Copolymer composite nano drilling fluid as well as preparation method and application thereof
By modifying copper oxide nanorods and other materials to form NSD/M-CuO/lignite/phenolic copolymer nanofluid, combined with bentonite and water-based slurry, a drilling fluid that can withstand high temperatures and reduce fluid loss is produced, which solves the problem of drilling fluids under high temperatures. The problem of polymer degradation improves well wall stability and fluidity.
Patent Information
- Application Number
- CN202410795605.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-08
AI Technical Summary
The polymer molecular chains of existing drilling fluids are prone to degradation at high temperatures, resulting in the failure of the synergistic effect with clay, causing well wall cracks, and affecting well wall stability and drilling fluid performance.
Using the preparation method of copolymer composite nano-drilling fluid, a nano-graft copolymer is formed by modifying copper oxide nanorods and materials such as N-phenylmethacrylamide, styrene and dimethyldiallylammonium chloride. Sulfonated lignite and sulfonated phenolic resin are added to form NSD/M-CuO/lignite/phenolic copolymer nanofluid, which is combined with bentonite and water-based slurry to produce drilling fluid that can withstand high temperatures and reduce fluid loss.
Significantly improves the temperature resistance and fluid loss performance of drilling fluid at high temperatures, reduces solid insoluble matter, prevents clay from agglomerating, forms a thin and dense mud cake, reduces fluid loss, and improves the stability of the well wall and drilling fluid fluidity.
Smart Images

Figure CN118745338A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of drilling fluid development, and relates to a copolymer composite nano drilling fluid and a preparation method and application thereof. Background Art
[0002] The exploration and exploitation of oil and gas resources requires drilling. The drilling fluid can maintain the stability of the wellbore during the drilling process and effectively control fluid loss and filter cake quality. The polymer in the drilling fluid is adsorbed on the clay surface. The polymer's ability to protect the glue makes the clay particles aggregate to form a mud cake layer to stabilize the well wall. At the same time, the hydrophilic groups on the clay particle surface and the polymer molecular chain are hydrated to form a hydration film. The combined effect of the two further enhances the polymer's ability to protect the glue, reduces the filtration loss of the drilling fluid, and increases the rheological properties. As exploration and exploitation continue to develop into deep and complex formations, the probability of drilling in high temperature and high pressure formations is increasing.
[0003] However, under high temperature, the molecular chains of polymers in commonly used drilling fluids are prone to high temperature degradation and high temperature desorption, and the synergistic effect between polymers and clay fails, making it difficult to control the drilling fluid loss and rheological properties. It is necessary to add more polymers to maintain the drilling fluid performance, which increases the cost of drilling. In addition, due to the failure of the synergistic effect between polymers in traditional drilling fluids and clay at high temperatures, the drilling fluid performance changes dramatically, such as high temperature thickening, high temperature viscosity reduction, increased filtration loss and thickening of mud cake, resulting in a large number of micron- and nano-scale cracks. These cracks not only affect the performance of the drilling fluid, but also threaten the stability of the well wall. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a copolymer composite nano drilling fluid and a preparation method and application thereof, thereby solving the technical problems in the prior art that the polymer in the drilling fluid is easily degraded at high temperature, the synergistic effect between the polymer and the clay fails, resulting in cracks in the well wall and affecting the stability of the well wall.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a copolymer composite nano-drilling fluid comprises the following steps:
[0007] S1: adding a double bond coupling agent to an organic dispersion of copper oxide nanorods, stirring and mixing the mixture evenly, and then performing a reflux reaction to obtain copper oxide nanorods modified with the double bond coupling agent;
[0008] S2: N-phenylmethyl acrylamide, styrene and dimethyl diallyl ammonium chloride are dispersed in water, and after adjusting the pH value of the system, the copper oxide nanorods modified by the double bond coupling agent are added, and the mixture is stirred and dispersed uniformly, and then the reaction system is placed under a nitrogen atmosphere, and after continuous stirring, an initiator is added to the system, and after stirring and reacting, sulfonated lignite and sulfonated phenolic resin are added to continue the reaction, and finally, an anion salt is added, and the mixture is stirred and reacted to obtain NSD / M-CuO / lignite / phenolic copolymer nanofluid;
[0009] S3: After mixing bentonite with water, potassium carbonate is added to prepare a water-based slurry, and the mixture is aged to prepare an aged water-based slurry. The NSD / M-CuO / lignite / phenolic copolymer nanofluid is added to the aged water-based slurry and stirred to prepare the copolymer composite nano drilling fluid.
[0010] Preferably, the preparation process of the copper oxide nanorods is: copper salt and alkali solution are uniformly mixed, after hydrothermal reaction, calcined in air atmosphere to obtain the copper oxide nanorods.
