Cooperative utilization method of waste plastic barrel and slag steel

By forming a composite of small slag steel and waste plastic particles, and using hot-pressing treatment and insulation room cooling technology, the problem of difficulty in putting waste plastic barrels and slag steel into the furnace has been solved, achieving harmless disposal and resource utilization, and reducing costs. Disposal costs and streamlined processes.

CN118745508APending Publication Date: 2024-10-08武汉钢铁有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410782435.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Waste plastic barrels and slag steel are difficult to effectively utilize in the iron and steel metallurgical process, resulting in high disposal costs and waste of resources, and the existing technology has a greater impact on coke oven production and coke quality.

Method used

The small slag steel and waste plastic particles are formed into a composite body through hot-pressing treatment. The heat of the slag steel is used to melt the plastic particles and cooled in the insulation chamber to form a steel-plastic composite charge, which is used in the steelmaking process and combines lime insulation rings and asbestos. Insulated panels to control temperature and heat transfer.

Benefits of technology

It achieves harmless disposal and resource utilization of waste plastic barrels and slag steel, reduces external disposal costs, simplifies the process, avoids adverse effects on coke oven production, and saves energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745508A_ABST
    Figure CN118745508A_ABST
Patent Text Reader

Abstract

The invention discloses a cooperative utilization method of waste plastic barrels and slag steel, which comprises the following steps: heating small slag steel to about 600-800 DEG C, and keeping for 5-10 minutes; loading into a hot-pressing annular mold, and carrying out hot-pressing treatment to obtain a slag steel hot-pressing ring; naturally cooling the slag steel hot-pressing ring to 600-700 DEG C, then horizontally placing the slag steel hot-pressing ring on an asbestos heat-insulating plate, putting a lime heat-insulating ring into the inner side of the slag steel hot-pressing ring, and filling a cavity in the lime heat-insulating ring with plastic granules; feeding the assembled steel-plastic composite furnace burden blank together with the asbestos heat insulation plate into a heat preservation chamber provided with a ventilation system, preserving heat for 4-6 hours, and cooling to room temperature; removing the asbestos heat insulation plate, and feeding the obtained steel-plastic composite furnace charge into a furnace for a steelmaking process; according to the method, the plastic particles are melted and cured by utilizing heat of the slag steel hot-pressing block, the slag steel hot-pressing block and the plastic particles are processed into a composite body for use, the waste heat of the hot-pressing iron block and the thermoplastic characteristic of plastic are reasonably utilized, the problem that small-particle slag steel and the plastic particles are difficult to enter a furnace is solved, and harmless treatment and resource utilization of hazardous waste are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for coordinated utilization of waste plastic barrels and slag steel. Background Art

[0002] In their daily work, steel enterprises need to use various auxiliary materials and thus generate a large number of waste plastic barrels and other packaging materials. Since these waste plastic barrels are inevitably stained with paint and other substances, they are hazardous wastes explicitly stipulated by the Ministry of Environment. In order to dispose of this type of hazardous waste, steel enterprises need to entrust external qualified units to dispose of it in compliance with regulations at a price of thousands of yuan per ton each year, which consumes a lot of disposal costs.

[0003] There has been some basic research on the recycling of waste plastics in steel companies. Japan crushes waste plastics into powder and reuses it in blast furnace smelting together with pulverized coal. However, the process of preparing plastic powder suitable for blast furnace injection is complicated and lacks application in China. There has also been some research on the use of plastics in coke ovens, but this method has a certain impact on coke oven production and the quality stability of coke products. The reuse of plastics in converter steelmaking has little impact on production and can provide a certain amount of heat, but there is little research on the use of waste plastics in converter steelmaking, mainly because there is a certain negative pressure in the converter, and plastics have a low density and light weight, which can be easily blown away by coal gas and are difficult to enter the furnace.

[0004] Slag steel is a typical secondary resource solid waste of iron and steel metallurgical enterprises. Small particles of slag steel have low metal grade, are difficult to enter the furnace, and have low recovery rate, so they are not suitable for direct reuse in converters. CN114196824B provides a method for preparing slag steel hot pressed blocks, which purifies the slag steel and hot presses it into a metal material suitable for the steelmaking process, which can replace scrap steel. However, in actual practice, the technical concept of hot delivery and hot loading is limited by the production rhythm of converter smelting and hot pressed blocks in practice, which is difficult to match, has limited energy-saving effects, and brings difficulties in high-temperature operation. Summary of the invention

[0005] In view of the problems that waste plastic barrels are difficult to put into the furnace and there is heat loss in slag steel hot-pressed blocks, the present invention provides a method for the coordinated disposal of the two, using the heat of the slag steel hot-pressed blocks to melt and solidify plastic particles, and processing the two into a composite for use, rationally utilizing the waste heat of the hot-pressed iron blocks and the thermoplastic characteristics of the plastic, solving the problem that small particles of slag steel and plastic particles are difficult to put into the furnace, achieving the harmless disposal and resource utilization of hazardous waste, and having good technical and economic benefits.

