With the change of time and environment, the internal plasticizer will still gradually precipitate, and once the content of the plasticizer reaches saturation, the elongation at break of the plasticized product may decrease due to phase separation. Summary of the invention
[0006] The first object of the present invention is to provide a method for plasticizing PLA with a bio-based plasticizer to improve the plasticizing effect and reduce the migration and volatilization rate of the plasticizer.
[0007] The second object of the present invention is to provide a PLA plasticized masterbatch obtained according to the method of plasticizing PLA with a bio-based plasticizer.
[0008] The third object of the present invention is to provide the use of the PLA plasticizer masterbatch in self-plasticizing PLA, which can further reduce the migration and volatility of the plasticizer while reducing the amount of bio-based plasticizer used.
[0009] To achieve the above object, the present invention provides the following solutions:
[0010] In a first aspect, the present invention provides a method for plasticizing PLA with a bio-based plasticizer, wherein the raw materials are mixed and then melt-extruded or kneaded by a twin-screw extruder, and then cooled to obtain a PLA modified material; the raw materials include the following components, and the component contents are expressed in parts by weight:
[0011] PLA 65-75 parts
[0012] Plasticizer 25-35 parts
[0013] Additives 0.05-1 part
[0014] Antioxidant 0.1-0.5 parts
[0015] The plasticizer is cardanol ethyl ester and / or epoxidized cardanol ethyl ester;
[0016] The auxiliary agent is a free radical initiator or a catalyst for catalyzing the reaction between epoxy groups and carboxyl groups.
[0017] Preferably, the plasticizer is cardanol ethyl ester, the auxiliary agent is a free radical initiator, and the free radical initiator is at least one of di-tert-butyl peroxyisopropylbenzene (BIBP) and diisopropylbenzene peroxide (DCP), which is used to initiate the reaction between the double bonds on the cardanol and the PLA main chain.
[0018] Preferably, the plasticizer is epoxidized cardanol ethyl ester, the auxiliary agent is a catalyst for catalyzing the reaction between epoxy groups and carboxyl groups, and the catalyst for catalyzing the reaction between epoxy groups and carboxyl groups is triphenylethyl phosphonium bromide, which is used to catalyze the reaction between epoxy groups and PLA terminal carboxyl groups.
[0019] Preferably, the antioxidant is at least one of antioxidant 168 and antioxidant 1010, more preferably a compound of antioxidant 1010 and antioxidant 168, with the compounding mass ratio being 2:1.
[0020] Preferably, the method is implemented according to the following steps:
[0021] Weigh each component by weight, mix the additive, antioxidant and plasticizer evenly to obtain a liquid mixture, pour PLA into the feed port, and when the PLA material reaches the first vacuum port, add the liquid mixture from the first vacuum port through a constant flow pump, perform melt extrusion with a twin-screw extruder, and cool and pelletize to obtain a PLA modified material.
[0022] Preferably, the twin-screw extruder is a 35-speed machine, the screw aspect ratio is 52:1, and the processing temperature of each zone is (°C):
[0023] 130, 145, 150, 153, 155, 160, 165, 165, 150, 140, 130, 130, 135.
[0024] Preferably, the mixing conditions are as follows: pouring PLA into a mixing torque rheometer, adding plasticizer, additive and oxidant after melting, the temperature is 170-180°C, the rotation speed is 50-60rpm / min, the time is 5-8min, and cooling after mixing is completed to obtain PLA modified material.
[0025] In a second aspect, the present invention provides a PLA plasticizer masterbatch, wherein the raw materials for preparing the PLA plasticizer masterbatch and the amounts thereof are as follows:
[0026] Low molecular weight PLA 50-60 parts
[0027] Plasticizer 40-50 parts
[0028] Catalyst 0.05-1 part
[0029] The acid value (terminal carboxyl content) of the low molecular weight PLA is 600-650 mol / t; the catalyst is triphenylethyl phosphonium bromide; the plasticizer is epoxy cardanol ethyl ester;
[0030] The PLA plasticizer masterbatch is prepared by the following method: low molecular weight PLA is added into a reaction container, heated and melted under nitrogen protection, and then epoxy cardanol ethyl ester and a catalyst are added, stirred for reaction, poured into another container, cooled and shaped to obtain a wax block plasticizer, and then crushed to obtain the PLA plasticizer masterbatch.