[0011] Preferably, the temperature of the hydrothermal reaction is 130-180° C., and the time is 3-4 hours; the temperature of the calcination is 450-600° C., and the time is 1-4 hours.
[0012] Preferably, the copper oxide nanorods have a diameter of 8 to 30 nm and a length of 3 to 12 μm.
[0013] Preferably, in step S1, the reaction temperature of the reflux reaction is 50-100° C., and the reaction time is 2-5 h.
[0014] Preferably, in step S1, the double bond coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, tri(isoallyloxy)vinylsilane, vinyltri(2-methoxyethoxy)silane, and vinyltriethoxysilane.
[0015] Preferably, in step S1, the ratio of the copper oxide nanorods to the double bond coupling agent is (0.1-1):(0.5-5) by mass.
[0016] Preferably, in step S3, the ratio of bentonite, water and NSD / M-CuO / lignite / phenolic copolymer nanofluid is (4-10):(100-500):(1.5-3.5) by weight.
[0017] A copolymer composite nano drilling fluid is prepared by the above method.
[0018] The above-mentioned copolymer composite nano drilling fluid is used in drilling.
[0019] Compared with the prior art, the present invention has the following beneficial technical effects:
[0020] The invention discloses a preparation method of a copolymer composite nano drilling fluid. The preparation method uses a coupling agent containing a diene bond to modify copper oxide nano rods. CuO has excellent high temperature and high pressure resistance properties. The diene bond can self-polymerize to form a nano graft copolymer with N-phenylmethyl acrylamide (N-PhAM), styrene (ST) and dimethyldiallyl ammonium chloride (DMDAAC) and the copper oxide nano rods. The cyclic rigid groups contained in the two monomers of N-PhAM and ST can make the polymer have good temperature resistance. Anionic salt, sulfonated lignite and nano fluid sulfonated into phenolic resin are added to further improve the high temperature resistance and fluid loss reduction performance. The sulfonated lignite can effectively control the fluid loss and viscosity of the drilling fluid, and the sulfonated phenolic resin can reduce the fluid loss of the drilling fluid under high temperature and high pressure conditions. On the one hand, nanofluids can improve the viscosity of drilling fluids and maintain stability at higher temperatures. On the other hand, they can enhance the interface between polymers and nanofillers, so that they are evenly dispersed in the completion fluid of the water system without precipitation, thereby giving full play to their functions of enhancement, high temperature resistance and filtration loss reduction. Secondly, the rod-like structure of nano CuO can effectively improve the support of drilling fluids for clay layers. At the same time, nanofluid particles enter the nano-scale pores of shale by adsorption, ensuring the synergistic effect between polymers and clay, and further reducing the filtration loss of drilling fluids. The present invention uses modified CuO nanorods grafted with polymers to make polymer nanofluids. This nanofluid can reduce the amount of solid insolubles. In addition, it has excellent compatibility with other formation fluids. The connection between it and clay effectively prevents pollution, reduces the aggregation of clay, makes the particle size distribution of clay particles wider, forms a thin and dense mud cake, and enhances the high-temperature filtration loss performance of drilling fluids. Secondly, nanoparticles enter the nano-scale pores of shale by adsorption, reducing the filtration loss of drilling fluids. The rod-like structure can better support the clay layer, thereby further reducing the filtration loss. The thermal weight loss temperature of the drilling fluid under air atmosphere is increased to 300-500°C, the API filtration loss is ≤1.5mL, the HTHP filtration loss is ≤6mL, the API filtration loss cement cake thickness is 0.3-0.7mm, while the HTHP filtration loss cement cake thickness is less than 1.5mm, and the solid insoluble matter is ≤3.5%. The entire preparation process of the high temperature resistant filtration loss reduction drilling fluid provided by the present invention has mild conditions, is simple and easy to control, has low cost, is easy to scale up, and can still function under high temperature and high pressure.
[0021] Furthermore, the preparation process of the copper oxide nanorods is: copper salt and alkali solution are mixed evenly, after hydrothermal reaction, calcined in an air atmosphere to obtain the copper oxide nanorods. This method for preparing copper oxide nanorods has the advantages of being simple, low-cost, controllable in morphology, high in purity and environmentally friendly.
[0022] Furthermore, the hydrothermal reaction temperature is 130-180°C and the time is 3-4 hours, so that the copper salt can fully react to form copper hydroxide nanoparticles. The calcination temperature is 450-600°C and the time is 1-4 hours, so that the copper hydroxide nanoparticles undergo crystal phase transformation and thermal decomposition during the high-temperature calcination process, and the copper hydroxide is converted into copper oxide nanorods.