[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0007] A method for the coordinated utilization of waste plastic barrels and slag steel comprises the following steps:

[0008] 1) heating the small slag steel to about 600-800° C. and maintaining it for 5-10 minutes; placing it into a hot pressing ring mold, and obtaining a slag steel hot pressing ring through hot pressing treatment;

[0009] 2) After the slag steel hot pressing ring is naturally cooled to 600-700°C, it is placed horizontally on the asbestos insulation board, the lime insulation ring is installed inside the slag steel hot pressing ring, and the cavity inside the lime insulation ring is filled with plastic granules;

[0010] 3) The steel-plastic composite charge embryo composed of slag steel hot pressing ring, lime insulation ring, plastic granules and asbestos insulation board are sent to an insulation room equipped with a ventilation system, and cooled to room temperature after insulation for 4 to 6 hours;

[0011] 4) Remove the asbestos insulation board and put the obtained steel-plastic composite charge into the furnace for steelmaking process.

[0012] According to the above scheme, the chemical composition of the small slag steel in step 1 is: TFe 85.0% to 90.0%, CaO≤2.0%, MgO≤1.0%, SiO2≤0.5%, Al2O3≤0.2%, and the remainder is O element combined with Fe element and other inevitable impurity elements; its particle size characteristic is that the mass of particles below 4mm (5 mesh) is ≥95%.

[0013] According to the above scheme, the outer diameter of the internal cavity of the hot pressing annular mold in step 1 is ≦20 cm, the inner diameter is ≧15 cm, the difference between the inner and outer diameters is 3 to 4 cm, and the height is 15 to 20 cm.

[0014] According to the above scheme, the hot pressing temperature in step 1 does not exceed 1250°C.

[0015] According to the above scheme, the plastic granules in step 2 are prepared by processing waste plastic barrels; the material is high-density polyethylene (HDPE) or polypropylene (PP); the particle size of the plastic granules is 5 to 10 mm.

[0016] According to the above scheme, the asbestos insulation board in step 2 is a rectangular parallelepiped with a side length of 20 to 25 cm and a thickness of 1 to 2 cm.

[0017] According to the above scheme, the outer diameter of the lime insulation ring in step 2 matches the inner diameter of the slag steel hot pressing ring, and the two are highly flush; the difference between the inner and outer diameters of the lime insulation ring is 2 cm.

[0018] In the above scheme, the lime heat insulation ring in step 2 is made by burning quicklime, and its chemical composition is: CaO 96-99%, and the remainder is inevitable impurity elements.

[0019] In the above scheme, the insulation chamber in step 3 is provided with heat insulation materials on the inner wall; and the ventilation system is provided with an activated carbon purification section.

[0020] In the above scheme, step 4 also includes reusing the removed asbestos insulation board.

[0021] The present invention utilizes the residual heat of hot pressing blocks to melt plastic particles and compound the two. The residual heat of the hot pressing blocks is 600-700°C, which is higher than the decomposition temperature of polyethylene or polypropylene (about 350°C). Direct contact between the two will cause the plastic to decompose and cannot form a composite. In response to this problem, the present invention proposes to use a CaO-based insulation ring as a heat insulation-heat transfer body. On the one hand, CaO is a necessary raw material in the steelmaking process, does not affect steelmaking and has a positive effect on pure steel smelting. On the other hand, CaO can be used as a refractory material, has the advantages of high refractoriness and is not easy to deform. Its specific heat capacity and heat transfer coefficient are moderate, and the heat of the hot pressing blocks can be slowly transferred to the plastic layer to avoid rapid decomposition of the plastic.

