EH690-grade maritime work steel and manufacturing method thereof
By optimizing the alloy composition and process design, we solved the problems of high thickness and cost of marine steel in the existing technology, and developed low-cost and high-performance EH690 grade marine steel, which achieved high strength, low-temperature toughness and good welding performance of the steel plate, meeting the requirements Thickness and performance requirements for marine engineering.
Patent Information
- Application Number
- CN202410851193.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing high-performance EH690 grade marine steel products have small thickness specifications, high production costs, and complex heat treatment processes, making them unsuitable for mass production.
By optimizing the coupling design of alloy composition and smelting, controlled rolling, controlled cooling and quenching and tempering heat treatment processes, a low-cost, high-performance EH690 grade marine steel with a maximum thickness of 60mm was developed, using LF refining and RH refining, and four-stage hot rolling. Preparation, DQ+ACC rapid cooling and off-line quenching + tempering processes form tempered martensite + bainite microstructure.
It achieves the ultra-high strength, low-temperature toughness and good welding performance of the steel plate. The yield strength of the finished steel plate is ≥690MPa, the tensile strength is 770-940MPa, the low-temperature fracture CTOD characteristic value is ≥0.5mm, the Z-direction shrinkage rate is ≥65%, and the maximum thickness is up to 60mm, suitable for marine engineering needs.
Smart Images

Figure CN118745558A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of offshore steel production, and in particular to a low-cost, high-performance EH690-grade offshore steel and a manufacturing method thereof. Background Art
[0002] In recent years, with the continuous exploration and development of the ocean, the steel materials and R&D and production required for the corresponding ships and marine engineering have received increasing attention; with the increasing requirements for large-scale development of marine equipment, ultra-deepwater operation safety of offshore platforms and lightweight marine equipment, the performance requirements for steel used in marine engineering equipment are also increasing, such as the need to design lighter and thinner load-bearing structures, thereby reducing the center of gravity of the platform, improving stability, reducing welding volume, and increasing the payload of important equipment and improving equipment efficiency. In order to meet the demand for high-performance steel plates in marine engineering, it is urgent to develop low-cost, high-performance EH690 grade marine steel.
[0003] The Chinese invention patent with the authorization announcement number CN 102226255 B discloses a "yield strength 690MPa high-toughness steel plate and its preparation process". The yield strength of the ship plate steel is not less than 690MPa, with good low-temperature (-80℃) impact toughness, and the thickness is 50-100mm. It is suitable for ships and offshore oil platforms, especially for ship plate manufacturing processes that require high strength and low-temperature toughness and good welding performance. However, the Cu content of the steel plate is 1.00%-1.50%, which exceeds the design specification requirements of existing ship-grade steel plates, and the Ni content is high, resulting in increased production costs, which is not conducive to promotion and application.
[0004] The Chinese invention patent with authorization announcement number CN 109652733 B discloses "a 690MPa grade extra-thick steel plate and its manufacturing method". It adopts die casting and then forging the slab and rolling and heat treatment the forged slab, so that the obtained extra-thick steel plate has excellent core mechanical properties and lamellar tearing resistance with high strength, high plasticity and high toughness, which can meet the demand for high-performance extra-thick steel plates in harsh service environments such as marine engineering, but its process is complicated and not suitable for mass production.
[0005] The Chinese invention patent with authorization announcement number CN 102888571 B discloses "a 690MPa-grade low welding crack sensitivity steel and its manufacturing method". Through reasonable composition design, Pcm.20 is guaranteed. Two-stage controlled rolling, controlled cooling and reasonable heat treatment process are adopted to obtain a steel plate with a tensile strength of ≥90MPa. However, the thickness of the finished product is only 15 to 30mm, which cannot meet the demand for large thickness specifications of ultra-high-strength marine engineering steel used in marine engineering platform equipment.