[0023] Furthermore, the copper oxide nanorods have a diameter of 8 to 30 nm and a length of 3 to 12 μm, which can make the copper oxide nanorods with this morphology and structure have a higher aspect ratio, which is conducive to increasing the probability of contact with each other, building a faster heat transfer network, and improving its high temperature resistance. At the same time, it can better support the clay layer and reduce the filtration loss.
[0024] Furthermore, in step S1, the reaction temperature of the reflux reaction is 50-100° C., and the reaction time is 2-5 hours. The reflux operation in step S1 can promote the reaction, control the reaction conditions and uniformly heat the process of coupling agent modification of copper oxide nanorods, which is helpful to obtain high-quality modified copper oxide nanorod products.
[0025] Further, in step S1, the double bond coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, tri(isoallyloxy)vinylsilane, vinyltri(2-methoxyethoxy)silane, and vinyltriethoxysilane, so that the double bond portion of the double bond coupling agent in step S1 can be chemically or physically adsorbed with the active hydroxyl groups on the surface of the copper oxide nanorods to form a stable cross-linked network. This cross-linking can enhance the stability and antioxidant capacity of the copper oxide nanorods and prevent them from being oxidized or degraded in the environment. In addition, the double bond coupling agent can also provide more functional groups for further modification, giving the copper oxide nanorods more functions, etc., to facilitate subsequent self-polymerization reactions.
[0026] Furthermore, in step S1, the ratio of the copper oxide nanorods to the double bond coupling agent is (0.1-1):(0.5-5) by weight, so that the ratio of each material in step S1 can effectively improve the dispersibility of the copper oxide nanorods, prevent their agglomeration and precipitation, and also enhance their interfacial compatibility with other materials, which is conducive to further functionalization treatment.
[0027] Furthermore, in step S3, the ratio of bentonite, water and NSD / M-CuO / lignite / phenolic copolymer nanofluid is (4-10):(100-500):(1.5-3.5) by weight, so that the ratio of each material in step S3 can make the nanoparticles evenly dispersed, prevent agglomeration and precipitation, and also make the nanofluid have better flow properties and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a schematic diagram of a process for preparing a copolymer composite nano-drilling fluid in the present invention;
[0030] Figure 2 The thermogravimetric test diagrams of Examples 1 and 2 are shown. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0032] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0033] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0034] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0035] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0036] like Figure 1 As shown, the present invention provides a method for preparing a copolymer composite nano-drilling fluid, which specifically comprises the following steps:
[0037] 1) Preparation of modified M-CuO nanorods
[0038] First, by weight, 0.1-1 parts of copper salt are added to 100 parts of 0.1-1 parts of alkali solution, mixed evenly, and placed in a hydrothermal kettle with a volume capacity of 120 parts to react at 130-180°C for 3-4 hours. Secondly, the product obtained by the reaction is vacuum dried at 80-150°C, and calcined at 450-600°C in an air atmosphere for 1-4 hours to obtain copper oxide (CuO) nanorods. Next, the prepared 0.1-1 parts of CuO nanorods are uniformly dispersed in 50-200 parts of ethanol, and then mixed and stirred evenly with 0.5-5 parts of a coupling agent containing a double bond, and then refluxed and condensed at 50-100°C for 2-5 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0039] Wherein, the copper salt is one or more of copper nitrate, copper sulfate and copper acetate;
[0040] The alkali in the alkali solution is one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ethylenediamine, hydrazine hydrate and urea;
[0041] The double bond coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, tri(isoallyloxy)vinylsilane, vinyltri(2-methoxyethoxy)silane and vinyltriethoxysilane.
[0042] The diameter of the prepared copper oxide nanorod is 8-30nm and the length is 3-12μm.
[0043] 2) Preparation of NSD / M-CuO / lignite / phenolic copolymer nanofluid
[0044] First, by weight, 10 to 30 parts of N-phenylmethylacrylamide (N-PhAM), 3 to 20 parts of styrene (ST) and 5 to 10 parts of dimethyldiallylammonium chloride (DMDAAC) are mixed evenly in 100 to 200 parts of water, and a certain concentration of alkali solution is added to adjust the pH of the system to 7 to 9, and then 0.5 to 5 parts of M-CuO are added and stirred until uniformly dispersed, and heated at 60 to 100°C for 10 to 30 minutes under a nitrogen atmosphere. The main purpose of the reaction under a nitrogen atmosphere in this step is to protect the reactants and products in the reaction system from the influence of oxygen. Oxygen will induce some unnecessary oxidation reactions, resulting in a decrease in the purity and yield of the product. Secondly, 0.02 to 0.08 parts of initiator are continued to be added to the above solution, and the reaction is maintained for 4 to 6 hours. Then, 2 to 4 parts of sulfonated lignite and 5 to 8 parts of sulfonated phenolic resin are added to the reactants and the reaction is continued for 3 to 5 hours. Finally, 1 to 10 parts of anion salt are added to the above reactants, and the reaction is stirred for 10 to 30 hours. The product is vacuum distilled at 60°C to obtain N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid, namely NSD / M-CuO / lignite / phenolic copolymer nanofluid.