[0031] The low molecular weight PLA used in the present invention can be obtained by hydrolyzing commercial PLA, specifically by adding water to PLA, heating at 80-95°C for a certain period of time, and drying to obtain low molecular weight PLA. During the above reaction, PLA undergoes hydrolysis and chain scission to obtain low molecular weight PLA. The degree of hydrolysis is controlled by the change of the acid value of the product, so the heating time can be determined by the molecular weight of commercial PLA (characterized by the acid value in the present invention) and the acid value of the desired low molecular weight.
[0032] Preferably, the stirring reaction time is 8-15 min.
[0033] In a third aspect, the present invention provides an application of the PLA plasticizer masterbatch described in the second invention in PLA self-plasticization, wherein the feed mass ratio of PLA to the PLA plasticizer masterbatch is 9:1 to 7:3.
[0034] The application is specifically as follows: after mixing PLA, plasticizer masterbatch and antioxidant, pouring into a mixing torque rheometer, the temperature is 170-180° C., the rotation speed is 50-60 rpm / min, and the time is 5-8 min. After the mixing is completed, plasticized PLA is obtained; the mass amount of the antioxidant is 0.1-0.5% of the total mass amount of PLA and PLA plasticizer masterbatch.
[0035] Preferably, the antioxidant is at least one of antioxidant 168 and antioxidant 1010, more preferably a compound of antioxidant 1010 and antioxidant 168, with the compounding mass ratio being 2:1.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) Conventional plasticization is to infiltrate plasticizer molecules into the molecular chains to separate the molecular chains, thereby improving the mobility of the chain segments. This is external plasticization. In addition to external plasticization, the present invention also grafts the plasticizer molecules onto the PLA chain through reaction (i.e., internal plasticization), which not only improves the plasticization effect but also reduces the precipitation mobility of the plasticizer.
[0038] (2) For the traditional twin-screw processing method, the materials are first mixed and then added to the hopper. This is suitable for solid materials or materials containing a small amount of liquid phase, but it is not suitable for materials with a large amount of liquid phase. This will cause the liquid to be lost quickly and the material ratio cannot be controlled. The present invention uses a constant flow pump to add the liquid material to the extruder through the first vacuum port, and controls the different ratios of the product by different flow rates. It has the advantages of uniform speed and stability, and the ratio of each phase in the product is uniform.
[0039] (3) The present invention utilizes low molecular weight PLA and epoxy cardanol ethyl ester to fully react, forming a solid plasticizer, namely PLA plasticizer masterbatch, which is used again for PLA plasticization, which is called self-plasticization. PLA plasticized in this way has the advantage of low mobility, while maintaining a good plasticizing effect, the utilization rate of low molecular weight PLA is improved, and solid plasticizers are more convenient in processing than liquids, solving the cumbersome and unstable process problem of liquid feeding in the extruder. In addition, compared with direct plasticization of bioplasticizers, PLA plasticizer masterbatch can achieve lower bioplasticizer precipitation and mobility with lower content of bioplasticizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is the infrared spectra of PLA, ethyl cardanol and the grafted product (Example 1). DETAILED DESCRIPTION
[0041] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0042] The "parts" and "phr" mentioned in the present invention refer to parts by weight unless otherwise specified.
