Metal dot matrix reinforced ceramic and preparation method thereof
Through the preparation of metal lattice-reinforced ceramics, combining alumina ceramics with 3D printed titanium alloy lattice, and using discharge plasma sintering process, the problem of difficulty in combining ceramics and metals is solved, and the manufacturing of ceramics with high strength, toughness and complex structures is achieved. Suitable for aerospace and other fields.
Patent Information
- Application Number
- CN202410746127.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to effectively combine ceramics and metals with existing technology, especially in the application of complex structures and high-performance ceramics. The low toughness and processing difficulty of ceramic materials have limited their applications in aerospace and other fields.
By preparing metal lattice reinforced ceramics, alumina ceramics are combined with 3D printed titanium alloy lattice, and the discharge plasma sintering process is used to reduce the ceramic sintering temperature to achieve a good combination of ceramics and metals and the manufacture of complex structures.
It achieves a good combination of excellent mechanical properties and complex structures of ceramics and metals, enhances the toughness and impact resistance of ceramics, and is suitable for high-performance fields such as aerospace and aerospace.
Smart Images

Figure CN118745545A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a metal lattice reinforced ceramic and a preparation method thereof. Background Art
[0002] Ceramic materials have been widely used in many fields such as cutting tools, refractory materials, aerospace, etc. due to their excellent physical and chemical properties such as high hardness, high temperature resistance, and corrosion resistance. However, due to the inherent low toughness and high hardness of ceramic materials, on the one hand, they are prone to fracture due to stress concentration caused by surface or internal defects; on the other hand, they are difficult to process and it is difficult to manufacture complex structural parts. Compared with ceramic materials, metal materials have lower hardness and better toughness. The support and restraint of metals on ceramics can partially make up for the high brittleness of ceramic materials, thereby better exerting the excellent performance of ceramic materials.
[0003] Due to the different physical and chemical properties between metals and ceramics, such as thermal conductivity, thermal expansion coefficient, etc., the method of combining the two has always received widespread attention. Commonly used methods include diffusion bonding, brazing and liquid phase bonding. When using these methods to combine ceramics and metals, the ceramic and metal substrates are first prepared, and then the two are connected through an intermediate layer material. These methods can usually only be used for external bonding of simple-shaped substrates. In addition to using entities for external connection, some researchers also combine ceramics with metal materials by powder sintering, but the samples prepared by this method mostly use bioceramic materials for orthopedic implant research. The densification effect and mechanical properties of ceramics are generally limited to non-stress occasions, and cannot meet the application requirements of high-performance ceramics in cutting-edge industries such as aerospace and military protection. Therefore, developing a method for using metal-reinforced high-performance ceramics that can achieve good bonding of complex structures is a difficult problem that technicians in this field urgently need to solve. Summary of the invention
[0004] The purpose of the present invention is to provide a metal lattice reinforced ceramic and a preparation method thereof to solve the problems existing in the above-mentioned prior art. The metal lattice reinforced ceramic prepared by adjusting the raw materials and the preparation method of the present invention has high integrity and excellent mechanical properties, and the ceramic and the internal metal are well combined, and a good combination of complex structures can be achieved.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention: a metal lattice reinforced ceramic, comprising a plurality of metal reinforcement units coated with a ceramic material, wherein the plurality of metal reinforcement units are arranged in an array, adjacent metal reinforcement units are fixedly connected, and the plurality of metal reinforcement units are an integrated structure;
[0007] The ceramic material includes alumina ceramic.
[0008] Furthermore, the alumina ceramic comprises the following raw materials, in parts by weight: 90 to 99 parts of Al2O3, 0 to 10 parts of Y2O3, 0 to 10 parts of MgO, and 1 to 10 parts of Co.
[0009] The ceramic part prepared with the above raw materials has good comprehensive mechanical properties (high Vickers hardness and fracture toughness), which can ensure that the external ceramic has sufficient strength. In addition, the metal lattice reinforced ceramic obtained with the above raw materials has good integrity, no defects such as cracks in the ceramic part, good interface bonding, interconnected with the internal metal, and no fracture occurs in the ceramic and metal.