[0045] Wherein, the alkali solution used to adjust the pH value of the system is one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium bicarbonate and sodium bicarbonate;
[0046] The initiator is one or more of ammonium persulfate, sodium bisulfite and azobisisobutylamidine hydrochloride;
[0047] The anion salt is one or more of sodium fluoroborate, sodium tetrachloroaluminate, sodium hexafluorophosphate, sodium acetate, sodium toluenesulfonate, sodium methanesulfonate, sodium alkyl sulfate, and sodium serine;
[0048] 3) Preparation of drilling fluid
[0049] First, 4 to 10 parts of bentonite are dispersed in 100 to 500 parts of water by weight, and then 0.25 to 1 part of potassium carbonate is added and stirred for 10 to 40 minutes to obtain a water-based slurry. Then, the water-based slurry is aged at room temperature for 20 to 30 hours. Finally, 1.5 to 3.5 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid is added to the water-based slurry and stirred for 1 to 3 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0050] Wherein, the bentonite is one or more of sodium-based bentonite, calcium-based bentonite, hydrogen-based bentonite and organic bentonite;
[0051] In addition, the present invention also discloses a copolymer composite nano drilling fluid prepared by the above method. After testing, the thermal weight loss of the drilling fluid prepared by the present invention is 300-500°C, the API filtration loss is ≤1.5mL, the HTHP filtration loss is ≤6mL, the API filtration loss cement cake thickness is 0.3-0.7mm, and the HTHP filtration loss cement cake thickness is less than 1.5mm. It can be seen that the high temperature resistant and low filtration loss nano composite drilling fluid has excellent high temperature resistance and filtration loss reduction capabilities. Even after a series of hot rolling aging, its HTHP filtration loss changes very little, and still does not lose high temperature resistance and filtration loss reduction. The thermal weight loss (TWL) of the drilling fluid refers to the mass lost by certain components in the drilling fluid due to thermal decomposition, evaporation or chemical reaction under high temperature conditions. The API filtration loss is also called static filtration loss, which refers to the amount of water lost by the drilling fluid through a filtration area with a diameter of 75mm within 30 minutes under normal temperature and a certain pressure difference (about 0.689MPa). This measurement standard is mainly used to evaluate the performance of drilling fluids under specific conditions, especially in preventing wellbore instability and protecting oil and gas formations. HTHP fluid loss, or High Temperature and High Pressure Fluid Loss, refers to the volume of filtrate that passes through the filter medium and the mud cake formed under high temperature (usually the temperature is specified in brackets, such as HTHP (100) represents 100 degrees Celsius) and high pressure (pressure is generally 3.5 atmospheres, divided into upper pressure 4.2 and lower pressure 0.7) conditions. The smaller the HTHP fluid loss of the drilling fluid, the easier it is to form a low-permeability, flexible, thin and dense filter cake, which is conducive to stabilizing the wellbore and protecting the oil and gas formations.
[0052] The invention discloses a method for preparing a high-temperature resistant filtration loss reducing drilling fluid. The method comprises the following steps: modifying copper oxide nanorods with a coupling agent containing diene bonds, mixing the modified copper oxide nanorods with N-phenylmethacrylamide (N-PhAM), styrene (ST), dimethyldiallyl ammonium chloride (DMDAAC), anionic salt sulfonated lignite and sulfonated phenolic resin to prepare N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid, and finally uniformly mixing the modified copper oxide nanorods with water-based slurry to prepare the copolymer composite nano drilling fluid. The prepared drilling fluid has the characteristics of high temperature resistance and reduced filtration loss, among which nano CuO has excellent high temperature and high pressure resistance. At the same time, CuO nanorods can effectively improve the support of the drilling fluid for the clay layer. The cyclic rigid groups contained in the two monomers N-PhAM and ST can make the drilling fluid have good temperature resistance. In addition, this nanofluid can reduce the amount of solid insolubles and has excellent compatibility with other formation fluids. The connection between it and clay effectively prevents pollution, reduces the aggregation of clay, makes the particle size distribution of clay particles wider, forms a thin and dense mud cake, ensures the synergistic effect between polymer and clay, and enhances the high temperature filtration loss performance of the drilling fluid. At the same time, the nanoparticles of the nanofluid enter the nano-scale pores of the shale through adsorption, further reducing the filtration loss. In addition, the drilling fluid has the advantages of mild preparation process conditions, simple and easy control, low cost, and easy scale-up preparation.