[0043] In the following examples, the PLA used is REVODE101 purchased from Zhejiang Haizheng Biomaterial Co., Ltd., the cardanol ethyl ester (CA) and epoxidized cardanol ethyl ester (ECA) used are produced by Jiangsu Lianmeng Chemical Co., Ltd., and the initiator, catalyst, antioxidant 1010 and antioxidant 168 used are all commercially available industrial-grade reagents. The antioxidant 1010 / 168 used in the examples is composed of antioxidants 1010 and 168 in a mass ratio of 2:1.
[0044] Comparative Example 1
[0045] PLA 100phr
[0046] Antioxidant 1010 / 168 0.5phr
[0047] The preparation method comprises the following steps: weighing the above raw materials by weight, mixing them, performing twin-screw melt extrusion, and cooling to obtain a biodegradable material, wherein the temperature of each section of the twin-screw extruder is set as follows: 140° C. for the first section, 145° C. for the second section, 150° C. for the third section, 155° C. for the fourth section, 155° C. for the fifth section, 160° C. for the sixth section, 165° C. for the seventh section, 170° C. for the eighth section, 170° C. for the ninth section, 165° C. for the tenth section, 160° C. for the eleventh section, and 150° C. for the twelfth section, the die temperature is 155° C., the melt pressure of the extrusion is 2 MPa, the main screw speed is 160 rpm / min, and the feeding speed is 5.5 Hz.
[0048] Comparative Example 2
[0049] Plasticized PLA was prepared using the following raw materials in the following ratios:
[0050] PLA 75phr
[0051] Ethyl cardanol 25phr
[0052] Antioxidant 1010 / 168 0.5phr
[0053] The preparation method comprises the following steps: weighing the above raw materials by weight, pouring PLA into a hopper, opening a constant flow pump to add a plasticizer when the material reaches a first vacuum port, performing twin-screw melt extrusion, cooling and pelletizing to obtain a biodegradable material, and during reactive extrusion, setting the temperature of each section of the twin-screw extruder as follows: 130° C. for the first section, 145° C. for the second section, 150° C. for the third section, 153° C. for the fourth section, 155° C. for the fifth section, 160° C. for the sixth section, 165° C. for the seventh section, 165° C. for the eighth section, 150° C. for the ninth section, 140° C. for the tenth section, 130° C. for the eleventh section, 130° C. for the twelfth section, a die head temperature of 135° C., an extruded melt pressure of 2 MPa, a main screw speed of 160 rpm / min, and a feeding speed of 5.5 rpm / min to obtain PLA-25CA.
[0054] Comparative Example 3
[0055] The same as comparative example 2, except that 70 parts of PLA and 30 parts of cardanol ethyl ester were used to obtain PLA-30CA.
[0056] Comparative Example 4
[0057] The same as comparative example 2, the only difference is that 65 parts of PLA and 35 parts of cardanol ethyl ester are used to obtain PLA-35CA.
[0058] Example 1
[0059] Plasticized PLA was prepared using the following raw materials in the following ratios:
[0060]
[0061] The preparation method is the same as that of Comparative Example 2.
[0062] Example 2
[0063] Same as Example 1, except that PLA is 70 parts and cardanol ethyl is 30 parts.
[0064] Example 3
[0065] Same as Example 1, except that the amount of PLA is 65 parts and the amount of cardanol ethyl ester is 35 parts.
[0066] Comparative Example 5
[0067] The same as comparative example 2, the only difference is that 75 parts of PLA and 25 parts of epoxy cardanol ethyl ester (replacing cardanol ethyl ester) are used to obtain PLA-25ECA.
[0068] Comparative Example 6
[0069] The same as comparative example 2, the only difference is that 70 parts of PLA and 30 parts of epoxy cardanol ethyl ester (replacing cardanol ethyl ester) are used to obtain PLA-30ECA.
[0070] Comparative Example 7
[0071] The same as comparative example 2, the only difference is that 65 parts of PLA and 35 parts of epoxy cardanol ethyl ester (replacing cardanol ethyl ester) are used to obtain PLA-35ECA.
[0072] Example 4
[0073] Plasticized PLA was prepared using the following raw materials in the following ratios:
[0074]
[0075] The preparation method is the same as that of Example 1.
