Environment-friendly anti-adhesion acrylate coating as well as preparation method and application thereof

The silicone-modified acrylate coating is prepared through an emulsion polymerization process and combined with nano-silica sol, which solves the problems of easy loss of existing anti-adhesion material structures and solvent usage, and achieves environmentally friendly, durable low adhesion and anti-fouling effects, which is suitable for many applications. kind of base material.

CN118745309AInactive Publication Date: 2024-10-08GUANGZHOU UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410977859.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing anti-adhesion materials have problems such as easy wear of structure, easy loss of lubricating oil, and the use of organic solvents, resulting in durability and environmental safety risks in practical applications.

Method used

Using water as the solvent, silicone-modified acrylate polymer emulsion and nano-silica sol composite materials are prepared through an emulsion polymerization process to form an environmentally friendly anti-adhesion acrylate coating and improve the hardness and adhesion of the coating.

Benefits of technology

It has achieved a VOC-free, environmentally friendly anti-adhesion coating with good low adhesion, antifouling, transparency and mechanical properties. It is suitable for a variety of substrates, reduces production costs, and is in line with the green development trend.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745309A_ABST
    Figure CN118745309A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly anti-adhesion acrylate coating as well as a preparation method and application thereof. The invention relates to an anti-adhesion acrylate coating. The preparation raw materials of the coating comprise an organic silicon modified acrylate polymer emulsion and nano silica sol. The environment-friendly anti-adhesion acrylate coating is prepared by utilizing an emulsion polymerization system, VOC emission is avoided in the coating process, threats to biological safety and environmental safety are avoided, and preparation of the environment-friendly anti-adhesion functional coating is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of novel polymer functional materials and polymer coatings, and in particular to an environmentally friendly anti-adhesion acrylate coating and a preparation method and application thereof. Background Art

[0002] The wetting and non-wetting behavior of contact liquids on solid surfaces has received great attention in daily life and industrial production. Surfaces with extremely low liquid adhesion have very promising applications in anti-fouling self-cleaning, anti-icing, drag reduction, oil-water separation and anti-corrosion, so this type of material has attracted the research and development interest of more and more scientific and technical workers. With the development of science and technology, existing anti-adhesion materials mainly include super-amphiphobic surfaces with micro-nano structures inspired by bio-inspired "lotus leaf-like", "nepenthes-like" lubricant-injected porous surfaces and monolayer or polymer-based liquid-like surfaces. These materials show repulsive behavior to water, oil and liquids with multiple complex components, that is, by giving the material surface a certain tilt angle, the contact liquid can easily detach from the surface, thereby maintaining the self-cleaning of the material surface. However, super-amphiphobic surface materials have the characteristics of easy wear of the structure, and the lubricant-injected porous surface faces the problem of easy loss of the lubricant, which limits their practical application scenarios. Liquid-like surfaces are grafted with flexible polymer chains or silane monolayers onto smooth solid surfaces, and are not limited by the complex rough structure design and easy loss of functional components on the surface, so they have more application advantages than the former two. Among them, the silane monolayer liquid-like materials are only a few nanometers thick and lack ideal durability in practical applications.

[0003] In contrast, polymer-based liquid-like materials have the advantage of more stable performance. At present, most of the reports on polymer-based liquid-like materials are polymerized through organic solutions. A few silicone-containing polyurethane anti-adhesion water dispersions also require the addition of organic solvents before phase transition in the synthesis process. The use of organic solvents has a negative impact on human health and environmental safety, and also increases production and transportation costs. Therefore, it is of great significance to develop solvent-free or water-based continuous phase polymer emulsion anti-adhesion coatings. Summary of the invention

[0004] In order to overcome the problems existing in the above-mentioned prior art, the present invention provides an environmentally friendly anti-adhesion acrylate coating and a preparation method and application thereof. The anti-adhesion acrylate coating of the present invention uses water as a solvent, which is safe and environmentally friendly.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A first aspect of the present invention provides an anti-adhesion acrylic coating, wherein raw materials for preparing the coating include organosilicon-modified acrylic polymer emulsion and nano-silica sol.