[0022] The present invention also needs to control the relationship between the slag steel hot pressing ring, the lime insulation ring, and the plastic layer. The total heat of the composite of the three in the insulation chamber cannot be too low, otherwise the melting temperature of the system plastic (about 170°C) cannot be reached. At the same time, the total heat cannot be too high, otherwise the temperature of the composite exceeds 350°C and the plastic will decompose. In addition, the heat of the slag steel ring is also used to heat the air in the insulation chamber, so that the entire insulation chamber has a certain ambient temperature. Therefore, within the control range of the technical solution described in the present invention, the total heat can control the thermal equilibrium end temperature between 200 and 300°C, meeting the preparation technical requirements.

[0023] Conventional methods using external adhesives are difficult to implement in the situations described in the present invention. The present invention takes advantage of the characteristics of thermoplastics. After the inner plastic particles melt, the particles bond to each other to form a whole. On the other hand, the plastic in contact with the lime insulation ring melts and cools and solidifies, and naturally forms a whole with the lime ring (the two will cool down synchronously during the cooling process). The outermost slag steel ring has the property of thermal expansion and contraction. At the beginning, the slag steel hot pressing ring has a high temperature and expands to a certain extent. After cooling, the volume shrinks, and internal force is naturally generated, which is fastened together with the two inner layers. The circular cross-section of the slag steel ring itself also ensures that the internal stress distribution is relatively uniform, and there will be no local fracture or deformation problems.

[0024] In addition, due to the general limitations of converter scrap steel equipment, the size of the slag steel hot pressing ring is controlled within the range of φ20×20cm to meet the charging requirements and facilitate operation. At the same time, the overall weight of the slag steel-lime-plastic composite is moderate, which can be smoothly charged without causing excessive impact on the converter lining. The ventilation system of the insulation room has an activated carbon purification section. Plastic granules are inevitably contaminated with a small amount of low-melting and boiling point organic matter, which is easy to volatilize. During the ventilation and cooling process, they can be adsorbed and purified by activated carbon to avoid environmental pollution.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] Due to the negative pressure of the converter and the limitation of steelmaking process, plastic barrels or plastic particles have low density and cannot be directly loaded into the converter. The present invention composites plastic and metal to solve the problem of loading plastic into the converter.

[0027] The present invention relies on the existing slag steel hot-pressed briquette preparation process production line of the steel plant, and collaboratively solves the problem of disposal and utilization of waste plastic barrels within the steel plant. It has small additional investment, saves a large amount of external disposal costs of waste plastic barrels, and also enables the energy utilization of plastic waste in steel plant production, saving enterprise fuel.

[0028] This method processes plastic barrels and reuses them in steelmaking. Compared with using waste plastics for blast furnace injection, its processing process and use technology are simpler. Compared with using waste plastics for coking in coke ovens, it avoids adverse effects on coking production and coke quality.

[0029] Waste plastic barrels are made of high-density polyethylene or polypropylene, both of which are thermoplastics. The melting-solidification process of the plastic effectively utilizes the sensible heat of the hot pressing block, without the need for additional heating, thus saving energy.

[0030] Waste plastic barrels are inevitably stained with a small amount of paint and other substances. The ventilation system of the insulated box has an activated carbon adsorption section, which can purify the volatile harmful substances and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 : Schematic diagram of the assembly of the steel-plastic composite charge embryo of the present invention. DETAILED DESCRIPTION

[0032] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0033] The specific implementation method provides a method for the coordinated utilization of waste plastic barrels and slag steel, comprising the following steps:

[0034] 1) Disassemble the waste plastic barrels, remove metal parts such as metal handles, separate the plastic parts, and use a plastic shredder to process the plastic barrels into plastic granules, which are collected for later use; the waste plastic barrels are plastic barrels recycled after use in various processes in steel enterprises, and are made of high-density polyethylene (HDPE) or polypropylene (PP). The size of the shredded plastic granules is 5 to 10 mm;

[0035] 2) feeding the small slag steel into a heating furnace, heating to about 600-800°C, and maintaining for 5-10 minutes; the small slag steel is obtained by crushing and screening the small particle slag steel purified by the method described in CN114196824B, and its chemical composition characteristics are: TFe85.0%-90.0%, CaO≤2.0%, MgO≤1.0%, SiO2≤0.5%, Al2O3≤0.2%, and the remainder is O element combined with Fe element and other inevitable impurity elements; its particle size characteristic is that the mass of particles below 4mm (5 mesh) is ≥95%;

