Al-Mg-Si series cast aluminum alloy, forming process and heat treatment method

By adding vanadium element to Al-Mg-Si cast aluminum alloy and combining it with vacuum smelting and heat treatment processes, the problems of pinhole defects and performance degradation during aluminum alloy forming and heat treatment are solved, and its strength and corrosion resistance are significantly improved. Optimized the organizational structure.

CN118745540APending Publication Date: 2024-10-08泛锐云智科技(郑州)有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410955843.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Al-Mg-Si cast aluminum alloys are prone to pinhole defects during the molding and heat treatment processes, which affect their mechanical properties and corrosion resistance. The existing heat treatment process has a complex impact on performance and is difficult to effectively improve.

Method used

The metallic vanadium element is added to the Al-Mg-Si cast aluminum alloy, and by strictly controlling the amount and timing of vanadium addition, combined with vacuum smelting and heat treatment processes, a thermally stable compound of vanadium and aluminum is formed to refine the grains and prevent microscopic Cracks and grain boundary corrosion, optimizing the mechanical and corrosion resistance properties of aluminum alloys.

Benefits of technology

It significantly improves the strength, hardness and corrosion resistance of Al-Mg-Si cast aluminum alloy, reduces the pinhole rate, optimizes the organizational structure, and enhances the mechanical properties and heat resistance of the aluminum alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745540A_ABST
    Figure CN118745540A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of alloy material processing, and particularly relates to an Al-Mg-Si series cast aluminum alloy, a forming process and a heat treatment method. The Al-Mg-Si series cast aluminum alloy comprises the following chemical components in percentage by mass: 9%-10.5% of Si, 0.2%-0.3% of Mg, 0.2%-0.5% of Mn, 0.05%-0.1% of V, less than or equal to 0.3% of impurity element Fe, less than or equal to 0.05% of the sum of other impurity elements and the balance of Al. According to the method, the vanadium element is added into the Al-Mg-Si series cast aluminum alloy for the first time, a forming process and a heat treatment process of the aluminum alloy are combined, so that vanadium and aluminum form a thermally stable compound, the strength and hardness of the aluminum alloy are effectively improved, in addition, vanadium and aluminum can also form phases which are not mutually dissolved, and therefore micro cracks and grain boundary corrosion are prevented from occurring, and the service life of the aluminum alloy is prolonged. And the hot working performance and the corrosion resistance of the aluminum alloy are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy material processing, and in particular relates to an Al-Mg-Si series cast aluminum alloy, a molding process and a heat treatment method. Background Art

[0002] Aluminum alloys have the advantages of high strength, low density, good heat dissipation, low elastic modulus, anti-electromagnetic radiation, and corrosion resistance, making them widely used in engineering structures that have high requirements for light weight and corrosion resistance, and have important application value in the fields of microelectronics, lightweight transportation, aerospace, automotive industry, and ships. For example, Al-Mg-Si cast aluminum alloys have excellent castability, good corrosion resistance, small linear shrinkage, and good air tightness. They are suitable for casting parts with complex shapes, thin walls, corrosion resistance, and high static and impact loads. They are widely used in aerospace, transportation, construction, ships, marine engineering, and other fields.

[0003] However, in the Al-Mg-Si cast aluminum alloy forming and heat treatment process, since the aluminum alloy easily absorbs hydrogen during the smelting process, it is easy to form pinhole defects, which affects the mechanical properties and appearance quality of the casting, and even reduces the mechanical properties such as the bearing capacity and fracture toughness of the aluminum alloy as well as the corrosion resistance, shortening its service life. In response to this problem, researchers such as Zhao Aibin and others have studied the heat treatment process of Al-Mg-Si cast aluminum alloy. By solution treatment at 535±5℃ for 4h, water cooling to 80℃, and then aging at 175±5℃ for 6h, the aluminum alloy has a relatively high hardness, but there is still a large gap with its theoretical maximum value. It is speculated that this is due to the presence of Mg in the precipitate phase. 2 Si causes the hardness to decrease, and the corrosion resistance of the aluminum alloy specimens after only solution treatment is relatively good. After solution and aging treatment, obvious cracks appear due to the precipitation of the second phase and the segregation of alloy elements, resulting in a decrease in corrosion resistance.