[0006] From the above prior art, it can be seen that the currently available high-performance EH690 grade marine steel has the following deficiencies:
[0007] 1. The product thickness is too small to meet the requirements of large thickness specifications;
[0008] 2. High precious metal content or complex heat treatment process, resulting in high production costs;
[0009] In view of the above shortcomings, the present invention optimizes the alloy content and adopts the coupling design of alloy composition and smelting + controlled rolling + controlled cooling + tempering heat treatment process, and finally obtains a low-cost, high-performance EH690 grade marine steel with a maximum thickness of 60 mm. Summary of the invention
[0010] The invention provides an EH690-grade marine engineering steel and a manufacturing method thereof. Through the alloy composition-deformation-heat treatment process coupling design, the product has good comprehensive mechanical properties, and solves the problem that the strength, plasticity and low-temperature toughness (-40°C) of a 690MPa-grade steel plate are difficult to match and reconcile; the finished steel plate has the characteristics of ultra-high strength (yield strength ≥690MPa, tensile strength 770-940MPa, elongation after fracture ≥14%), excellent low-temperature toughness (-40°C core impact energy ≥100J), excellent low-temperature fracture toughness (-10°C low-temperature fracture CTOD characteristic value ≥0.5mm), excellent Z-direction performance (Z-direction section shrinkage ≥65%), uniform organizational performance, and good plate shape (steel plate unevenness ≤4mm / 2m).
[0011] In order to achieve the above object, the present invention adopts the following technical solutions:
[0012] An EH690 grade marine steel, the chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.10%-0.16%; Si: 0.15%-0.40%; Mn: 1.00%-1.50%; P≤0.012%; S≤0.002%; Ni: 0.25%-0.50%; Cr: 0.50%-0.90%; Nb: 0.015%-0.04%; Mo: 0.25%-0.50%; Ti: 0.007%-0.015%; B: 0.000 7%~0.002%; Als: 0.04%~0.08%; O≤0.001%; N≤0.004%; H≤0.002%; the balance is Fe and unavoidable impurities; Ceq≤0.64%, Pcm≤0.33%; wherein, Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5, Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B.
[0013] A method for manufacturing EH690 grade marine engineering steel, the process route includes smelting and slow cooling of ingot, controlled rolling, controlled cooling and off-line quenching and tempering heat treatment; wherein the following processes are controlled:
[0014] 1) Smelting and slow cooling of ingots;
[0015] LF refining and RH refining are 20-40 minutes each, the superheat of molten steel in the tundish is 22-28℃, the gas content is controlled to be [N]≤40ppm, [O]≤10ppm, [H]≤2.0ppm; full protection casting, various inclusions in the steel meet the following requirements: Class A inclusions ≤1.0 level, Class B inclusions ≤1.0 level, Class C inclusions ≤1.0 level, Class D inclusions ≤1.0 level; light reduction is adopted in the continuous casting billet forming process, and the reduction amount is 6-8mm; after the continuous casting billet is off the line, it is stacked and slowly cooled, and the stacking temperature is ≥600℃, and the time is ≥48h;
[0016] 2) Controlled rolling;
[0017] The continuous casting billet is heated in four stages, including the first heating stage, the second heating stage, the third heating stage and the soaking stage; the upper and lower heating temperatures of each heating stage and the soaking stage are controlled separately; the total heating time of the continuous casting billet is 10-12min / mm; the starting rolling temperature is 950-1000℃, and the single pass reduction rate is ≥15% except the widening pass; the second stage starting rolling temperature is 720-760℃, the single pass reduction rate is ≥11%, and the final rolling temperature is 680-720℃;
[0018] 3) Controlled cooling;
[0019] After final rolling, the steel plate is directly cooled by DQ+ACC rapid cooling system, with an average cooling rate of ≥10℃ / s and a return temperature of 200~300℃;
[0020] 4) Offline quenching and tempering heat treatment;
[0021] Quenching: The steel plate is subjected to quenching heat treatment, the quenching heating temperature is 860-910°C, the heating rate is 1.3-2min / mm, the holding time is 20-40min, and the steel plate is quenched in water to room temperature after being taken out of the furnace;
[0022] Tempering: The steel plate is tempered at a temperature of 580-630°C and a furnace time of 3-4.5 min / mm. After being taken out of the furnace, it is air-cooled to obtain a finished steel plate.
[0023] In the step 2), the lower heating temperature of the first heating section is 1000-1120°C, and the upper heating temperature of the first heating section is 1050-1180°C; the lower heating temperature of the second heating section is 1130-1180°C, and the upper heating temperature of the second heating section is 1180-1220°C; the lower heating temperature of the third heating section is 1150-1200°C, and the upper heating temperature of the third heating section is 1200-1250°C; the lower heating temperature of the soaking section is 1050-1150°C, and the upper heating temperature of the soaking section is 1150-1200°C.