[0036] 3) loading the small slag steel into a hot press annular mold, and obtaining a slag steel hot pressing ring through hot pressing treatment, wherein the pressing temperature does not exceed 1250° C.; the outer diameter of the inner cavity of the hot pressing annular mold is ≦20 cm, the inner diameter is ≧15 cm, the difference between the inner and outer diameters is 3-4 cm, and the height is 15-20 cm;

[0037] 4) Cool the slag steel hot pressing ring naturally to 600-700℃, place it horizontally in the middle of the asbestos insulation board at the paving station, quickly install the lime insulation ring into the inner side of the slag steel hot pressing ring, and fill the cavity in the lime insulation ring with plastic granules, compact it, and keep the upper surface of the filled plastic granules basically flush with the surface. Refer to the attached diagram for the assembly of the steel-plastic composite charge embryo. Figure 1 As shown; the asbestos insulation board is a cuboid with a side length of 20 to 25 cm and a thickness of 1 to 2 cm; the outer diameter of the lime insulation ring is the same as the inner diameter of the cavity inside the hot pressing ring mold, the difference between the inner and outer diameters is 2 cm, and the ring height is the same as the cavity inside the slag steel hot pressing ring mold; the lime insulation ring is made of quicklime, and its chemical composition is characterized by: CaO 96 to 99%, and the balance is inevitable impurity elements;

[0038] 5) Send the paved assembly consisting of asbestos insulation board, slag steel hot pressing ring, lime insulation ring and plastic granules into an insulation room equipped with a ventilation system and keep it warm for 4 to 6 hours;

[0039] 6) The insulation box is ventilated and cooled to room temperature by using the ventilation system of the insulation chamber; the insulation chamber is provided with heat insulation materials on the inner wall, which can greatly reduce heat loss, and the ventilation system of the insulation chamber has an activated carbon purification section;

[0040] 7) Take out the assembly, remove the asbestos insulation board and reuse it, and the obtained steel-plastic composite charge can be used as a product in the steelmaking process.

[0041] Example 1

[0042] The chemical composition of the small slag steel used is: TFe 88.9%, CaO 1.2%, MgO 0.6%, SiO2 0.3%, Al2O3 0.1%, and the balance is O element combined with Fe element and other inevitable impurity elements. Screening of the small particle slag steel sample shows that the particle size characteristic is that the mass of particles below 4mm (5 mesh) accounts for 98.4%.

[0043] The plastic barrel used is made of high-density polyethylene (HDPE), and the size of the shredded plastic particles is 5 to 10 mm.

[0044] The inner cavity of the hot pressing annular mold used has an outer diameter of 20 cm, an inner diameter of 16 cm and a height of 20 cm.

[0045] The asbestos insulation board used is a cuboid with a side length of 25×22×2cm.

[0046] The lime heat-insulating ring used has an outer diameter of 16 cm, an inner diameter of 14 cm, and a ring height of 20 cm; the chemical composition is CaO 96.9%, and the remainder is inevitable impurity elements.

[0047] A method for collaboratively utilizing waste plastic barrels and slag steel comprises the following steps:

[0048] 1) Disassemble the waste plastic barrel, remove metal parts such as metal handles, separate the plastic parts, use a plastic shredder to process the plastic barrel into plastic granules, and collect them for later use;

[0049] 2) Send the small slag steel into the heating furnace, heat it to about 620°C, and keep it for 6 minutes;

[0050] 3) The small slag steel is loaded into a hot press ring mold, and the hot press mold is subjected to hot pressing treatment to obtain a slag steel hot pressing ring, and the pressing temperature is about 1200°C;

[0051] 4) Cool the slag steel hot pressing ring naturally to 650°C, place it horizontally in the middle of the asbestos insulation board at the paving station, quickly install the lime insulation ring into the inner side of the slag steel hot pressing ring, and fill the cavity in the lime insulation ring with plastic granules, compact it, and keep the upper surface of the filled plastic granules basically flush;

[0052] 5) Send the paved assembly consisting of asbestos insulation board, slag steel hot pressing ring, lime insulation ring and plastic granules into an insulation room equipped with a ventilation system and keep it warm for 4 hours;

[0053] 6) Use the ventilation system of the insulation room to ventilate and cool the insulation box to room temperature;

[0054] 7) The assembly is taken out, the asbestos insulation board is removed and reused, and the obtained steel-plastic composite charge is used as a product in the steelmaking process.

[0055] Example 2

[0056] The chemical composition of the small slag steel used is: TFe 87.2%, CaO 1.0%, MgO 0.4%, SiO2 0.2%, Al2O3 0.1%, and the balance is O element combined with Fe element and other inevitable impurity elements. Screening of the small particle slag steel sample shows that the particle size characteristic is that the mass of particles below 4mm (5 mesh) accounts for 97.7%.