[0004] Although heat treatment process is one of the important means to improve the performance of aluminum alloy, the influence of heat treatment process on the performance of aluminum alloy is relatively complex and is closely related to the composition and forming process of aluminum alloy. Therefore, how to improve the performance of Al-Mg-Si cast aluminum alloy is still a technical problem that needs to be overcome in the preparation of Al-Mg-Si cast aluminum alloy. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention aims to provide an Al-Mg-Si cast aluminum alloy, a molding process and a heat treatment method. The present invention significantly improves the strength and hardness of the Al-Mg-Si cast aluminum alloy, and enhances its heat resistance and corrosion resistance by adding metal vanadium to the raw materials for preparing the Al-Mg-Si cast aluminum alloy, strictly controlling the amount and timing of vanadium addition, and combining the heat treatment process.

[0006] Based on the above purpose, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides an Al-Mg-Si based cast aluminum alloy, comprising the following chemical components in mass percentage: Si 9% to 10.5%, Mg 0.2% to 0.3%, Mn 0.2% to 0.5%, V 0.05% to 0.1%, impurity element Fe not exceeding 0.3%, the sum of other impurity elements not exceeding 0.05%, and the balance being Al.

[0007] The present invention adds vanadium (V) element to Al-Mg-Si cast aluminum alloy for the first time, and combines the forming process and heat treatment process of the aluminum alloy so that vanadium and aluminum form a thermally stable compound, which effectively improves the strength and hardness of the aluminum alloy. In addition, vanadium and aluminum can also form mutually insoluble phases, thereby preventing the occurrence of micro cracks and intergranular corrosion, and improving the hot working performance and corrosion resistance of the aluminum alloy.

[0008] The present invention strictly controls the amount of vanadium added in the system to be 0.05-0.1%. If the amount added is too low, it is easily consumed by the impurity reaction in the system, resulting in the failure to achieve the purpose of improving the performance of the aluminum alloy, while avoiding excessive addition leading to a decrease in the performance of the aluminum alloy. By strictly controlling the amount of vanadium added, the mechanical properties, heat resistance and corrosion resistance of the aluminum alloy are further improved without changing the basic components of the Al-Mg-Si cast aluminum alloy.

[0009] In a second aspect, the present invention provides a forming process for the above-mentioned Al-Mg-Si series cast aluminum alloy, comprising the following steps: S1: According to the chemical composition of the Al-Mg-Si cast aluminum alloy, Al ingots, Mg ingots, manganese-aluminum alloy, V powder, and Si powder are prepared, and refining agent and slag-forming agent are weighed for use; S2: After drying the Al ingot, the manganese-aluminum alloy and the Si powder, vacuum melting technology is used, and the refining agent and the slag-making agent are added at 700-730°C for 5-8 minutes, and stirring and slagging are performed; S3: adding Mg ingots to the melt refined in step S2, until the Mg ingots are melted and fully deoxidized, then heating the melt, adding V powder to the melt for mechanical stirring and ultrasonic vibration, and adding a refining agent to the melt for refining; S4: Cooling the molten metal obtained in step S3 and casting it into a preheated mold, and naturally cooling it to obtain a cast Al-Mg-Si aluminum alloy.

[0010] Since vanadium has a great affinity for oxygen and is easily oxidized, the present invention adopts vacuum melting technology to reduce the oxygen content in the melt. At the same time, after the other raw material components are melted, refined, deslagging and deoxidized, the melt is in a reduction period with a relatively low oxygen content. At this time, adding vanadium to the melt is conducive to the stable existence and alloying of vanadium. After adding vanadium, sufficient stirring and refining are required to ensure that the vanadium is evenly distributed in the melt and fully reacts with other alloy elements.

[0011] Preferably, the refining agent is a mixture of hexachloroethane and mixed rare earth in a mass ratio of 2:(0.5-1.5), and the amount of the refining agent added is 1-2.5 g / kg of melt.

[0012] The mixed rare earth consists of 50wt% to 60wt% of cerium (Ce), 25wt% to 35wt% of lanthanum (La) and 15wt% to 20wt% of neodymium (Nd).