[0024] In the step 2), after the continuous casting billet is taken out of the furnace, high-pressure water is used to remove phosphorus for 2 to 3 times.
[0025] In the step 2), the intermediate billet thickness is 2 to 2.5 times the thickness of the finished steel plate, and the intermediate billet is water-cooled at a cooling rate of ≥4°C / s.
[0026] The microstructure of the finished steel plate is tempered martensite + bainite, and the grain size is ≥ grade 7.
[0027] The yield strength of the finished steel plate is ≥690MPa, the tensile strength is 770~940MPa, the section elongation is ≥14%, the Z-direction section shrinkage is ≥65%, the -40℃ Charpy impact energy of the steel plate core is ≥100J, and the -10℃ low-temperature fracture CTOD characteristic value is ≥0.5mm.
[0028] The maximum thickness of the finished steel plate is 60mm.
[0029] The unevenness of the finished steel plate is ≤4mm / 2m.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention adopts the alloy composition-deformation-heat treatment process coupling design to make the product have good comprehensive mechanical properties, solve the problem that the strength, plasticity and low-temperature toughness (-40°C) of 690MPa grade steel plates are difficult to match and reconcile. The yield strength of the finished steel plate is ≥690MPa, the tensile strength is 770-940MPa, the cross-sectional elongation is ≥14%, the Z-direction cross-sectional shrinkage is ≥65%, the -40°C Charpy impact energy of the steel plate core is ≥100J, and the low-temperature fracture toughness is excellent (-10°C low-temperature fracture CTOD characteristic value is ≥0.5mm);
[0032] (2) The present invention gives full play to the technical equipment advantages of the wide and thick plate rolling mill and the heat treatment unit, and combines the 250-300 mm thick continuous casting slab to develop an ultra-high strength and high toughness marine steel plate with a maximum thickness of 60 mm;
[0033] (3) A reasonable rolling process is used in combination with the offline quenching and tempering (quenching + high temperature tempering) process. Compared with the TMCP or TMCP+T process commonly used for existing steel plates of the same strength, offline quenching can accurately control the starting temperature of quenching, and the temperature of the entire plate is uniform; it is also easier to control the flatness of the plate, and the unevenness of the finished steel plate within 2 meters is ≤4mm;
[0034] (4) The microstructure of the steel plate is tempered martensite / bainite, and the grain size is ≥7. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a metallographic structure photograph of the finished steel plate in Example 2 of the present invention (magnified 500 times).
[0036] Figure 2 This is a grain size photograph of the finished steel plate in Example 2 of the present invention (magnified 500 times). DETAILED DESCRIPTION
[0037] The EH690 grade marine engineering steel and its manufacturing method described in the present invention are designed from the aspects of alloy element selection and proportioning, steel cleanliness control, continuous casting process control, heating and controlled rolling and cooling, quenching and tempering heat treatment process optimization, microstructure strength and toughness matching, and finally determine the component system and manufacturing process that can meet the purpose of the present invention. The details are as follows:
[0038] Low-cost, high-performance EH690 grade marine engineering steel, characterized in that the chemical composition mass percentage of the steel plate is as follows: C: 0.10% to 0.16%; Si: 0.15% to 0.40%; Mn: 1.00% to 1.50%; P≤0.012%; S≤0.002%; Ni: 0.25% to 0.50%; Cr: 0.50% to 0.90%; Nb: 0.015% to 0.04%; Mo: 0.25% to 0.50%; Ti: 0.007% to 0.015%; B :0.0007%~0.002%;Als:0.04%~0.08%;O≤0.001%;N≤0.004%;H≤0.002%;the balance is Fe and unavoidable impurities;Ceq≤0.64%, Pcm≤0.33%;wherein, Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5,Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B.
[0039] The mechanism of action of each alloy component in the steel of the present invention is as follows:
[0040] C: It is a necessary and cheap element to ensure strength and hardenability. It has a significant effect on improving the strength of steel through solid solution strengthening and precipitation strengthening. However, as the carbon content increases, the plasticity, low-temperature toughness and welding crack sensitivity of the steel plate will be significantly reduced. With a low carbon content, the hardness and strength of the steel after quenching and tempering are low, but the plasticity and toughness are high. From the perspective of economy and product performance, the present invention controls the C content in the steel to 0.10% to 0.16%.