[0010] The second technical solution of the present invention is a method for preparing the above-mentioned metal lattice reinforced ceramic, comprising the following steps:
[0011] The raw materials of alumina ceramics are mixed and then ground to obtain ceramic powder;
[0012] The ceramic powder is spread flat in a mold, and then a metal reinforcement unit is placed on top of the ceramic powder. Subsequently, ceramic powder is added above and around the metal reinforcement unit to cover the metal reinforcement unit. Uniaxial pressure is applied and sintering is performed to obtain the metal lattice reinforced ceramic.
[0013] Furthermore, the sintering is spark plasma sintering;
[0014] The uniaxial pressure is 20-30 MPa.
[0015] Furthermore, the spark plasma sintering is carried out in an inert atmosphere, the sintering temperature is 1300-1450° C., the pressure is 0.05 MPa, the heating rate is 100° C. / min, and the holding time is 5 min.
[0016] Furthermore, the metal reinforcement unit is a 3D-printed titanium alloy lattice with a length and width of 20 to 25 mm, a height of 5 to 8 mm, and a diameter of 2.5 to 3.5 mm at the circular cross section.
[0017] Furthermore, the metal reinforcement unit includes three connecting columns, and the middle parts of the three connecting columns vertically intersect at one point.
[0018] Metal lattice reinforced ceramics are made by sintering metal reinforcement units wrapped with ceramic powder. If the ceramic filling amount is too little, it is impossible to completely cover the metal reinforcement units; if it is too much, the external ceramic will be too thick and the internal metal reinforcement units will lose their reinforcement effect. Therefore, the size of the final composite component is slightly larger than the internal metal entity size.
[0019] Furthermore, the length and width of the metal lattice reinforced ceramic are both 30 mm, and the height is 10 mm.
[0020] The sintering temperature of Al2O3 ceramics sintered by conventional sintering methods such as pressureless sintering and hot pressing is generally 1600-1700℃. The melting point of titanium alloy is about 1650℃. If the performance of Al2O3 ceramics is enhanced by titanium alloy lattice, the titanium alloy lattice will be deformed or melted due to the high sintering temperature. Therefore, it is difficult to achieve the effect of enhancing Al2O3 ceramics by titanium alloy lattice.
[0021] The present invention can reduce the sintering temperature of Al2O3 ceramics to 1300°C by regulating the components and the spark plasma sintering process. At this time, titanium alloy lattice is selected as the metal entity material inside the Al2O3 ceramic, which can effectively avoid the problem of deformation or melting of the titanium alloy lattice caused by excessively high sintering temperature. Therefore, the titanium alloy lattice can be used to enhance the mechanical properties of Al2O3 ceramics (to achieve support and constraint on the ceramics).
[0022] The third technical solution of the present invention: an application of the above-mentioned metal lattice reinforced ceramic in cutting tools, refractory materials or aerospace fields.
[0023] The present invention discloses the following technical effects:
[0024] (1) The metal lattice reinforced ceramic of the present invention is a composite of external ceramic and internal metal lattice, which fully utilizes the strength and toughness of metal. The internal metal lattice restrains and supports the ceramic, thereby enhancing the toughness and strengthening the ceramic, thereby compensating for the defect of high brittleness of the ceramic and preventing the problem of overall fracture caused by the high brittleness of the ceramic.
[0025] (2) The metal lattice reinforced ceramic of the present invention has excellent mechanical properties, with a relative density of 99.5%, a Vickers hardness of 19.35 GPa, and a fracture toughness of 4.03 MPa·m 1 / 2 The flexural strength reaches 479MPa; there are no obvious pores, fractures and other defects inside the ceramic and metal, and the bonding effect between ceramic and metal is good.
[0026] (3) The metal lattice reinforced ceramic of the present invention can be formed under one sintering condition, and the manufacturing process is simple and efficient, and has extremely high promotion and application value in the fields of armor protection, energy chemical industry, aerospace, etc. In addition, the metal lattice reinforced ceramic of the present invention can be mass-produced by conventional technology, with low manufacturing cost, and is easy to promote and apply.