[0053] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0054] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0055] Example 1
[0056] 1) Preparation of modified M-CuO nanorods
[0057] First, 0.1 parts of nitrate are added to 100 parts of an aqueous solution containing 0.1 parts of potassium carbonate, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 130°C for 3 hours. Secondly, the product obtained by the reaction is vacuum dried at 80°C and calcined in an air atmosphere at 450°C for 4 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods are uniformly dispersed in 50 parts of ethanol, mixed and stirred evenly with 0.5 parts of tri(isoallyloxy)vinylsilane, and then refluxed and condensed at 50°C for 5 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0058] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid
[0059] First, 10 parts of N-phenylmethylacrylamide (N-PhAM), 3 parts of styrene (ST) and 5 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 100 parts of water, and a certain concentration of sodium hydroxide solution was added to adjust the pH of the system to 7, and then 0.5 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 60°C for 30 minutes under a nitrogen atmosphere. Secondly, 0.02 parts of initiator were added to the above solution, and the reaction was maintained for 4 hours. Then, 4 parts of sulfonated lignite and 5 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 1 part of anionic salt was added to the above reactants, and the reaction was stirred for 10 hours. After the product was vacuum distilled at 60°C, N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was obtained.
[0060] 3) Preparation of drilling fluid
[0061] First, 4 parts of bentonite were dispersed in 100 parts of water, and then 0.25 parts of potassium carbonate were added and stirred for 10 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 20 hours. Finally, 1.5 parts of N-PhAM / ST / DMDAAC / M-CuO copolymer nanofluid was added to the water-based slurry and stirred for 1 hour to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0062] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 380°C, API filtration loss = 1.5mL, HTHP filtration loss = 5.7mL, API loss cement cake thickness was 0.7mm, and HTHP loss cement cake thickness was equal to 1.3mm.
[0063] Example 2
[0064] 1) Preparation of modified M-CuO nanorods
[0065] First, 1 part of nitrate is added to 100 parts of an aqueous solution containing 1 part of sodium carbonate, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 180°C for 3 hours. Secondly, the product obtained by the reaction is vacuum dried at 150°C and calcined at 600°C in an air atmosphere for 1 hour to obtain copper oxide (CuO) nanorods with an outer diameter of 10nm and a length of 12μm. Next, the prepared CuO nanorods are uniformly dispersed in 200 parts of ethanol, and then mixed and stirred evenly with 5 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and then refluxed and condensed at 75°C for 4 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0066] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid
[0067] First, 30 parts of N-phenylmethylacrylamide (N-PhAM), 20 parts of styrene (ST) and 10 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 200 parts of water, and a certain concentration of potassium hydroxide solution was added to adjust the pH of the system to 7-9, and then 5 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 100°C for 12 minutes under a nitrogen atmosphere. Secondly, 0.08 parts of ammonium persulfate were added to the above solution, and the reaction was maintained for 6 hours. Then, 4 parts of sulfonated lignite and 6 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 5 hours. Finally, 10 parts of sodium fluoroborate were added to the above reactants, and the reaction was stirred for 30 hours. After the product was vacuum distilled at 60°C, N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was obtained.
[0068] 3) Preparation of drilling fluid
[0069] First, 10 parts of bentonite were dispersed in 250 parts of water, and then 1 part of potassium carbonate was added and stirred for 40 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 30 hours. Finally, 3.5 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was added to the water-based slurry and stirred for 1 hour to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0070] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 470°C, API filtration loss = 0.3mL, HTHP filtration loss = 1.7mL, API loss cement cake thickness was 0.3mm, and HTHP loss cement cake thickness was equal to 0.8mm.
[0071] Example 3
[0072] 1) Preparation of modified M-CuO nanorods
[0073] First, 0.3 parts of nitrate are added to 100 parts of an aqueous solution containing 3 parts of ethylenediamine and 0.3 parts of hydrazine hydrate, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 130°C for 3 hours. Secondly, the product obtained by the reaction is vacuum dried at 100°C and calcined at 500°C in an air atmosphere for 2 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 30nm and a length of 12μm. Next, the prepared CuO nanorods are uniformly dispersed in 90 parts of ethanol, and then mixed and stirred evenly with 1.5 parts of γ-methacryloxypropyltrimethoxysilane (KH570), and then refluxed and condensed at 70°C for 3 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0074] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid
[0075] First, 17 parts of N-phenylmethylacrylamide (N-PhAM), 13 parts of styrene (ST) and 3 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 150 parts of water, and a certain concentration of potassium hydroxide solution was added to adjust the pH of the system to 8, and then 0.3 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 60°C for 10 minutes under a nitrogen atmosphere. Secondly, 0.03 parts of initiator were added to the above solution, and the reaction was maintained for 4 hours. Then, 2 parts of sulfonated lignite and 6 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 3 parts of anionic salt were added to the above reactants, and the reaction was stirred for 15 hours. After the product was vacuum distilled at 60°C, N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was obtained.