[0013] The refining agent is added to the aluminum melt twice. The first time, when the temperature of the aluminum melt reaches 700-730℃, the refining agent is added. The second time, the refining agent is added again before it is taken out of the furnace. By adding the refining agent in batches, it has an obvious purification effect on the aluminum alloy, which can greatly reduce the pinhole rate, optimize the structure of the aluminum alloy, and significantly improve the thermal conductivity, processing performance and mechanical properties of the aluminum alloy.

[0014] Preferably, the specific adding process of Mg ingot and V powder in step S3 is as follows: First, add Mg ingot to the melt refined in step S2, heat to 740-750°C and keep warm for 3-8 minutes for vacuum melting. After the melt is fully deoxidized, add V powder to the melt, and perform mechanical stirring and ultrasonic vibration at 800-1000°C.

[0015] Since vanadium has a strong affinity with oxygen and is easily oxidized, adding it too early is not conducive to the stable existence and alloying of vanadium. Therefore, vanadium is added in the later stage of alloy smelting, after the melt has been fully deoxidized. At the same time, during the process of adding vanadium, contact with slag on the surface of the melt is avoided to prevent oxidation and contamination of vanadium. Therefore, the melt also needs to be refined and slag-stripped before adding vanadium.

[0016] In order to make vanadium evenly distributed in the melt and fully react with other alloying elements, sufficient mechanical stirring and ultrasonic vibration treatment are required after adding vanadium. Based on the high melting point of vanadium, the reaction temperature of the melt is increased to accelerate the dispersion and reaction of vanadium in the melt, while avoiding excessive melting temperature, which may cause a large amount of alloying elements in the melt to burn out, and lead to an increase in oxides, nitrides, and carbides in the aluminum alloy melt. These tiny dispersed non-metallic inclusions may be embedded in the crystal or precipitated at the grain boundary during solidification, increasing the possibility of fatigue crack sources and reducing the mechanical properties and corrosion resistance of the base metal.

[0017] Preferably, in step S4, the temperature of the molten metal is reduced to 680-750°C; and the preheating temperature of the mold is 450-500°C.

[0018] The selection of pouring temperature is crucial to the casting quality of aluminum alloy. Too high a pouring temperature may cause defects such as shrinkage cavities and thermal cracks in the casting, while too low a pouring temperature may cause incomplete filling of the casting or cold shut. For the aluminum alloy of the composition described in the present invention, the pouring temperature range is preferably 680°C to 760°C. This temperature range can ensure that the aluminum liquid has good fluidity while avoiding excessive casting defects.

[0019] The mold temperature is a key factor affecting the cooling rate and solidification process of the casting. If the mold temperature is too high, the casting may cool slowly, resulting in defects such as shrinkage cavities and thermal cracks; if the mold temperature is too low, the casting may have defects such as cold shut and insufficient pouring. For the aluminum alloy of the composition described in the present invention, since the aluminum alloy has high casting performance and air tightness, the mold temperature range is preferably 450°C to 500°C. This temperature range can ensure that the casting maintains good dimensional stability and surface quality during the cooling process.

[0020] In a third aspect, the present invention provides a heat treatment method for an Al-Mg-Si cast aluminum alloy, the heat treatment method being performed on a cast Al-Mg-Si aluminum alloy prepared by the above-mentioned molding process, and the heat treatment method comprising the following steps: (1) Annealing treatment: heat the cast Al-Mg-Si aluminum alloy to 280-300°C, keep it at this temperature for 2-3 hours, and then cool it to room temperature in the furnace; (2) Solution treatment: The cast Al-Mg-Si aluminum alloy annealed in step (1) is heated to 490-525°C, kept at this temperature for 2-4 hours, and water-cooled at 60-100°C for a solid solution treatment; The cast Al-Mg-Si aluminum alloy of the primary solid solution is heated to 530-545°C, kept at this temperature for 2-4 hours, and water-cooled at 60-100°C for strengthening solid solution; (3) Re-aging treatment: The cast Al-Mg-Si aluminum alloy after the solution treatment in step (2) is kept at 160-170° C. for 1-5 hours, and then cooled to room temperature for pre-aging treatment; The cast Al-Mg-Si aluminum alloy after pre-aging treatment is kept at 500-520°C for 1-5 hours, cooled to room temperature along with the furnace, and then subjected to retrograde heat treatment; The cast Al-Mg-Si aluminum alloy subjected to the retrograde heat treatment is kept at 170-180°C for 1-5 hours, and then cooled to room temperature for re-aging treatment.