[0057] The plastic barrel used is made of polypropylene (PP), and the size of the shredded plastic particles is 5 to 10 mm.

[0058] The inner cavity of the hot pressing annular mold used has an outer diameter of 18 cm, an inner diameter of 15 cm, and a height of 15 cm.

[0059] The asbestos insulation board used is a cuboid with a side length of 20×20×1 cm.

[0060] The lime heat-insulating ring used has an outer diameter of 15 cm, an inner diameter of 13 cm, and a ring height of 15 cm; the chemical composition is CaO 98.3%, and the remainder is inevitable impurity elements.

[0061] A method for collaboratively utilizing waste plastic barrels and slag steel comprises the following steps:

[0062] 1) Disassemble the waste plastic barrel, remove metal parts such as metal handles, separate the plastic parts, use a plastic shredder to process the plastic barrel into plastic granules, and collect them for later use;

[0063] 2) Send the small slag steel into the heating furnace, heat it to about 690°C, and keep it for 10 minutes;

[0064] 3) The small slag steel is loaded into a hot press ring mold, and the hot press mold is subjected to hot pressing treatment to obtain a slag steel hot pressing ring, and the pressing temperature is about 1180°C;

[0065] 4) Cool the slag steel hot pressing ring naturally to 610°C, place it horizontally in the middle of the asbestos insulation board at the paving station, quickly install the lime insulation ring into the inner side of the slag steel hot pressing ring, and fill the cavity in the lime insulation ring with plastic granules, compact it, and keep the upper surface of the filled plastic granules basically flush;

[0066] 5) Send the paved assembly consisting of asbestos insulation board, slag steel hot pressing ring, lime insulation ring and plastic granules into an insulation room equipped with a ventilation system and keep it warm for 5 hours;

[0067] 6) Use the ventilation system of the insulation room to ventilate and cool the insulation box to room temperature;

[0068] 7) The assembly is taken out, the asbestos insulation board is removed and reused, and the obtained steel-plastic composite charge is used as a product in the steelmaking process.

[0069] Example 3

[0070] The chemical composition of the small slag steel used is: TFe 86.3%, CaO 0.8%, MgO 0.5%, SiO2 0.3%, Al2O3 0.1%, and the balance is O element combined with Fe element and other inevitable impurity elements. Screening of the small particle slag steel sample shows that the particle size characteristic is that the mass of particles below 4mm (5 mesh) accounts for 96.2%.

[0071] The plastic barrel used is made of polypropylene (PP), and the size of the shredded plastic particles is 5 to 10 mm.

[0072] The inner cavity of the hot pressing annular mold used has an outer diameter of 15 cm, an inner diameter of 12 cm, and a height of 17 cm.

[0073] The asbestos insulation board used is a cuboid with a side length of 24×20×1 cm.

[0074] The lime heat-insulating ring used has an outer diameter of 12 cm, an inner diameter of 10 cm, and a ring height of 17 cm; the chemical composition is CaO 97.6%, and the remainder is inevitable impurity elements.

[0075] A method for collaboratively utilizing waste plastic barrels and slag steel comprises the following steps:

[0076] 1) Disassemble the waste plastic barrel, remove metal parts such as metal handles, separate the plastic parts, use a plastic shredder to process the plastic barrel into plastic granules, and collect them for later use;

[0077] 2) Send the small slag steel into the heating furnace, heat it to about 650°C, and keep it for 8 minutes;

[0078] 3) The small slag steel is loaded into a hot press ring mold, and the hot press mold is subjected to hot pressing treatment to obtain a slag steel hot pressing ring, and the pressing temperature is about 1150°C;

[0079] 4) Cool the slag steel hot pressing ring naturally to 640°C, place it horizontally in the middle of the asbestos insulation board at the paving station, quickly install the lime insulation ring into the inner side of the slag steel hot pressing ring, and fill the cavity in the lime insulation ring with plastic granules, compact it, and keep the upper surface of the filled plastic granules basically flush;

[0080] 5) Send the assembled materials consisting of asbestos insulation board, slag steel hot pressing ring, lime insulation ring and plastic granules into the insulation room equipped with ventilation system and keep them warm for 6 hours;

[0081] 6) Use the ventilation system of the insulation room to ventilate and cool the insulation box to room temperature;

[0082] 7) The assembly is taken out, the asbestos insulation board is removed and reused, and the obtained steel-plastic composite charge is used as a product in the steelmaking process.