[0076] 3) Preparation of drilling fluid
[0077] First, 5 parts of bentonite were dispersed in 125 parts of water, and then 0.25 parts of potassium carbonate were added and stirred for 10 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 24 hours. Finally, 1.8 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was added to the water-based slurry and stirred for 1.5 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0078] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 390°C, API filtration loss = 1.3 mL, HTHP filtration loss = 5.0 mL, API loss cement cake thickness was 0.5 mm, and HTHP loss cement cake thickness was equal to 1.2 mm.
[0079] Example 4
[0080] 1) Preparation of modified M-CuO nanorods
[0081] First, 0.4 parts of sulfate are added to 100 parts of an aqueous solution containing 0.4 parts of sodium hydroxide, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 170°C for 4 hours. Secondly, the product obtained by the reaction is vacuum dried at 90°C and calcined at 470°C in an air atmosphere for 3 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods are uniformly dispersed in 120 parts of ethanol, mixed and stirred evenly with 2 parts of tri(isoallyloxy)vinylsilane, and then refluxed and condensed at 70°C for 5 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0082] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO nanofluids
[0083] First, 19 parts of N-phenylmethylacrylamide (N-PhAM), 12 parts of styrene (ST) and 4 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 130 parts of water, and a certain concentration of sodium bicarbonate solution was added to adjust the pH of the system to 9, and then 0.4 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 90°C for 30 minutes under a nitrogen atmosphere. Secondly, 0.05 parts of initiator were added to the above solution, and the reaction was maintained for 6 hours. Then, 3 parts of sulfonated lignite and 6 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 4 parts of anionic salt were added to the above reactants, and the reaction was stirred for 13 hours. After the product was vacuum distilled at 60°C, N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was obtained.
[0084] 3) Preparation of drilling fluid
[0085] First, 6 parts of bentonite were dispersed in 150 parts of water, and then 0.4 parts of potassium carbonate were added and stirred for 30 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 24 hours. Finally, 2 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid were added to the water-based slurry and stirred for 3 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0086] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 400°C, API filtration loss = 1.0 mL, HTHP filtration loss = 3.5 mL, API loss cement cake thickness was 0.5 mm, and HTHP loss cement cake thickness was equal to 1.0 mm.
[0087] Example 5
[0088] 1) Preparation of modified M-CuO nanorods
[0089] First, 0.5 parts of sulfate are added to 100 parts of an aqueous solution containing 0.1 parts of sodium nitrate, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 150°C for 4 hours. Secondly, the product obtained by the reaction is vacuum dried at 120°C and calcined at 500°C in an air atmosphere for 4 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods are uniformly dispersed in 150 parts of ethanol, mixed and stirred evenly with 2.5 parts of vinyl tris (2-methoxyethoxy) silane, and then refluxed and condensed at 60°C for 4 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 90°C in vacuum for 2 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0090] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO nanofluids
[0091] First, 21 parts of N-phenylmethylacrylamide (N-PhAM), 15 parts of styrene (ST) and 5 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 150 parts of water, and a certain concentration of sodium bicarbonate solution was added to adjust the pH of the system to 8, and then 0.5 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 80°C for 30 minutes under a nitrogen atmosphere. Secondly, 0.05 parts of initiator were added to the above solution, and the reaction was maintained for 6 hours. Then, 4 parts of sulfonated lignite and 6 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 5 parts of anionic salt were added to the above reactants, and the reaction was stirred for 14 hours. After the product was vacuum distilled at 60°C, N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was obtained.
[0092] 3) Preparation of drilling fluid
[0093] First, 7 parts of bentonite were dispersed in 175 parts of water, and then 0.45 parts of potassium carbonate were added and stirred for 30 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 26 hours. Finally, 2.2 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was added to the water-based slurry and stirred for 2 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0094] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / DMDAAC / M-CuO / lignite / phenolic drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 415°C, API filtration loss = 0.8mL, HTHP filtration loss = 3.0mL, API loss cement cake thickness was 0.5mm, and HTHP loss cement cake thickness was equal to 0.9mm.