[0041] Si: It is a solid solution strengthening element. Although Si is beneficial to improving the strength of the steel plate and the oxidation resistance at high temperature, Si will promote the coarsening of the packet size, seriously damaging the low-temperature toughness, elongation and weldability of the ultra-high strength steel plate. Taking into account the economy and operability of steelmaking, the present invention controls the Si content in the steel to 0.15% to 0.40%.
[0042] Mn: As the most important alloying element, in addition to improving the strength of the steel plate, it also has the effect of expanding the austenite phase region, reducing the Ar3 point temperature, and refining the ferrite grains, thereby improving the low-temperature toughness of the steel plate; but when the Mn element content is too high, Mn segregation and strip-shaped MnS are easily formed, resulting in poor low-temperature toughness and lamellar tearing resistance in the core of the thick plate, and reduced performance of the welding heat-affected zone; therefore, the present invention controls the Mn content in the steel to 1.00% to 1.50%.
[0043] P: is an element that has an adverse effect on the impact value. It will segregate in the center of the slab and gather at the grain boundaries to impair the low-temperature toughness. The P content in the steel is controlled to be no higher than 0.012% in the present invention.
[0044] S: is an element that has an adverse effect on the impact value and can form sulfide inclusions and become a crack source. In the present invention, the S content in the steel is controlled to be no higher than 0.002%.
[0045] Ni: Nickel dissolves in austenite, which can inhibit austenite recrystallization, refine austenite grains, and improve the low-temperature toughness of steel plates. Ni can reduce the diffusion rate of each element in steel, thereby delaying the decomposition and transformation of austenite, and further improving the permeability of steel. When Ni and Mo are added at the same time, the toughness of steel can be improved while increasing the strength of steel, but when the Ni element is too high, Ceq and Pcm will be increased, affecting the welding performance; therefore, the present invention controls the Ni content in steel to 0.25% to 0.50%.
[0046] Cr: It can improve the hardenability and strength of the steel plate. The presence of Cr element can enhance the tempering stability of the steel and ensure that the steel obtains tempered bainite / martensite structure during high temperature tempering. Cr has similar solid solution strengthening effect as Mn and is not easy to segregate. Too high Cr content will increase the tendency of temper brittleness and increase the difficulty of welding; while too low Cr content will not effectively play its strengthening role. The present invention controls the Cr content in the steel to 0.50% to 0.90%.
[0047] Nb: Niobium is added to refine the grain size after quenching, thereby effectively refining the microstructure and strengthening the matrix through precipitation. The composite addition of Nb and B can effectively inhibit the recrystallization of austenite during rolling to refine the grains while inhibiting the diffusion of C, thereby effectively inhibiting the precipitation of M23 (C, B) 6 at the austenite grain boundary, ensuring the effective segregation of B at the ferrite nucleation position, improving the hardenability of the steel, and making the steel have higher strength and better low-temperature toughness. The addition of Nb and the formation of Nb (C, N) in the steel inhibit the appearance of M23 (C, B) 6 coarse structure. While reducing C diffusion and improving the utilization efficiency of B, it can also promote the homogenization of the structure. However, when the Nb content exceeds a certain range, the HAZ after welding will form MA islands, which is not conducive to the toughness of the steel. The present invention controls the Nb content in the steel to 0.015% to 0.04%.
[0048] Mo: can make the C curve of steel shift and thus significantly improve the hardenability of steel, promote the formation of martensite or bainite with a large number of dislocations in the crystal within a large cooling range, produce phase transformation strengthening and dislocation strengthening, and significantly improve the strength and structural uniformity of steel. In the present invention, Mo and Nb elements are added in combination, in addition to the strengthening effect of adding molybdenum and niobium separately, molybdenum can also segregate on the NbC matrix interface, preventing the coarsening of NbC particles. Mo and B are added in combination, which can increase the content of effective (solid solution) B in steel, inhibit the diffusion of C to the grain boundary, inhibit the precipitation and growth of M23 (C, B) 6 at the grain boundary, promote the segregation of B at the grain boundary, reduce the nucleation core of ferrite, and improve the hardenability of steel. Mo and Ni are added in combination, which can improve the toughness of steel while improving the strength of steel. However, when the Mo element is increased, the number of Mo-containing carbides also increases, and the Mo-containing carbides distributed at the grain boundary destroy the continuity of the matrix and deteriorate the toughness of steel. Therefore, the present invention controls the Mo content in the steel to be between 0.25% and 0.50%.