[0007] Preferably, the raw materials for preparing the coating include 30-100 wt % of organosilicon-modified acrylate polymer emulsion and 0-70 wt % of nano-silica sol.

[0008] Preferably, the raw materials for preparing the coating include 50-70 wt % of organosilicon-modified acrylate polymer emulsion and 30-50 wt % of nano-silica sol.

[0009] The nano-silica sol is a commercially available 30 wt% nano-silicon dioxide aqueous solution, which is used as reinforcing particles and compounded into an organosilicon-modified acrylate polymer emulsion to improve mechanical properties such as hardness and adhesion of the latex film.

[0010] Preferably, the organosilicon-modified acrylate polymer emulsion is prepared by emulsion polymerization of vinyl monomer and organosilicon monomer in the presence of an initiator, an emulsifier, a pH adjuster and water.

[0011] The organosilicon-modified acrylate polymer emulsion has the characteristics of high transparency, good film-forming property, low surface energy and antifouling.

[0012] Preferably, the vinyl monomer includes at least one of acrylic acid, methacrylic acid, styrene, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, isobutyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, octadecyl methacrylate, octadecyl acrylate, lauryl acrylate, and lauryl methacrylate; further preferably, the vinyl monomer includes at least one of methacrylic acid, styrene, methyl methacrylate, n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, octadecyl methacrylate, octadecyl acrylate, lauryl acrylate, and lauryl methacrylate.

[0013] Preferably, the organosilicon monomer is vinyl-modified silicone oil; further preferably, the vinyl-modified silicone oil comprises 3572, 3572F5, 3821F3, 3821F8, 3855, At least one of 3826.

[0014] Preferably, the initiator is a water-soluble thermal decomposition initiator, including persulfate and azo initiators; further preferably, the persulfate initiator includes at least one of ammonium persulfate and potassium persulfate, and the azo initiator includes azobisisobutylamidine hydrochloride.

[0015] Preferably, the emulsifier is an anionic emulsifier, a nonionic emulsifier or an anionic and nonionic composite emulsifier; the anionic emulsifier includes at least one of sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and tridecyl polyoxyethylene ether ammonium phosphate; the nonionic emulsifier includes reactive and non-reactive nonionic emulsifiers, wherein the reactive nonionic emulsifier includes at least one of ER-20 and ER-30; the non-reactive nonionic emulsifier includes at least one of AEO-9, LCN287, and LCN118.

[0016] Preferably, the pH adjuster includes at least one of sodium carbonate, sodium bicarbonate, hydrochloric acid, sodium hydroxide and ammonia water.

[0017] In some embodiments of the present invention, the acrylic ester polymer emulsion is prepared by a semi-continuous seed emulsion polymerization process; the semi-continuous seed emulsion polymerization process includes a core pre-emulsion and a shell pre-emulsion.

[0018] Preferably, the method for preparing the silicone-modified acrylate polymer emulsion comprises the following steps:

[0019] (1) dissolving a portion of the emulsifier in water, adding a portion of the vinyl monomer, mixing and stirring to obtain a nuclear pre-emulsion;

[0020] (2) dissolving another portion of the emulsifier in water, and then adding the remaining vinyl monomer and silicone monomer, mixing and stirring to obtain a shell pre-emulsion;

[0021] (3) mixing part of the emulsifier, pH adjuster and water, and preheating to 75-90° C.; adding 15-40 wt % of the core pre-emulsion and part of the aqueous solution of the initiator thereto, and continuing the reaction for 10-30 min after the blue light appears to obtain a seed emulsion, and then dripping the remaining core pre-emulsion for 25-60 min, and then keeping warm for 10-45 min to obtain a core emulsion;

[0022] (4) adding the shell pre-emulsion and the aqueous solution of the remaining initiator to the core emulsion for 60-100 min, keeping the temperature for 50-120 min, then cooling the temperature to below 45° C., adjusting the pH of the emulsion to 7-9, and filtering the material to obtain the organosilicon-modified acrylate polymer emulsion.