[0095] Example 6
[0096] 1) Preparation of modified M-CuO nanorods
[0097] First, 0.6 parts of sulfate are added to 100 parts of an aqueous solution containing 0.6 parts of potassium hydroxide, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 180°C for 3 hours. Secondly, the product obtained by the reaction is vacuum dried at 100°C and calcined at 500°C in an air atmosphere for 3 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods are uniformly dispersed in 180 parts of ethanol, mixed and stirred evenly with 3 parts of vinyl tris (2-methoxyethoxy) silane, and then refluxed and condensed at 70°C for 4 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0098] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO nanofluids
[0099] First, 25 parts of N-phenylmethylacrylamide (N-PhAM), 19 parts of styrene (ST) and 6 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 150 parts of water, and a certain concentration of potassium bicarbonate solution was added to adjust the pH of the system to 8, and then 0.5 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 70°C for 30 minutes under a nitrogen atmosphere. Secondly, 0.06 parts of initiator were added to the above solution, and the reaction was maintained for 4 hours. Then, 3 parts of sulfonated lignite and 7 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 6 parts of anionic salt were added to the above reactants, stirred and reacted for 20 hours, and the product was vacuum distilled at 60°C to obtain N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid.
[0100] 3) Preparation of drilling fluid
[0101] First, 8 parts of bentonite were dispersed in 200 parts of water, and then 0.5 parts of potassium carbonate were added and stirred for 40 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 24 hours. Finally, 2.5 parts of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid were added to the water-based slurry and stirred for 3 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0102] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / DMDAAC / M-CuO drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 435°C, API filtration loss = 0.8 mL, HTHP filtration loss = 1.9 mL, API loss cement cake thickness was 0.6 mm, and HTHP loss cement cake thickness was equal to 0.8 mm.
[0103] Example 7
[0104] 1) Preparation of modified M-CuO nanorods
[0105] First, 0.4 parts of acetate are added to 100 parts of an aqueous solution containing 0.4 parts of urea, mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts to react at 140°C for 3.5 hours. Secondly, the product obtained by the reaction is vacuum dried at 120°C and calcined at 500°C in an air atmosphere for 3 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods are evenly dispersed in 120 parts of ethanol, mixed and stirred evenly with 2 parts of vinyltriethoxysilane, and then refluxed and condensed at 80°C for 2.5 hours. After the reaction is completed, it is filtered and washed with anhydrous ethanol. Finally, it is dried at 60°C in vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0106] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO nanofluids
[0107] First, 13 parts of N-phenylmethylacrylamide (N-PhAM), 11 parts of styrene (ST) and 7 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 100 parts of water, and a certain concentration of potassium hydroxide solution was added to adjust the pH of the system to 7, and then 0.4 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 80°C for 25 minutes under a nitrogen atmosphere. Secondly, 0.05 parts of initiator were added to the above solution, and the reaction was maintained for 5 hours. Then, 3 parts of sulfonated lignite and 5 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 2.5 hours. Finally, 7 parts of anionic salt were added to the above reactants, stirred and reacted for 24 hours, and the product was vacuum distilled at 60°C to obtain N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid.
[0108] 3) Preparation of drilling fluid
[0109] First, 4 parts of bentonite were dispersed in 100 parts of water, and then 0.3 parts of potassium carbonate were added and stirred for 30 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 24 hours. Finally, 3 parts of N-PhAM / ST / DMDAAC / M-CuO copolymer nanofluid were added to the water-based slurry and stirred for 1 hour to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0110] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / DMDAAC / M-CuO drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 450°C, API filtration loss = 0.5mL, HTHP filtration loss = 2.5mL, API loss cement cake thickness was 0.6mm, and HTHP loss cement cake thickness was equal to 0.6mm.
[0111] Example 8
[0112] 1) Preparation of modified M-CuO nanorods
[0113] First, 0.2 acetate was added to 100 parts of an aqueous solution containing 0.2 parts of urea and mixed evenly, and then placed in a hydrothermal autoclave with a volume capacity of 120 parts and reacted at 160°C for 3 hours. Secondly, the product obtained by the reaction was vacuum dried at 100°C and calcined at 520°C in an air atmosphere for 3 hours to obtain copper oxide (CuO) nanorods with an outer diameter of 15nm and a length of 3μm. Next, the prepared CuO nanorods were evenly dispersed in 60 parts of ethanol, mixed and stirred evenly with 1 part of vinyltriethoxysilane, and then refluxed and condensed at 60°C for 4 hours. After the reaction was completed, it was filtered and washed with anhydrous ethanol. Finally, it was dried at 60°C under vacuum for 4 hours to obtain coupling agent-modified copper oxide nanorods (M-CuO).