[0083] In the traditional steelmaking process, scrap steel is used as a coolant (effective component iron), a recarburizer is used as a heating agent (effective component carbon), and metallurgical lime is used as a slag-forming agent (effective component lime). The slag steel ring part of the steel-plastic composite charge of the present invention has the function of scrap steel, the inner layer of the plastic granular material has the function of heating, and the lime insulation ring has the function of a slag-forming agent. To further illustrate the use effect of the steel-plastic composite charge of the present invention, the application effect of the steel-plastic composite charge obtained in the embodiment of the present invention is compared with that of the traditional steelmaking charge, as shown in Table 1.

[0084] Table 1 Comparison of application effects of steel-plastic composite furnace charge

[0085]

[0086] In the embodiment, about 5 tons of steel-plastic composite charge is added to the converter, and in the comparative example, 3.5-3.8 tons of scrap steel and 0.6-0.8 tons of lime are used to replace the steel-plastic composite charge and added to the converter. The rest adopts normal smelting operation and raw material addition. The results show that in terms of molten steel tapping temperature, the embodiment is better than the comparative example as a whole. This is mainly because the plastic is oxygenated during the blowing process, providing a certain amount of heat to the molten steel, and at the same time realizing the digestion and utilization of waste plastics. The sulfur content of molten steel is usually less than 0.05%. The embodiment is equivalent to the comparative example, indicating that the use of steel-plastic composite charge has no obvious effect on the quality of molten steel. The application of the technology of the present invention realizes the resource utilization of slag steel and the harmless disposal and utilization of waste plastic barrels without affecting the quality of molten steel, and has good technical and economic effects.

Claims

1. A method for the coordinated utilization of waste plastic barrels and slag steel, characterized in that The following steps are involved: 1) heating the small slag steel to about 600-800° C. and maintaining it for 5-10 minutes; placing it into a hot pressing ring mold, and obtaining a slag steel hot pressing ring through hot pressing treatment; 2) After the slag steel hot pressing ring is naturally cooled to 600-700°C, it is placed horizontally on the asbestos insulation board, the lime insulation ring is installed inside the slag steel hot pressing ring, and the cavity inside the lime insulation ring is filled with plastic granules; 3) The steel-plastic composite charge embryo composed of slag steel hot pressing ring, lime insulation ring, plastic granules and asbestos insulation board are sent to an insulation room equipped with a ventilation system, and cooled to room temperature after insulation for 4 to 6 hours; 4) Remove the asbestos insulation board and put the obtained steel-plastic composite charge into the furnace for steelmaking process.

2. The method for synergistic utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The chemical composition of the small slag steel in step 1 is as follows: TFe 85.0% to 90.0%, CaO≤2.0%, MgO≤1.0%, SiO2≤0.5%, Al2O3≤0.2%, and the remainder is O element combined with Fe element and other inevitable impurity elements; Its particle size characteristic is that the mass of particles below 4 mm is ≥95%.

3. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The outer diameter of the internal cavity of the hot pressing annular mold in step 1 is ≦20 cm, the inner diameter is ≧15 cm, the difference between the inner and outer diameters is 3 to 4 cm, and the height is 15 to 20 cm.

4. The method for the coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The hot pressing temperature in step 1 does not exceed 1250°C.

5. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The plastic granules in step 2 are prepared by processing waste plastic barrels; the material is high-density polyethylene or polypropylene; the particle size of the plastic granules is 5 to 10 mm.

6. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The asbestos insulation board in step 2 is a cuboid with a side length of 20 to 25 cm and a thickness of 1 to 2 cm.

7. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that In step 2, the outer diameter of the lime insulation ring matches the inner diameter of the slag steel hot pressing ring, and the two are highly flush; the difference between the inner and outer diameters of the lime insulation ring is 2 cm.

8. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that The lime heat insulation ring in step 2 is made by burning quicklime, and its chemical composition is: CaO 96-99%, and the remainder is inevitable impurity elements.

9. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that In step 3, the insulation chamber is provided with heat-insulating materials on the inner wall; and the ventilation system is provided with an activated carbon purification section.

10. The method for coordinated utilization of waste plastic barrels and slag steel as claimed in claim 1, characterized in that Step 4 also includes removing the asbestos insulation board for reuse.