[0076] Example 5
[0077] Same as Example 4, except that the amount of PLA is 70 parts and the amount of epoxy cardanol ethyl is 30 parts.
[0078] Example 6
[0079] Same as Example 4, except that the amount of PLA is 65 parts and the amount of epoxy cardanol ethyl is 35 parts.
[0080] Comparative Example 8
[0081] Plasticized PLA was prepared using the following raw materials in the following ratios:
[0082]
[0083] Pour PLA into a mixing torque rheometer, add epoxy cardanol ethyl ester, catalyst and antioxidant after melting, temperature 180°C, rotation speed 60rpm / min, time 6min, and cool after mixing to obtain plasticized PLA.
[0084] Comparative Example 9
[0085] The same as Comparative Example 8, the only difference is that PLA 85 parts, epoxy cardanol ethyl ester 15 parts.
[0086] Comparative Example 10
[0087] The same as comparative example 8, the difference is only 80 parts of PLA and 20 parts of epoxy cardanol ethyl ester.
[0088] Comparative Example 11
[0089] The same as comparative example 8, the only difference is that PLA is 75 parts and epoxy cardanol ethyl is 25 parts.
[0090] Comparative Example 12
[0091] The same as comparative example 8, the only difference is that PLA is 70 parts and epoxy cardanol ethyl is 30 parts.
[0092] Example 7
[0093] 1. Preparation of low molecular weight PLA
[0094] PLA (REVODE101 from Zhejiang Hisun Biomaterials Co., Ltd.) was added to water, heated at 90°C for 24 hours, and then placed in an oven for thorough drying to obtain low molecular weight PLA, whose acid value was measured to be 642.5 mol / t.
[0095] 2. Preparation of PLA plasticizer masterbatch
[0096] Nitrogen was introduced into the flask, 50 parts of low molecular weight PLA were melted in the flask at 180°C, and then 50 parts of epoxy cardanol ethyl ester and 0.5 parts of catalyst triphenylethyl phosphonium bromide were added. The reaction was stirred for 10 minutes until the reaction was completed. The mixture was poured into a container, cooled and shaped, and then crushed to obtain PLA plasticized masterbatch.
[0097] 3. Use the following proportions of raw materials to prepare plasticized PLA:
[0098] PLA 90phr
[0099] PLA plasticizer masterbatch 10phr
[0100] Antioxidant 1010 / 168 0.5phr
[0101] After mixing PLA plasticizer masterbatch and PLA, pour into mixing torque rheometer. The preparation method is the same as that of Comparative Example 8.
[0102] Example 8
[0103] Same as Example 7, except that the amount of PLA is 85 parts and the amount of plasticizer masterbatch is 15 parts.
[0104] Example 9
[0105] Same as Example 7, except that there are 80 parts of PLA and 20 parts of plasticizer masterbatch.
[0106] Example 10
[0107] Same as Example 7, except that the amount of PLA is 75 parts and the amount of plasticizer masterbatch is 25 parts.
[0108] Embodiment 11
[0109] Same as Example 7, except that there are 70 parts of PLA and 30 parts of plasticizer masterbatch.
[0110] The amounts of raw materials used in Comparative Examples 1-4 and Examples 1-3 are shown in Table 1:
[0111] Table 1
[0112]
[0113]
[0114] The amount of raw materials used in Comparative Examples 5-6 and Examples 4-6 is shown in Table 2
[0115] Table 2
[0116] PLA ECA catalyst Comparative Example 5 75 25 Comparative Example 6 70 30 Comparative Example 7 65 35 Example 4 75 25 0.05 Example 5 70 30 0.05 Example 6 65 35 0.05
[0117] The amount of raw materials used in Comparative Examples 8-12 and Examples 7-11 is shown in Table 3
[0118] Table 3
[0119]
[0120]
[0121] Performance Testing
[0122] The products obtained in each embodiment were characterized by the following method:
[0123] (1) Fourier transform infrared spectroscopy of plasticizers was performed using a PerkinElmer 782 infrared spectrometer.