[0114] 2) Preparation of N-PhAM / ST / DMDAAC / M-CuO nanofluids
[0115] First, 24 parts of N-phenylmethylacrylamide (N-PhAM), 14 parts of styrene (ST) and 4 parts of dimethyldiallylammonium chloride (DMDAAC) were mixed evenly in 100 parts of water, and a certain concentration of sodium bicarbonate solution was added to adjust the pH of the system to 7, and then 0.2 parts of M-CuO were added and stirred until uniformly dispersed, and heated at 70°C for 30 minutes under a nitrogen atmosphere. Secondly, 0.03 parts of initiator were added to the above solution, and the reaction was maintained for 5 hours. Then, 4 parts of sulfonated lignite and 5 parts of sulfonated phenolic resin were added to the reactants and the reaction was continued for 3 hours. Finally, 4 parts of anionic salt were added to the above reactants, stirred and reacted for 26 hours, and the product was vacuum distilled at 60°C to obtain N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid.
[0116] 3) Preparation of drilling fluid
[0117] First, 4 parts of bentonite were dispersed in 100 parts of water, and then 0.2 parts of potassium carbonate were added and stirred for 30 minutes to obtain a water-based slurry. Then, the water-based slurry was aged at room temperature for 25 hours. Finally, 1 part of N-PhAM / ST / DMDAAC / M-CuO / lignite / phenolic copolymer nanofluid was added to the water-based slurry and stirred for 1.5 hours to obtain a high temperature resistant and low filtration loss nanocomposite drilling fluid.
[0118] The performance of the obtained high temperature resistant and low filtration loss nano-composite drilling fluid N-PhAM / DMDAAC / M-CuO drilling fluid was tested, and the results showed that its thermal weight loss temperature started from 460°C, API filtration loss = 0.7 mL, HTHP filtration loss = 2.7 mL, API loss cement cake thickness was 0.4 mm, and HTHP loss cement cake thickness was equal to 0.7 mm.
[0119] Figure 2 It is the thermal weight loss test diagram of Example 1 and Example 2, that is, the thermal weight loss test diagram of Example 1 and Example 2. It can be seen from the figure that the thermal weight loss temperature of the drilling fluid in Example 1 is 380 degrees, and the thermal weight loss temperature of the drilling fluid in Example 2 is 470 degrees. It can be concluded that the high-temperature resistant drilling fluid prepared in this patent has high temperature resistance.
[0120] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a copolymer composite nano-drilling fluid, characterized in that: The following steps are involved: S1: adding a double bond coupling agent to an organic dispersion of copper oxide nanorods, stirring and mixing the mixture evenly, and then performing a reflux reaction to obtain copper oxide nanorods modified with the double bond coupling agent; S2: N-phenylmethyl acrylamide, styrene and dimethyl diallyl ammonium chloride are dispersed in water, and after adjusting the pH value of the system, the copper oxide nanorods modified by the double bond coupling agent are added, and the mixture is stirred and dispersed uniformly, and then the reaction system is placed under a nitrogen atmosphere, and after continuous stirring, an initiator is added to the system, and after stirring and reacting, sulfonated lignite and sulfonated phenolic resin are added to continue the reaction, and finally, an anion salt is added, and the mixture is stirred and reacted to obtain NSD / M-CuO / lignite / phenolic copolymer nanofluid; S3: After mixing bentonite with water, potassium carbonate is added to prepare a water-based slurry, and the mixture is aged to prepare an aged water-based slurry. The NSD / M-CuO / lignite / phenolic copolymer nanofluid is added to the aged water-based slurry and stirred to prepare the copolymer composite nano drilling fluid.
2. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: The preparation process of the copper oxide nanorods is as follows: copper salt and alkali solution are mixed evenly, and after hydrothermal reaction, calcination is carried out in an air atmosphere to obtain the copper oxide nanorods.
3. The method for preparing a copolymer composite nano-drilling fluid according to claim 2, characterized in that: The temperature of the hydrothermal reaction is 130-180° C., and the time is 3-4 hours; the temperature of the calcination is 450-600° C., and the time is 1-4 hours.
4. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: The copper oxide nanorod has a diameter of 8 to 30 nm and a length of 3 to 12 μm.
5. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: In step S1, the reaction temperature of the reflux reaction is 50-100° C., and the reaction time is 2-5 h.
6. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: In step S1, the double bond coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, tri(isoallyloxy)vinylsilane, vinyltri(2-methoxyethoxy)silane, and vinyltriethoxysilane.
7. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: In step S1, the ratio of the copper oxide nanorods to the double bond coupling agent is (0.1-1):(0.5-5) by mass.
8. The method for preparing a copolymer composite nano-drilling fluid according to claim 1, characterized in that: In step S3, the ratio of bentonite, water and NSD / M-CuO / lignite / phenolic copolymer nanofluid is (4-10):(100-500):(1.5-3.5) by weight.
9. A copolymer composite nano drilling fluid, characterized in that: It is prepared by the method according to any one of claims 1 to 8.
10. Use of the copolymer composite nano-drilling fluid as claimed in claim 9 in drilling.