[0023] Preferably, in step (1), the mass ratio of the vinyl monomer, the emulsifier and the water is (10-30):1:(5-20); in step (2), the mass ratio of the vinyl monomer, the silicone monomer, the emulsifier and the water is (15-30):1:(0.5-1.5):(5-20).

[0024] Preferably, the mass ratio of the vinyl monomer in step (1) to the vinyl monomer in step (2) is 1:(1-3).

[0025] Preferably, the mass ratio of the core pre-emulsion in step (1) to the shell pre-emulsion in step (2) is 1:(1-4).

[0026] In the present invention, the solid content of the organosilicon-modified acrylate polymer emulsion is 30wt%-50wt%.

[0027] The second aspect of the present invention provides an anti-adhesion acrylate coating, which is prepared by coating the anti-adhesion acrylate coating on a substrate.

[0028] Preferably, the substrate comprises at least one of glass, wood, paper, fiber cement board and metal sheet.

[0029] The third aspect of the present invention provides a method for preparing the anti-adhesion acrylate coating, comprising the following steps: applying the anti-adhesion acrylate coating on a substrate, and drying at 40-120° C. for 1-10 hours to obtain the anti-adhesion acrylate coating.

[0030] A fourth aspect of the present invention provides an application of the anti-adhesion acrylic paint in the preparation of glass paint, wood paint, paper coating, architectural paint and metal paint.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The present invention utilizes an emulsion polymerization system to prepare an environmentally friendly anti-adhesion acrylic coating. The coating process has no VOC emissions, thus avoiding threats to biological and environmental safety, conforming to the trend of green development, and realizing the preparation of an environmentally friendly and environmentally friendly anti-adhesion functional coating.

[0033] The invention adopts a relatively traditional emulsion polymerization process, the raw materials are easily available, the cost is low, and large-scale industrial production is easy to achieve.

[0034] The coating of the present invention can be applied to various substrates such as glass, wood boards, paper sheets, fiber cement boards and metal sheets, and is expected to be used in technical fields such as glass baking varnish, wood paint, paper coating agent, architectural coating and metal paint.

[0035] The coating of the invention has good low adhesion and antifouling properties to water, oil and liquids with various complex components.

[0036] The coating of the invention has high transparency (visible light transmittance ≥ 85%).

[0037] The coating of the present invention has excellent hardness (pencil hardness can reach 2H) and adhesion (rated as level 0 by the cross-sectional method). BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a test diagram of the low adhesion antifouling performance of the composite emulsion coating of Example 4;

[0039] Figure 2 is an application diagram of the composite emulsion of Example 4 on various substrates;

[0040] Figure 3 It is a transparency test chart of the composite emulsion coating of Examples 1-6;

[0041] Figure 4 It is a hardness test diagram of the composite emulsion coating of Examples 1-6;

[0042] Figure 5 This is an adhesion test diagram of the composite emulsion coating of Example 4. DETAILED DESCRIPTION

[0043] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0044] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0045] Examples 1-6

[0046] In Examples 1-6, the organosilicon-modified acrylate polymer emulsion is prepared by the following steps:

[0047] (1) Add methyl methacrylate (5.632 g), styrene (5.280 g), isooctyl acrylate (5.632 g), and methacrylic acid (1.056 g) to 8.247 g of a 10 wt % RS610A25 emulsifier aqueous solution, stir at 500 rpm-800 rpm for 10-60 min until a milky white state is obtained, and disperse and emulsify to obtain a nuclear pre-emulsion for standby use;

[0048] (2) Methyl methacrylate (8.448 g), styrene (7.920 g), isooctyl acrylate (8.448 g), methacrylic acid (1.584 g), 3821F8 (1.320 g) was added to 12.989 g of 10 wt% RS610A25 emulsifier aqueous solution, stirred at 500 rpm-800 rpm for 20-90 min until it became milky white, dispersed and emulsified to obtain shell pre-emulsion, which was set aside;