[0124] (FTIR) analysis. The scanning frequency was 32, the scanning range was 400-4000cm-1, and the resolution was 4cm -1 FTIR spectrum of
[0125] (2) Determination of acid value (terminal carboxyl content): According to FZ / T 50012-2006, the sample is dissolved in a mixed solvent of phenol-chloroform under reflux, cooled and titrated with a potassium hydroxide-ethanol standard titration solution using bromophenol blue as an indicator. The terminal carboxyl content is calculated based on the volume consumed by the standard titration solution.
[0126] (3) The mechanical properties of the specimens were tested on a universal material testing machine controlled by Jiangsu Qiantong (QT-6201S) according to GB / T 1040.1-2006 to obtain the elongation at break (EB, %) and tensile strength (TS, MPa) of the samples. The specimens were 5A type, the spacing between the splines was set to 30 mm, the tensile speed was 100 mm / min, and each group of samples was tested 3-5 times. The average value was taken and the error was calculated.
[0127] (4) Migration test: According to ISO 177:1988, a circular specimen with a thickness of 0.5 mm and contact material of oil-absorbing cotton was used. The weighed specimen and the oil-absorbing cotton were assembled and covered with two glass plates and a 5 kg weight was pressed on top. The specimen was placed in an oven at 70°C for 24 h and then the weight change of the specimen and the oil-absorbing cotton was measured.
[0128] (5) Volatility test: According to ISO 176:2005, "Determination of plasticizer loss in plastics - Activated carbon test method". Place the test piece in the bottom of a metal container and sprinkle 120cm 3 The sample is covered with activated carbon and the lid is closed. The PVC sample container is placed in a 70±1℃ oven or a constant temperature water bath. After 24 hours, the test piece is taken out and the mass loss is measured after the activated carbon on the surface is removed.
[0129] Results Analysis
[0130] 1. Characterization of plasticizer masterbatch structure
[0131] The PLA modified material sample obtained in Example 1 was dissolved in chloroform by heating under reflux for 30 minutes and then cooled to room temperature. The product was precipitated with ethanol and rinsed several times to wash away the plasticizer and PLA contained in the product. The washed product was placed in a 60° C. oven for 12 hours.
[0132] Figure 1 PLA, cardanol ethyl ester and washing products at 4000-400cm -1 The infrared absorption spectrum between Figure 1 It can be seen that at 1595 and 1455cm -1 The characteristic peaks at 696 and 910 cm-1 are the skeleton vibrations of the benzene ring. -1 The peak at the center is the out-of-plane bending vibration peak of the CH on the benzene ring, indicating that the product contains a benzene ring, that is, the plasticizer molecule is successfully grafted onto the PLA main chain.
[0133] Table 4 Changes in product acid value
[0134] Comparative Example 5 Comparative Example 6 Comparative Example 7 Example 4 Example 5 Example 6 Acid value mol / t 20.13 18.79 17.44 11.41 8.23 6.19
[0135] Table 4 shows the changes in acid values of Comparative Examples 5-7 and Examples 4-6, which is a test of the terminal carboxyl content in PLA, to roughly analyze whether the epoxy group in the plasticizer reacts with the terminal carboxyl group of PLA. The decrease in acid value in Comparative Examples 5-7 is due to the decrease in the proportion of PLA in the plasticized PLA. It can be seen that the terminal carboxyl content in the product is significantly reduced after the addition of the catalyst, indicating that the terminal carboxyl group of PLA reacts with the epoxy group, and the plasticizer molecule is grafted onto the PLA main chain.