[0021] The Al-Mg-Si cast aluminum alloy prepared by the above-mentioned molding process is pre-annealed at 490-525°C to eliminate internal stress, promote grain rearrangement, and provide good organizational preparation for subsequent solution and aging treatments.

[0022] After the annealed aluminum alloy is subjected to the first solid solution treatment, Mg 2 Si dissolves in α(Al) to form a solid solution saturated body of α phase. After the second solid solution treatment, it further promotes the strengthening phase β(Mg 2 The formation of Si) phase helps to enhance the tensile strength and hardness of the aluminum alloy; at the same time, the two solid solution treatments enable the vanadium element in the alloy to further refine the grains, reduce the intergranular space, and hinder the dislocation movement, which helps to further enhance the tensile strength and hardness of the aluminum alloy.

[0023] After the solid solution aluminum alloy is subjected to regression and aging treatment, the strengthening phase β (Mg 2 The Si) phase dissolves and re-precipitates, optimizing the grain boundary structure of the alloy, causing the continuous chain-like precipitated phases at the grain boundaries to merge and aggregate, and no longer be distributed continuously, thereby significantly improving the corrosion resistance of the aluminum alloy.

[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention adds vanadium to the Al-Mg-Si cast aluminum alloy for the first time. Without changing the basic composition of the Al-Mg-Si cast aluminum alloy, on the one hand, vanadium and aluminum are promoted to form a thermally stable compound, and grain refinement, reduction of intergranular space, and inhibition of dislocation movement are promoted, which helps to enhance the tensile strength and hardness of the aluminum alloy. On the other hand, vanadium and aluminum form mutually insoluble phases, which prevents the occurrence of microcracks and intergranular corrosion, and improves the hot working performance and corrosion resistance of the aluminum alloy.

[0025] (2) The forming process of the Al-Mg-Si cast aluminum alloy of the present invention adopts the method of pre-melting other raw materials, refining, deslagging and deoxidizing, and then adding vanadium to the melt, and adding a refining agent for refining and deslagging. On the one hand, by adjusting the order of adding the raw materials, it is possible to effectively avoid the oxidation of vanadium added in the early stage due to the high oxygen content in the melt, thereby failing to achieve the purpose of vanadium alloying. On the other hand, the refining agent is added to the melt in batches, which has a significant purification effect on the aluminum alloy, greatly reduces the pinhole rate of the aluminum alloy, optimizes the alloy structure, and improves its mechanical properties and corrosion resistance.

[0026] (3) The present invention promotes the formation of strengthening phases in the alloy by subjecting the Al-Mg-Si cast aluminum alloy to annealing, two solid solution treatments and regression re-aging treatment in sequence, while refining the grain size, hindering dislocation movement, and merging and aggregating the continuous chain-like precipitation phases at the grain boundary instead of continuously distributing them, thereby significantly improving the tensile strength, hardness and corrosion resistance of the aluminum alloy.

[0027] In summary, the present invention improves the composition of Al-Mg-Si cast aluminum alloy, adjusts its molding process and optimizes the heat treatment process, thereby comprehensively improving the mechanical properties and corrosion resistance of Al-Mg-Si cast aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the Euler diagram of the Al-Mg-Si cast aluminum alloy prepared in Example 1. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. Example 1

[0030] The present embodiment provides an Al-Mg-Si cast aluminum alloy, including the following chemical components in mass percentage: Si 9.8%, Mg 0.25%, Mn 0.37%, V 0.07%, impurity element Fe 0.25%, and the total of other impurity elements such as Cu, Zn, Sn, Pb, etc. does not exceed 0.05%, and the balance is Al.