[0049] (3) 25% of the nuclear pre-emulsion and 1.7573 g of a 5 wt % ammonium persulfate aqueous solution were added to 43.607 g of an aqueous solution containing 1 wt % sodium bicarbonate and 4 wt % RS610 A25 preheated to 83° C. After the aqueous solution turned blue, the solution was kept warm for 15-25 min, and then the remaining nuclear pre-emulsion and 1.1715 g of a 5 wt % ammonium persulfate aqueous solution were added dropwise at the same time. The addition time was 25-40 min, and the solution was kept warm for 10-30 min to obtain a nuclear emulsion;

[0050] (4) The shell pre-emulsion and 2.3431 g of 5 wt% ammonium persulfate initiator aqueous solution are simultaneously added dropwise to the core emulsion for 70-90 min. After the addition is completed, the mixture is kept warm for 60-90 min, then cooled to below 45° C., ammonia water is added dropwise to adjust the pH of the emulsion to 8-9, and the material is filtered to obtain the target synthesized organosilicon-modified acrylate polymer emulsion.

[0051] In Examples 1-6, the organosilicon-modified acrylate polymer emulsion and nano-silica sol are mixed according to the ratio in Table 1, and then applied to a substrate such as glass by scraping. The coating is pre-baked at 40-60° C. for 0-20 min, and then baked at 100-120° C. for 1-8 h to obtain an environmentally friendly anti-adhesion acrylate coating.

[0052] Table 1

[0053]

[0054] The following performance tests were performed on the anti-adhesion acrylate coatings prepared in Examples 1-6:

[0055] Test 1: Low adhesion and antifouling performance of coating

[0056] like Figure 1 As shown, the composite emulsion of Example 4 was scraped onto a glass sheet to prepare a coating, which was placed on a bracket with an inclination of 25°, and then high-surface-energy water, low-surface-energy n-hexadecane, common aqueous liquids in life such as cola and ink, common oily liquids such as pump oil and soybean oil, high-viscosity honey, and complex liquids composed of multiple ingredients such as soy sauce were dripped onto the surface of the coating respectively. These liquids were able to slide cleanly on the surface of the coating, indicating that the coating had low-adhesion and anti-fouling properties.

[0057] Test 2: Coating suitability for various substrates

[0058] like Figure 2As shown, the composite emulsion of Example 4 is scraped onto wood chips (Figure a), paper chips (Figure b), fiber cement boards (Figure c) and iron sheets (Figure d), and blue ink is dripped onto the coating surface at a certain inclination. There are slight ink stains on the wood chips, which may be caused by the barbed fibers on the wood chips, which cause slight ink stains after the ink slides off, but it can be easily rinsed clean with water and kept dry. On paper chips, fiber cement boards and iron sheets, the ink can easily slide off. It can be seen that the coating of the present invention can be applied to a variety of substrates such as glass, wood boards, paper chips, fiber cement boards and metal sheets, and imparts anti-adhesion and anti-fouling functions to the substrates, and is expected to be applied in technical fields such as glass paint, wood lacquer, paper coating agents, architectural coatings and metal paints.

[0059] Test 3: Transparency of coating

[0060] like Figure 3 As shown, the coatings of the above-mentioned Examples 1-6 are applied to a glass sheet (the upper half is coated with the coating, Examples 1-6 from left to right, and the lower half is an uncoated glass sheet), and it is placed on a map of a thousand miles of rivers and mountains. From the picture, it can be seen that the coated part does not affect the visual effect, and through a visible light transmittance test using an ultraviolet spectrophotometer, with a blank glass sheet as a control, the visible light transmittance of the glass coatings of Examples 1-6 is ≥85%, indicating that the coating has good transparency.