[0027] (4) The preparation method of the present invention realizes the internal bonding of complex structure metal entities (the use of 3D printing to make metal entities can realize the manufacture of complex titanium alloy structures, which are connected inside the ceramic to achieve support and constraint on the ceramic) and ceramics, with good bonding effect and internal integrity, thereby enhancing the strength, toughness and impact resistance of the ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 Schematic diagram of the metal lattice enhanced ceramic spark plasma integral sintering of the present invention, wherein 1 is a graphite indenter, 2 is a graphite mold body, 3 is a titanium alloy lattice, and 4 is ceramic powder;
[0030] Figure 2 A three-dimensional model diagram of the metal lattice reinforced ceramic of the present invention;
[0031] Figure 3 This is a physical picture of the titanium alloy lattice used in Example 1 of the present invention and the prepared metal lattice reinforced ceramic;
[0032] Figure 4 The cross-sectional images of the metal lattice reinforced ceramic prepared in Example 1 of the present invention, wherein (a) is a longitudinal cross-sectional image and (b) is a cross-sectional image;
[0033] Figure 5 The cross-sectional images of the metal lattice reinforced ceramic prepared in Comparative Example 2 of the present invention, wherein (a) is a longitudinal cross-sectional image and (b) is a cross-sectional image;
[0034] Figure 6 These are cross-sectional images of the metal lattice reinforced ceramic prepared in Comparative Example 3 of the present invention, wherein (a) is a longitudinal cross-sectional image and (b) is a cross-sectional image. DETAILED DESCRIPTION
[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0036] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0038] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0039] The words “include,” “including,” “have,” “contain,” etc. used in this article are open-ended terms, meaning including but not limited to.
[0040] The “parts” described in the following examples are all “parts by weight”.
[0041] In a first aspect, the present invention provides a metal lattice reinforced ceramic, comprising a titanium alloy lattice coated with a ceramic material;
[0042] The ceramic material includes alumina ceramic.
[0043] The alumina ceramics used in the present invention include the following raw materials, calculated by weight: 90-99 parts of Al2O3, 0-10 parts of Y2O3, 0-10 parts of MgO, and 1-10 parts of Co.
[0044] In a second aspect, the present invention provides a method for preparing the above-mentioned metal lattice reinforced ceramic, comprising the following steps:
[0045] (1) The raw materials of alumina ceramics were mixed, and anhydrous ethanol was used as a medium (the weight ratio of the raw materials to anhydrous ethanol was 1:3) for 1 to 2 hours of ultrasonic oscillation (the power of ultrasonic oscillation was 200 W) and stirring (the stirring speed was 150 r / min) to obtain a slurry. The slurry was vacuum dried at 120° C. for 2 hours, ground, and passed through a 100-mesh sieve to obtain a ceramic powder.
[0046] (2) Ultrasonic cleaning and drying of the 3D printed titanium alloy lattice.
[0047] (3) First, the ceramic powder prepared in step (1) is added to the mold, and then the titanium alloy lattice is placed on the ceramic powder, and then the ceramic powder prepared in step (1) is added on top, and a graphite mold pressure head is pressed and a uniaxial sintering pressure of 20 to 30 MPa is applied. Then, the spark plasma sintering furnace is purged once, evacuated to 40 Pa, and then filled with argon protective atmosphere to 0.05 MPa, and rapidly heated to 1300 to 1450°C at a heating rate of 100°C / min, and kept at a constant pressure for 5 minutes (for spark plasma sintering), and then the pressure is slowly released to 0.1 MPa, and the contact pressure is maintained at about 0.1 MPa (i.e., the uniaxial sintering pressure is reduced to about 0.1 MPa) and cooled to room temperature with the furnace.
[0048] The length and width of the 3D-printed titanium alloy lattice (lattice frame) used in the present invention are both 20 to 25 mm, the height is 5 to 8 mm, and the diameter of the circular cross section is 2.5 to 3.5 mm.
[0049] Furthermore, the titanium alloy lattice includes three connecting columns, and the middle parts of the three connecting columns vertically intersect at one point.