[0031] The forming process of the Al-Mg-Si series cast aluminum alloy comprises the following steps: S1: According to the chemical composition of the Al-Mg-Si cast aluminum alloy, Al ingots, Mg ingots, manganese-aluminum alloy, V powder, and Si powder are prepared, and refining agent and slag-forming agent are weighed for use; S2: After drying the Al ingot, the manganese-aluminum alloy and the Si powder, vacuum melting technology is used, and after keeping the temperature at 720°C for 8 minutes, a refining agent and a slag-forming agent are added, and stirring and slagging are performed; wherein, the amount of the refining agent added is 1.5 g / kg of the melt; S3: First add Mg ingot to the melt refined in step S2, heat to 745°C and keep warm for 5 minutes for vacuum melting, add V powder to the melt after the melt is fully deoxidized, perform mechanical stirring and ultrasonic vibration at 850°C, and add refining agent to the melt for refining; the amount of refining agent added is 2.5g / kg melt; S4: Cooling the molten metal obtained in step S3 to 700° C. and casting it into a preheated mold, the preheating temperature of the mold is 480° C., and naturally cooling to obtain a cast Al-Mg-Si aluminum alloy.

[0032] The refining agent in steps S2 and S3 is a mixture of hexachloroethane and mixed rare earth in a mass ratio of 2:1, and the mixed rare earth is composed of 55wt% of cerium (Ce), 30wt% of lanthanum (La) and 15wt% of neodymium (Nd).

[0033] The cast Al-Mg-Si aluminum alloy prepared by the above molding process is subjected to heat treatment, comprising the following steps: (1) Annealing treatment: heat the cast Al-Mg-Si aluminum alloy to 280°C, keep it at this temperature for 3 hours, and then cool it to room temperature in the furnace; (2) Solution treatment: The cast Al-Mg-Si aluminum alloy annealed in step (1) is heated to 500°C, kept at this temperature for 3 hours, and water-cooled at 80°C for a solid solution treatment; The cast Al-Mg-Si aluminum alloy of the primary solid solution was heated to 535°C, kept at this temperature for 2 hours, and water-cooled at 80°C for strengthening solid solution; (3) Re-aging treatment: The cast Al-Mg-Si aluminum alloy after the solution treatment in step (2) is kept at 165° C. for 2 h, and then cooled to room temperature for pre-aging treatment; The cast Al-Mg-Si aluminum alloy after pre-aging treatment is kept at 520°C for 3 hours, cooled to room temperature with the furnace, and then subjected to retrograde heat treatment; The cast Al-Mg-Si aluminum alloy after retrograde heat treatment was kept at 175°C for 2 hours and then cooled to room temperature for re-aging treatment.

[0034] The Euler diagram of the Al-Mg-Si cast aluminum alloy after the above-mentioned forming process and heat treatment is as follows: Figure 1 As shown in the figure, it can be seen that the Al-Mg-Si cast aluminum alloy contains β(Mg 2 Si) phase, the grains are fine and the presence of pinholes is almost unobservable. Example 2

[0035] Based on the aluminum alloy composition, forming process and heat treatment method in Example 1, only the amount of vanadium added in the aluminum alloy raw material is adjusted, and the aluminum alloy after the final heat treatment is tested for room temperature tensile properties using a universal tensile testing machine with reference to GB / T 228-2022. The tensile rate is 0.025 mm / s, and the tensile strength and elongation of the 3 mm thick aluminum alloy are tested, and the Rockwell hardness is tested; the corrosion resistance of the aluminum alloy is evaluated with reference to GB / T3880.1-2012, and the results are shown in Table 1, wherein the vanadium addition amount is 0.07%, which is Example 1.

[0036] Table 1 vanadium / % Tensile strength / MPa Rockwell hardness / HRB Elongation / % Corrosion resistance grade 0 503.7 55.3 13.7 F3 0.01 505.1 56.4 13.5 F2 0.05 523.9 75.2 12.8 F1 0.07 533.8 78.9 12.1 F1 0.1 533.4 78.5 12.5 F1 0.2 510.6 56.7 13.3 F1 From the results in Table 1, it can be seen that with the increase of vanadium addition in the melt, the tensile strength and Rockwell hardness of the aluminum alloy both show a trend of first increasing and then decreasing, and the corrosion resistance grade shows an increasing trend with the increase of vanadium addition. When the vanadium addition is 0.05% to 0.1%, it has relatively high tensile strength, hardness and strong corrosion resistance, and at the same time has low elongation, and its comprehensive performance is relatively good. Comparative Example 1