[0049] Ti: It inhibits excessive growth of austenite grains during slab heating and improves the toughness of steel. At the same time, Ti has the function of fixing N, ensuring that there is a certain amount of solid solution B in the steel and improving the hardenability of the steel plate. However, when the Ti element content is too high, the excess Ti is easy to precipitate as TiC on the martensite / bainite laths and on the grain boundaries, which seriously deteriorates the low-temperature toughness of the steel plate. Therefore, the present invention controls the Ti content in the steel to 0.007% to 0.015%.
[0050] B: can improve the hardenability and strength of the steel plate, but too high a content of the B element will form coarse BN particles that are detrimental to the hardenability and toughness, and will also affect the weldability and surface quality of the steel plate. Therefore, the present invention controls the Mo content in the steel to 0.0007% to 0.002%.
[0051] Als: deoxidizing and grain refining element. Al forms fine AlN precipitation at high temperature, which inhibits the growth of austenite grains when the slab / steel plate is heated for austenitization, thereby refining austenite grains and improving the toughness of steel at low temperatures. At the same time, because the excess Als in the steel can fix the free [N] in the steel, it can ensure that there is a certain amount of solid solution B in the steel, thereby improving the hardenability of the steel plate. Therefore, the added content needs to be above 0.04%; however, too high Al content will lead to the formation of larger Al oxides, reducing the low-temperature impact performance of the steel plate, and the casting is prone to cracks at the corners during the continuous casting process. Therefore, the present invention controls the Alt content in the steel to 0.04% to 0.08%.
[0052] O: An element that has an adverse effect on impact toughness. It combines with other elements in steel to form non-metallic inclusions and becomes a crack source. The present invention controls the O content in steel to below 10 ppm.
[0053] N: The N element will form BN with the B element, and form coarse ALN with the Al element, which will precipitate along the original austenite grain boundary, affecting the hardenability and low-temperature impact toughness of the steel. The present invention controls the N content in the steel to be below 40 ppm.
[0054] H: The most harmful element in steel. When the cooling speed is too fast, the high-pressure hydrogen cannot be precipitated out of the steel in time. The tension of high-pressure hydrogen and other stresses may exceed the material's σ b Therefore, many microcracks are generated, and round or oval silvery white spots appear on the longitudinal section of the steel, which are called "white spots". They are actually staggered small cracks. The present invention controls the H content in the steel to below 2ppm.
[0055] The key to the preparation of the EH690 grade marine engineering steel described in the present invention lies in the following steps:
[0056] 1) Smelting and slow cooling of ingots;
[0057] Select smelting raw materials. The raw materials should be mainly molten iron or high-quality return steel. The content of elements such as P and S should be as low as possible. The smelting composition should be controlled according to the target value. The residual element content should be strictly controlled to avoid the carbon equivalent exceeding the upper limit. LF refining and RH refining should be processed for 20 to 40 minutes each. The superheat of the molten steel in the tundish is 22 to 28°C. The residual element content should be strictly controlled, and the gas content should be controlled to be [N] ≤ 40ppm, [O] ≤ 10ppm, and [H] ≤ 2.0ppm. The casting should be protected throughout the process. The inclusions of Class A, B, C, and D in the steel should meet the requirements of Class A inclusions ≤ 1.0 level, Class B inclusions ≤ 1.0 level, Class C inclusions ≤ 1.0 level, and Class D inclusions ≤ 1.0 level. The continuous casting billet forming process adopts light reduction technology with a reduction of 6 to 8 mm, which can effectively solve the center segregation of the continuous casting billet; the continuous casting billets are stacked and slowly cooled after they come off the line, with the stacking temperature ≥ 600°C and the time ≥ 48h. The slow cooling of the continuous casting billets can improve the cracks of the continuous casting billets on the one hand, and the hydrogen embrittlement sensitivity of the product on the other hand, thereby improving the product performance.