[0050] The length and width of the metal lattice reinforced ceramic prepared by the invention are both 30 mm, and the height is 10 mm.
[0051] A third aspect of the present invention provides an application of the above-mentioned metal lattice reinforced ceramic in the field of cutting tools, refractory materials or aerospace.
[0052] The raw materials such as Al2O3, Y2O3 and MgO used in the present invention are all common commercial products.
[0053] The schematic diagram of the metal lattice enhanced ceramic spark plasma integral sintering of the present invention is shown in Figure 1 . Figure 1 In the figure, 1 is a graphite pressing head, 2 is a graphite mold body, 3 is a titanium alloy lattice, and 4 is a ceramic powder.
[0054] The three-dimensional model diagram of the metal lattice reinforced ceramic of the present invention is shown in Figure 2 .
[0055] Example 1
[0056] A method for preparing metal lattice reinforced ceramics:
[0057] (1) 95 parts of Al2O3 powder and 5 parts of Co powder were mixed and placed in a conical flask, and then anhydrous ethanol was added to the conical flask (the weight ratio of powder to anhydrous ethanol was 1:3), and the conical flask was placed in an ultrasonic oscillator for 2 h of ultrasonic oscillation (the power of ultrasonic oscillation was 200 W) and stirring (stirring speed was 150 r / min) to obtain a slurry, which was vacuum dried at 120°C for 2 h, and after cooling, ground in an agate mortar and sieved through a 100-mesh sieve to obtain a ceramic powder.
[0058] (2) Place the 3D printed titanium alloy lattice (length and width are both 24 mm, height is 7 mm, and diameter of the circular cross section is 2.8 mm) into a beaker, add anhydrous ethanol to the beaker to cover the titanium alloy lattice, and then place the beaker in an ultrasonic oscillator for ultrasonic cleaning for 2 minutes. After taking out the titanium alloy lattice, use a hot air blower to blow it dry.
[0059] (3) Graphite paper (thickness of 0.2 mm) is laid on the inner wall of a graphite mold with a square cross-section and an inner side length of 30.4 mm. Half of the weight of the ceramic powder is weighed so that the overall thickness of the sample after sintering is 10 mm. The weighed ceramic powder is poured into the graphite mold and the ceramic powder is laid flat in the mold by knocking and vibrating. Then, the cleaned and dried titanium alloy lattice is placed flat on the ceramic powder. The remaining half of the weight of the ceramic powder is weighed so that the overall thickness of the sample after sintering is 10 mm. The weighed ceramic powder is poured into the mold and laid on the titanium alloy lattice. The graphite mold indenter is pressed and pressed on the mold jacket. Insulated carbon felt, the mold is placed in a spark plasma sintering furnace for sintering, and a uniaxial sintering pressure of 25MPa is applied. Before sintering, it is first purged once, and then vacuumed to 40Pa and filled with argon protective atmosphere to 0.05MPa, and then rapidly heated to 1300℃ at a heating rate of 100℃ / min, and kept at a constant pressure for 5min (spark plasma sintering), and then the pressure is slowly released to 0.1MPa, and the contact pressure is maintained at about 0.1MPa (that is, the uniaxial sintering pressure is reduced to about 0.1MPa) and cooled to room temperature with the furnace, and finally the sintered sample is taken out, the graphite paper is polished to remove, and the metal lattice reinforced ceramics are obtained.
[0060] The actual picture of the titanium alloy lattice used in this embodiment and the prepared metal lattice reinforced ceramic is shown in Figure 3 .
[0061] Example 2
[0062] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1350°C.
[0063] Example 3
[0064] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1400°C.
[0065] Example 4
[0066] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1350° C. and the uniaxial sintering pressure is 20 MPa.
[0067] Example 5
[0068] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1400° C. and the uniaxial sintering pressure is 20 MPa.
[0069] Example 6
[0070] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1300° C. and the uniaxial sintering pressure is 30 MPa.