[0037] This comparative example is based on the aluminum alloy composition, forming process and heat treatment method in Example 1, only the refining agent is replaced by an equal amount of hexachloroethane, and the rest of the contents not mentioned are the same as Example 1, and the mechanical properties and corrosion resistance of the aluminum alloy after the final heat treatment are tested, and the tensile strength is 507.9 MPa, the Rockwell hardness is 60.5 HRB, the elongation is 13.0%, and the corrosion resistance grade is F2. It can be seen from the results that compared with Example 1, the tensile strength, hardness and corrosion resistance of the prepared aluminum alloy are all reduced, and the elongation is slightly increased. It is speculated that before the addition of vanadium, the refining in the melt is not thorough, and there are certain pinholes, which reduces the mechanical strength of the aluminum alloy, and is not conducive to the uniform dispersion of vanadium in the melt, resulting in no obvious improvement in the corrosion resistance of the aluminum alloy. Comparative Example 2

[0038] The difference between this comparative example and Example 1 is only that the molding process is different. The alloy composition and heat treatment process not described are the same as those in Example 1. This comparative example adopts vacuum melting by mixing all raw materials at one time. The molding process of the Al-Mg-Si cast aluminum alloy in this comparative example includes the following steps: S1: According to the chemical composition of the Al-Mg-Si cast aluminum alloy, Al ingots, Mg ingots, manganese-aluminum alloy, V powder, and Si powder are prepared, and refining agent and slag-forming agent are weighed for use; S2: After Al ingot, manganese aluminum alloy, Si powder, Mg ingot and V powder are dried, vacuum melting technology is used, and refining agent and slag-forming agent are added after keeping warm at 720℃ for 8 minutes, and stirring and slagging are carried out; wherein, the amount of refining agent added is 1.5g / kg melt; the refining agent is a mixture of hexachloroethane and mixed rare earth in a mass ratio of 2:1, and the mixed rare earth is composed of 55wt% cerium (Ce), 30wt% lanthanum (La) and 15wt% neodymium (Nd).

[0039] S3: Cooling the molten metal obtained in step S2 to 700° C. and casting it into a preheated mold, the preheating temperature of the mold is 480° C., and naturally cooling to obtain a cast Al-Mg-Si aluminum alloy.

[0040] The mechanical properties and corrosion resistance of the aluminum alloy after the final heat treatment were tested. The tensile strength was 501.1 MPa, the Rockwell hardness was 59.3 HRB, the elongation was 13.5%, and the corrosion resistance grade was F3. It can be seen from the results that compared with Example 1, the tensile strength, hardness and corrosion resistance of the prepared aluminum alloy were all reduced, and the elongation was slightly increased. It is speculated that the addition of Mg was too early, resulting in the subsequent strengthening phase β (Mg 2 At the same time, the premature addition of vanadium and the excessively high oxygen content in the melt cause the oxidation of vanadium, which is not conducive to its dispersion in the melt, resulting in a decrease in the corrosion resistance of the aluminum alloy. Comparative Example 3

[0041] The difference between this comparative example and Example 1 is only the heat treatment process. The composition and forming process of the alloy not mentioned are the same as those of Example 1. The heat treatment process of this comparative example includes the following steps: (1) Annealing treatment: heat the cast Al-Mg-Si aluminum alloy to 280°C, keep it at this temperature for 3 hours, and then cool it to room temperature in the furnace; (2) Solution treatment: The cast Al-Mg-Si aluminum alloy annealed in step (1) is heated to 500°C, kept at this temperature for 3 hours, and water-cooled at 80°C for solution treatment; (3) Timeliness treatment: The cast Al-Mg-Si aluminum alloy after the solution treatment in step (2) is kept at 165° C. for 2 h, and then cooled to room temperature for pre-aging treatment.

[0042] The mechanical properties and corrosion resistance of the aluminum alloy after the final heat treatment were tested, and the tensile strength was 512.9 MPa, the Rockwell hardness was 61.7 HRB, the elongation was 13.0%, and the corrosion resistance grade was F2. It can be seen from the results that compared with Example 1, the tensile strength, hardness and corrosion resistance of the prepared aluminum alloy are reduced, and the elongation is slightly increased. It is speculated that due to insufficient solid solution and aging treatment, the precipitation amount of the strengthening phase is relatively reduced, resulting in a decrease in the mechanical properties of the aluminum alloy, and the vanadium element has no significant effect on grain refinement and dislocation inhibition, resulting in no significant improvement in the corrosion resistance of the aluminum alloy.