[0058] 2) Controlled rolling;
[0059] The continuous casting billet is heated in four sections, and the four heating sections are heating section 1, heating section 2, heating section 3 and soaking section. The upper and lower temperatures of each section of the heating furnace are controlled separately. Specifically, the lower heating temperature of heating section 1 is 1000-1120℃, and the upper heating temperature of heating section 1 is 1050-1180℃; the lower heating temperature of heating section 2 is 1130-1180℃, and the upper heating temperature of heating section 2 is 1180-1220℃; the lower heating temperature of heating section 3 is 1150-1200℃, and the upper heating temperature of heating section 3 is 1200-1250℃; the lower heating temperature of soaking section is 1050-1150℃, and the upper heating temperature of soaking section is 1150-1200℃; the total heating time of continuous casting billet is 10-12min / mm. By controlling the heating in sections, the internal heating unevenness caused by overheating of the billet can be avoided, and at the same time, the C and N compounds can be fully dissolved to avoid abnormal growth of the cast structure.
[0060] After the continuous casting billet is taken out of the furnace, high-pressure water is used to remove phosphorus for 2 to 3 times to remove the surface iron oxide scale and reduce the temperature of the continuous casting billet; the starting rolling temperature is 950-1000℃, and the single-pass reduction rate is ≥15% except for the widening pass, which improves the as-cast structure of the slab, reduces the thickness of the billet waiting for temperature, and shortens the waiting time of the steel plate. The thickness of the intermediate billet is 2 to 2.5 times the thickness of the finished product, and the intermediate billet is water-cooled at a cooling rate of ≥4℃ / s. The second-stage starting rolling temperature is 720-760℃, the single-pass reduction rate is ≥11%, and the final rolling temperature is 680-720℃; the as-cast structure of the slab can be improved by rolling in the high-temperature section. The two-stage controlled rolling can promote the flattening and refinement of austenite grains. The phase change structure is uniformly refined through two-stage rolling to prepare the initial structure for quenching and tempering heat treatment.
[0061] 3) Controlled cooling;
[0062] After final rolling, the steel plate is directly cooled by the DQ+ACC rapid cooling system, with an average cooling rate of ≥10℃ / s and a red-return temperature of 200-300℃. The original structure is refined by combining the large deformation rolling process + post-rolling cooling process.
[0063] 4) Offline quenching and tempering heat treatment;
[0064] Quenching: The steel plate is subjected to quenching heat treatment, wherein the quenching heating temperature is controlled between 860 and 910°C, the heating rate is 1.3 to 2 min / mm, the heat preservation is 20 to 40 min, and the steel plate is taken out of the furnace and water quenched to room temperature. The quenching process is used to obtain the effect of homogenizing the original austenite grain size on the full thickness section of the thick steel plate.
[0065] Tempering: The steel plate is tempered at a temperature of 580-630°C and a furnace time of 3-4.5 min / mm. After being taken out of the furnace, it is air-cooled to obtain the finished steel plate. By controlling the tempering process, the composition of the phase change structure, the uniform refinement degree and the precipitation behavior of multiphase particles are controlled and adjusted, and the low-temperature impact toughness and low-temperature fracture resistance (CTOD) of the steel plate are improved.
[0066] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.
[0067] [Example]
[0068] The chemical composition of the steel of each embodiment is shown in Table 1, the carbon equivalent and welding crack sensitivity coefficient of the steel of each embodiment are shown in Table 2, the smelting process parameters of the steel of each embodiment are shown in Table 3, the slab heating process parameters of each embodiment are shown in Table 4, the rolling and cooling process parameters of the steel plate of each embodiment are shown in Table 5, the tempering heat treatment process parameters of the steel plate of each embodiment are shown in Table 6, the mechanical properties of the finished steel plate of each embodiment are shown in Table 7, the low-temperature fracture performance of the finished steel plate of each embodiment is shown in Table 8, and the roughness and grain size of the finished steel plate of each embodiment are shown in Table 9.