[0061] Test 4: Mechanical properties of coating

[0062] According to GB / T6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes", the hardness of the coatings of Examples 1-6 was tested. Figure 4 As shown in the figure, when the amount of silica sol added gradually increases from 0% (Example 1), 20% (Example 2), 40% (Example 3), to 60% (Example 4), the hardness of the coating also gradually increases from B (Example 1) to 2H (Example 4). According to GB / T9286-1998 "Scratching test for paint and varnish film", the adhesion of the coating of Example 4 is tested. Figure 5 As shown, compared with the coating before tape peeling (Figure a), the coating after tape peeling (Figure b) remains intact without falling off. According to the evaluation standard, it is level 0 with the best adhesion.

[0063] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. An anti-adhesion acrylic coating, characterized in that: The raw materials for preparing the coating include organic silicon modified acrylic ester polymer emulsion and nano silica sol.

2. The anti-adhesion acrylic coating according to claim 1, characterized in that: The raw materials for preparing the coating include 30-100 wt% of organic silicon modified acrylic ester polymer emulsion and 0-70 wt% of nano silica sol.

3. The anti-adhesion acrylic coating according to claim 1, characterized in that: The organosilicon-modified acrylate polymer emulsion is prepared by emulsion polymerization of vinyl monomer and organosilicon monomer in the presence of an initiator, an emulsifier, a pH regulator and water.

4. The anti-adhesion acrylic coating according to claim 3, characterized in that: The vinyl monomer includes at least one of acrylic acid, methacrylic acid, styrene, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, isobutyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, octadecyl methacrylate, octadecyl acrylate, lauryl acrylate, and lauryl methacrylate.

5. The anti-adhesion acrylic coating according to claim 3, characterized in that: The organic silicon monomer is vinyl modified silicone oil.

6. The anti-adhesion acrylic coating according to claim 3, characterized in that: The preparation method of the organosilicon-modified acrylate polymer emulsion comprises the following steps: (1) dissolving a portion of the emulsifier in water, adding a portion of the vinyl monomer, mixing and stirring to obtain a nuclear pre-emulsion; (2) dissolving another portion of the emulsifier in water, adding the remaining vinyl monomer and silicone monomer, mixing and stirring to obtain a shell pre-emulsion; (3) mixing part of the emulsifier, pH adjuster and water, and preheating to 75-90° C.; adding 15-40 wt % of the core pre-emulsion and part of the aqueous solution of the initiator thereto, and continuing the reaction for 10-30 min after the blue light appears to obtain a seed emulsion, and then dripping the remaining core pre-emulsion for 25-60 min, and then keeping warm for 10-45 min to obtain a core emulsion; (4) adding the shell pre-emulsion and the aqueous solution of the remaining initiator to the core emulsion for 60-100 min, keeping the temperature for 50-120 min, then cooling the temperature to below 45° C., adjusting the pH of the emulsion to 7-9, and filtering the material to obtain the organosilicon-modified acrylate polymer emulsion.

7. The anti-adhesion acrylic coating according to claim 6, characterized in that: In step (1), the mass ratio of the vinyl monomer, the emulsifier, and the water is (10-30):1:(5-20); in step (2), the mass ratio of the vinyl monomer, the silicone monomer, the emulsifier, and the water is (15-30):1:(0.5-1.5):(5-20).

8. The anti-adhesion acrylic coating according to claim 6, characterized in that: The solid content of the organosilicon-modified acrylate polymer emulsion is 30 wt %-50 wt %.

9. An anti-adhesion acrylic coating, characterized in that: The anti-adhesion acrylate coating according to any one of claims 1 to 8 is applied on a substrate.

10. Use of the anti-adhesion acrylic paint according to any one of claims 1 to 8 in the preparation of glass baking varnish, wood paint, paper coating agent, architectural paint and metal paint.

Citation Information

Patent Citations

  • Organosilicon-modified acrylate core-shell emulsion capable of filming at room temperature and preparation method as well as application thereof

    CN102391412A

  • Silicone-acrylate copolymer emulsion and preparation method thereof

    CN103772617A

  • Water-based waterproof acrylate emulsion and preparation method thereof

    CN104277172A

  • Aqueous paint composition and coating film

    CN108300090A

  • High-performance and environment-friendly nano-silicone acrylate outer wall coating and preparation method thereof

    CN109082189A