[0136] 2. Mechanical properties test
[0137] Table 5 Tensile strength and elongation at break
[0138]
[0139]
[0140] The tensile strength of pure PLA is 69.68MPa, and the elongation at break is 8.81%. With the addition of plasticizer, the tensile strength decreases rapidly and the elongation at break increases significantly. This is because the plasticizer molecules penetrate into the chains and separate the molecular chains, increasing the slippage between the molecular chains. In addition, a large amount of plasticizer causes phase separation, resulting in a significant decrease in tensile strength. For both systems, with the increase of plasticizer content, the tensile strength does not change much after the addition of initiator and catalyst, but the elongation at break increases to a certain extent.
[0141] Table 6 Tensile strength and elongation at break
[0142]
[0143]
[0144] From the perspective of mechanical properties, the PLA plasticized by the two plasticizers has similar performance. The PLA plasticized by the simple plasticizer has a higher plasticizing efficiency due to the higher actual content of the plasticizer, so the tensile strength is low and the elongation at break is high. The impact strength of the PLA plasticized by PLA-g-ELF is slightly higher, and when the content is increased, the sample is not broken, indicating that the PLA changes from brittle to tough as the plasticizer content increases. In addition, taking Example 11 as an example, it can be seen that the plasticizing effect of the self-plasticizing masterbatch is good. When the overall plasticizer content is about 15%, the elongation at break reaches 386%, which is equivalent to Comparative Example 10, and the tensile strength is slightly higher, reaching the plasticizing effect of 20% plasticizer content. This can be attributed to the uniform distribution of the plasticizer between the PLA molecular chains after secondary processing, reducing the situation of phase separation, and the mechanical properties are partially maintained. In addition, due to the grafting of the plasticizer molecules to the PLA main chain, the PLA chain is irregular, which inhibits its crystallization, making it more flexible, and the elongation at break is improved.
[0145] 3. Plasticizer migration / volatilization rate test
[0146] Table 7 Plasticizer migration rate / volatility rate
[0147]
[0148]
[0149] As can be seen from the table above, in the case of high-content plasticization without adding any conditions, the migration and volatility of the plasticizer is relatively high, and it cannot be used as a product. By adding an initiator and a catalyst to introduce the reaction, part of the plasticizer is grafted onto the PLA chain, preventing the precipitation of the plasticizer. By comparing Comparative Examples 2-4 and Examples 1-3, it can be seen that the migration and volatility are greatly reduced. The epoxy plasticizer itself has good compatibility with PLA, so the migration and volatility are already low. By introducing the reaction system, the migration and volatility are further reduced.
[0150] Table 8 Migration rate of PLA plasticized by plasticized masterbatch
[0151]
[0152]
[0153] It can be seen from the above table that when PLA is directly plasticized with epoxy cardanol ethyl ester without adding any additives, when the plasticizer content is higher than 20%, some analyses have shown that when the content reaches 25%-30%, the migration rate of the plasticizer exceeds 9%, which means that the plasticized PLA can no longer meet the use requirements. Under the same conditions, the migration rate of samples plasticized with low molecular weight PLA and ELF is significantly reduced. This may be because, on the one hand, some plasticizer molecules are grafted onto the short chain of PLA to prevent migration, and on the other hand, the plasticizer has undergone two processes to make the dispersion in PLA more uniform, making it less likely to precipitate.
[0154] Based on the above experiments, adding initiators or catalysts to graft plasticizer molecules onto PLA and using plasticizer masterbatches prepared from low molecular weight PLA to plasticize PLA have a relatively obvious improvement effect in preventing the precipitation and migration of plasticizers. At the same time, this method is suitable for mass production, and the plasticizer masterbatch also facilitates the feeding production, which has certain application prospects.
Claims
1. A method for plasticizing PLA with a bio-based plasticizer, wherein the raw materials are mixed and then melt-extruded or kneaded by a twin-screw extruder, and then cooled to obtain a PLA modified material; characterized in that: The raw materials include the following components, and the component contents are expressed in parts by weight: PLA 65-75 parts Plasticizer 25-35 parts Additives 0.05-1 part Antioxidant 0.1-0.5 parts The plasticizer is cardanol ethyl ester and / or epoxidized cardanol ethyl ester; The auxiliary agent is a free radical initiator or a catalyst for catalyzing the reaction between epoxy groups and carboxyl groups.