Claims

1. An Al-Mg-Si cast aluminum alloy, characterized in that: The chemical composition includes the following mass percentages: Si 9%~10.5%, Mg 0.2%~0.3%, Mn 0.2%~0.5%, V 0.05~0.1%, the impurity element Fe does not exceed 0.3%, the sum of the other impurity elements does not exceed 0.05%, and the balance is Al.

2. A forming process for the Al-Mg-Si cast aluminum alloy according to claim 1, characterized in that: The steps include: S1: preparing Al ingots, Mg ingots, manganese-aluminum alloy, V powder, Si powder according to the chemical composition of the Al-Mg-Si cast aluminum alloy according to claim 1, and weighing refining agent and slag-forming agent for use; S2: After drying the Al ingot, the manganese-aluminum alloy and the Si powder, vacuum melting technology is used, and the refining agent and the slag-making agent are added at 700-730°C for 5-8 minutes, and stirring and slagging are performed; S3: adding Mg ingots to the melt refined in step S2, until the Mg ingots are melted and fully deoxidized, then heating the melt, adding V powder to the melt for mechanical stirring and ultrasonic vibration, and adding a refining agent to the melt for refining; S4: Cooling the molten metal obtained in step S3 and casting it into a preheated mold, and naturally cooling it to obtain a cast Al-Mg-Si aluminum alloy.

3. The forming process of Al-Mg-Si based cast aluminum alloy according to claim 2, characterized in that: The refining agent is a mixture of hexachloroethane and mixed rare earth in a mass ratio of 2: (0.5-1.5), and the added amount of the refining agent is 1-2.5 g / kg of melt.

4. The forming process of Al-Mg-Si based cast aluminum alloy according to claim 2, characterized in that: The specific adding process of Mg ingot and V powder in step S3 is as follows: First, add Mg ingot to the melt refined in step S2, heat to 740-750°C and keep warm for 3-8 minutes for vacuum melting. After the melt is fully deoxidized, add V powder to the melt, and perform mechanical stirring and ultrasonic vibration at 800-1000°C.

5. The forming process of Al-Mg-Si based cast aluminum alloy according to claim 2, characterized in that: In step S4, the temperature of the molten metal is reduced to 680-750°C; the preheating temperature of the mold is 450-500°C.

6. A heat treatment method for Al-Mg-Si based cast aluminum alloy, characterized in that: The heat treatment method is carried out based on the cast Al-Mg-Si aluminum alloy prepared by the molding process according to any one of claims 2 to 5, and the heat treatment method comprises the following steps: (1) Annealing treatment: heat the cast Al-Mg-Si aluminum alloy to 280-300°C, keep it at this temperature for 2-3 hours, and then cool it to room temperature in the furnace; (2) Solution treatment: The cast Al-Mg-Si aluminum alloy annealed in step (1) is heated to 490-525°C, kept at this temperature for 2-4 hours, and water-cooled at 60-100°C for a solid solution treatment; The cast Al-Mg-Si aluminum alloy of the primary solid solution is heated to 530-545°C, kept at this temperature for 2-4 hours, and water-cooled at 60-100°C for strengthening solid solution; (3) Re-aging treatment: The cast Al-Mg-Si aluminum alloy after the solution treatment in step (2) is kept at 160-170° C. for 1-5 hours, and then cooled to room temperature for pre-aging treatment; The cast Al-Mg-Si aluminum alloy after pre-aging treatment is kept at 500-520°C for 1-5 hours, cooled to room temperature along with the furnace, and then subjected to retrograde heat treatment; The cast Al-Mg-Si aluminum alloy subjected to the retrograde heat treatment is kept at 170-180°C for 1-5 hours, and then cooled to room temperature for re-aging treatment.

Citation Information

Cited By

  • Heat treatment method for improving toughness and shrinkage deformation of rheo-die-cast Al-Mg-Zn alloy mobile phone middle frame

    CN121674867A

  • A heat treatment method for improving the strength and toughness and shrinkage deformation of a rheo-cast Al-Mg-Zn alloy mobile phone middle frame