[0071] Example 7
[0072] Same as Example 1, except that in step (1), the amount of Al2O3 powder is 90 parts and the amount of Co powder is 10 parts;
[0073] In step (3), the temperature of spark plasma sintering is 1350°C.
[0074] Example 8
[0075] Same as Example 1, except that the raw materials and amounts in step (1) are: 97.2 parts of Al2O3 powder, 1.4 parts of MgO powder, 1.4 parts of Y2O3 powder, and 10 parts of Co powder;
[0076] In step (3), the temperature of spark plasma sintering is 1350°C.
[0077] Effect Example 1
[0078] (1) Mechanical properties of metal lattice reinforced ceramics
[0079] The metal lattice reinforced ceramics prepared in Examples 1 to 8 were respectively taken, and the densification degree and mechanical properties of the ceramic parts were tested. The test results are shown in Table 1.
[0080] Table 1 Mechanical properties of metal lattice reinforced ceramics
[0081]
[0082]
[0083] The three-point bending strength test was carried out on Al2O3 ceramics, Al2O3 / 5wt.%Co ceramics and the metal lattice reinforced ceramics prepared in Example 1. The test results are shown in Table 2.
[0084] Table 2 Flexural strength test results
[0085] sample <![CDATA[Al2O3]]> <![CDATA[Al2O3 / 5wt.%Co]]> Example 1 Flexural strength(MPa) 355 412 479
[0086] The preparation methods of the Al2O3 ceramics and Al2O3 / 5wt.%Co ceramics in Table 2 are as follows:
[0087] Preparation method of Al2O3 ceramics: 97.2 parts of Al2O3 powder, 1.4 parts of MgO powder, and 1.4 parts of Y2O3 powder (the Al2O3 ceramic performance of this component is the best) are mixed and placed in a conical flask, and then anhydrous ethanol is added to the conical flask (the weight ratio of powder to anhydrous ethanol is 1:3), and the conical flask is placed in an ultrasonic oscillator for 2h ultrasonic oscillation (the power of ultrasonic oscillation is 200W) and stirring (stirring speed is 150r / min) to obtain slurry, and the slurry is vacuum dried at 120℃ for 2h, and after cooling, it is ground in an agate mortar and passed through a 100-mesh sieve to obtain Al2O3 ceramic powder. Graphite paper is laid on the inner wall of the graphite mold, and the prepared ceramic powder is poured into the mold. The mold is placed in a spark plasma sintering furnace, and sintered after washing. The heating rate is 100℃ / min, the sintering temperature is 1400℃, the sintering pressure is 25MPa, and the heat preservation is 5min (this process is the best sintering process for this ceramic).
[0088] Preparation method of Al2O3 / 5wt.%Co ceramic: 95 parts of Al2O3 powder and 5 parts of Co powder (the same ceramic components as those in Example 1) are mixed and placed in a conical flask, and then anhydrous ethanol (the weight ratio of powder to anhydrous ethanol is 1:3) is added to the conical flask, and the conical flask is placed in an ultrasonic oscillator for 2h ultrasonic oscillation (the power of ultrasonic oscillation is 200W) and stirring (stirring speed is 150r / min) to obtain a slurry, and the slurry is vacuum dried at 120℃ for 2h, ground in an agate mortar after cooling, and passed through a 100-mesh sieve to obtain Al2O3 / 5wt.%Co ceramic powder. Graphite paper is laid on the inner wall of a graphite mold, and the prepared ceramic powder is poured into the mold, and the mold is placed in a discharge plasma sintering furnace, and sintered after washing, with a heating rate of 100℃ / min, a sintering temperature of 1300℃, a sintering pressure of 25MPa, and a heat preservation of 5min (this process is the best sintering process for the ceramic).
[0089] (2) Internal integrity
[0090] The metal lattice reinforced ceramics prepared in each embodiment were subjected to computer tomography (CT) tests. The cross-sectional image of the metal lattice reinforced ceramic prepared in Example 1 was taken. The results are shown in FIG. Figure 4 , where (a) is the longitudinal section image and (b) is the cross-sectional image.