2. The method according to claim 1, characterized in that: The plasticizer is cardanol ethyl ester, the auxiliary agent is a free radical initiator, and the free radical initiator is at least one of di-tert-butyl peroxide isopropylbenzene and diisopropylbenzene peroxide.
3. The method according to claim 1, characterized in that: The plasticizer is epoxidized cardanol ethyl ester, the auxiliary agent is a catalyst for catalyzing the reaction between epoxy groups and carboxyl groups, and the catalyst for catalyzing the reaction between epoxy groups and carboxyl groups is triphenylethyl phosphonium bromide.
4. The method according to any one of claims 1 to 3, characterized in that: The antioxidant is at least one of the antioxidant 168 and the antioxidant 1010 .
5. The method according to any one of claims 1 to 3, characterized in that: The method is implemented according to the following steps: Weigh each component by weight, mix the additive, antioxidant and plasticizer evenly to obtain a liquid mixture, pour PLA into the feed port, and when the PLA material reaches the first vacuum port, add the liquid mixture from the first vacuum port through a constant flow pump, perform melt extrusion with a twin-screw extruder, and cool and pelletize to obtain a PLA modified material.
6. The method according to claim 5, characterized in that: The twin-screw extruder is a 35-inch machine with a screw length-to-diameter ratio of 52:
1. The processing temperature of each zone is (°C): 130,145,150,153,155,160,165,165,150,140,130,130,135。 7. The method according to claim 5, characterized in that: The mixing conditions are as follows: pouring PLA into a mixing torque rheometer, adding a plasticizer, an additive and an oxidant after melting, setting the temperature to 170-180° C., the rotation speed to 50-60 rpm / min, and the time to 5-8 min. After mixing is completed, cooling is performed to obtain a PLA modified material.
8. A PLA plasticizer masterbatch, the raw materials for preparing the PLA plasticizer masterbatch and the amounts thereof are as follows: Low molecular weight PLA 50-60 parts Plasticizer 40-50 parts Catalyst 0.05-1 part The acid value of the low molecular weight PLA is 600-650 mol / t; the catalyst is triphenylethyl phosphonium bromide; the plasticizer is epoxy cardanol ethyl ester; The PLA plasticizer masterbatch is prepared by the following method: low molecular weight PLA is added into a reaction container, heated and melted under nitrogen protection, and then epoxy cardanol ethyl ester and a catalyst are added, stirred for reaction, poured into another container, cooled and shaped to obtain a wax block plasticizer, and then crushed to obtain the PLA plasticizer masterbatch.
9. Use of the PLA plasticizer masterbatch in PLA self-plasticization as claimed in claim 8, wherein the feed mass ratio of PLA to the PLA plasticizer masterbatch is 9:1 to 7:
3.
10. The use according to claim 9, characterized in that: The application is specifically as follows: after mixing PLA, PLA plasticizer masterbatch and antioxidant, pouring into a mixing torque rheometer, the temperature is 170-180° C., the rotation speed is 50-60 rpm / min, and the time is 5-8 min. After the mixing is completed, plasticized PLA is obtained; the mass amount of the antioxidant is 0.1-0.5% of the total mass amount of PLA and the plasticizer masterbatch.
Citation Information
Patent Citations
Method for preparing low-mobility polylactic-acid-base plasticizing wood-plastic composite material
CN104262915A
Cardanol-based plasticizer, application thereof and PLA (polylactic acid) film
CN117229233A
Cited By
Environment-friendly lawn filling particles and preparation method thereof
CN119842193A
An environmentally friendly lawn infill granule and its preparation method
CN119842193B
Terpene alcohol ester full-bio-based polylactic acid plasticizer and application thereof
CN120794846A