[0091] from Figure 4 It can be seen that the use of the raw materials and preparation method of the present invention can significantly reduce the pore volume between the metal and the ceramic, improve the bonding effect between the metal and the ceramic, and improve the internal integrity of the metal lattice reinforced ceramic. The metal lattice reinforced ceramics prepared in other embodiments of the present invention can also achieve the same effect.
[0092] Comparative Example 1
[0093] The same as Example 1, except that in step (3), the spark plasma sintering temperature is 1250°C.
[0094] The metal lattice reinforced ceramic prepared in this comparative example failed to achieve densification of the ceramic part due to the low sintering temperature, resulting in a low Vickers hardness (16.89 GPa).
[0095] Comparative Example 2
[0096] The same as Example 1, except that in step (1), the raw materials for preparing the ceramic are: 97.2 parts of Al2O3 powder, 1.4 parts of Y2O3 powder, and 1.4 parts of MgO powder.
[0097] In step (3), the spark plasma sintering temperature is 1350° C., and the uniaxial sintering pressure (25 MPa) is maintained until cooling to room temperature.
[0098] The metal lattice reinforced ceramic prepared in this comparative example has cracks inside the lattice, and there are obvious pores between the lattice and the ceramic. The integrity and bonding effect of the metal lattice are poor. Figure 5 , where (a) is the longitudinal section image and (b) is the cross-sectional image.
[0099] Comparative Example 3
[0100] The same as Example 1, except that in step (1), the raw materials for preparing the ceramic are: 97.2 parts of Al2O3 powder, 1.4 parts of Y2O3 powder, and 1.4 parts of MgO powder.
[0101] In step (3), the temperature of spark plasma sintering is 1400°C.
[0102] The metal lattice reinforced ceramic prepared in this comparative example has cracks inside the metal lattice, and the integrity of the metal lattice is poor. Figure 6 , where (a) is the longitudinal section image and (b) is the cross-sectional image.
[0103] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A metal lattice reinforced ceramic, characterized in that: It comprises a plurality of metal reinforcement units coated with ceramic material, wherein the plurality of metal reinforcement units are arranged in an array, adjacent metal reinforcement units are fixedly connected, and the plurality of metal reinforcement units are an integrated structure; The ceramic material includes alumina ceramic.
2. The metal lattice reinforced ceramic according to claim 1, characterized in that: The alumina ceramic comprises the following raw materials, in parts by weight: 90 to 99 parts of Al2O3, 0 to 10 parts of Y2O3, 0 to 10 parts of MgO, and 1 to 10 parts of Co.
3. A method for preparing the metal lattice reinforced ceramic according to any one of claims 1 to 2, characterized in that: The following steps are involved: The raw materials of alumina ceramics are mixed and then ground to obtain ceramic powder; The ceramic powder is spread flat in a mold, and then a metal reinforcement unit is placed on top of the ceramic powder. Subsequently, ceramic powder is added above and around the metal reinforcement unit to cover the metal reinforcement unit. Uniaxial pressure is applied and sintering is performed to obtain the metal lattice reinforced ceramic.
4. The preparation method according to claim 3, characterized in that: The sintering is spark plasma sintering; The uniaxial pressure is 20-30 MPa.
5. The preparation method according to claim 4, characterized in that: The spark plasma sintering is carried out in an inert atmosphere, with a sintering temperature of 1300-1450° C., a pressure of 0.05 MPa, a heating rate of 100° C. / min, and a heat preservation time of 5 min.
6. Use of the metal lattice reinforced ceramic according to any one of claims 1 to 2 in cutting tools, refractory materials or aerospace fields.
Citation Information
Patent Citations
Metal and ceramic composite material and preparation method of metal and ceramic composite material
CN102700192A
Ceramic particle enhanced metal-based composite material and preparation method thereof
CN104593627A
Preparation method for ceramic particle reinforced metallic matrix space lattice composite material
CN109022882A
Metal-ceramic composite lattice manufacturing method and metal-ceramic composite lattice structure
CN114226755A
Preparation method of high-entropy alloy / ceramic composite lattice structure
CN115572153A
Cited By
Ceramic composite material and preparation method thereof
CN121735663A