[0069] Table 1 Chemical composition of steel (wt%)
[0070] Example C Si Mn P S Ni Cr Nb Mo Ti B Als O N 1 0.151 0.35 1.26 0.011 0.0018 0.35 0.77 0.026 0.35 0.011 0.002 0.076 0.0003 0.0014 2 0.124 0.29 1.44 0.01 0.002 0.31 0.69 0.019 0.41 0.015 0.0011 0.051 0.0008 0.0005 3 0.129 0.17 1.41 0.009 0.0016 0.39 0.56 0.034 0.44 0.008 0.001 0.044 0.0007 0.0024 4 0.121 0.19 1.49 0.01 0.0015 0.41 0.81 0.031 0.26 0.011 0.0007 0.061 0.0004 0.0019 5 0.111 0.25 1.31 0.008 0.002 0.49 0.85 0.039 0.31 0.014 0.0009 0.074 0.0001 0.0022 6 0.141 0.34 1.21 0.012 0.0019 0.31 0.59 0.029 0.32 0.012 0.0016 0.061 0.0005 0.0008 7 0.159 0.21 1.12 0.01 0.002 0.36 0.61 0.027 0.29 0.007 0.0013 0.055 0.0004 0.0036 8 0.149 0.27 1.18 0.012 0.0014 0.47 0.55 0.015 0.42 0.009 0.0017 0.052 0.0008 0.0015 9 0.131 0.31 1.33 0.009 0.0016 0.32 0.64 0.022 0.31 0.009 0.0014 0.049 0.0003 0.0027 10 0.139 0.28 1.23 0.01 0.002 0.26 0.66 0.032 0.39 0.012 0.0012 0.069 0.0002 0.0032
[0071] Table 2 Carbon equivalent of steel and welding crack sensitivity coefficient
[0072] Example Ceq / % Pcm / % 1 0.61 0.30 2 0.60 0.28 3 0.59 0.27 4 0.61 0.27 5 0.59 0.26 6 0.55 0.28 7 0.55 0.28 8 0.57 0.29 9 0.56 0.27 10 0.57 0.28
[0073] Table 3 Steel smelting process parameters
[0074]
[0075]
[0076] Table 4 Continuous casting slab heating process parameters
[0077]
[0078] Table 5 Rolling and cooling process parameters of steel plates
[0079]
[0080] Table 6 Quenching and tempering heat treatment process parameters of steel plates
[0081]
[0082]
[0083] Table 7 Mechanical properties of finished steel plates
[0084]
[0085] Table 8 Low temperature fracture properties of finished steel plates
[0086]
[0087] Table 9 Roughness and grain size of finished steel plate
[0088]
[0089]
[0090] The metallographic structure of the finished steel plate in Example 2 is shown in Figure 1 (Magnified 500 times), grain size photo see Figure 2 (Magnified 500 times).
[0091] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An EH690 grade marine engineering steel, characterized in that: The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.10% to 0.16%; Si: 0.15% to 0.40%; Mn: 1.00% to 1.50%; P≤0.012%; S≤0.002%; Ni: 0.25% to 0.50%; Cr: 0.50% to 0.90%; Nb: 0.015% to 0.04%; Mo: 0.25% to 0.50%; Ti: 0.007%~0.015%; B: 0.0007%~0.002%; Als: 0.04%~0.08%; O≤0.001%; N≤0.004%; H≤0.002%; the balance is Fe and unavoidable impurities; Ceq≤0.64%, Pcm≤0.33%; wherein, Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5, Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B.
2. The method for manufacturing EH690 grade marine engineering steel according to claim 1, characterized in that: The process route includes smelting and slow cooling of ingots, controlled rolling, controlled cooling and off-line quenching and tempering heat treatment; the following processes are controlled: 1) Smelting and slow cooling of ingots; LF refining and RH refining are 20-40 minutes each, the superheat of molten steel in the tundish is 22-28℃, the gas content is controlled to be [N]≤40ppm, [O]≤10ppm, [H]≤2.0ppm; full protection casting, various inclusions in the steel meet the following requirements: Class A inclusions ≤1.0 level, Class B inclusions ≤1.0 level, Class C inclusions ≤1.0 level, Class D inclusions ≤1.0 level; light reduction is adopted in the continuous casting billet forming process, and the reduction amount is 6-8mm; after the continuous casting billet is off the line, it is stacked and slowly cooled, and the stacking temperature is ≥600℃, and the time is ≥48h; 2) Controlled rolling; The continuous casting billet is heated in four stages, including the first heating stage, the second heating stage, the third heating stage and the soaking stage; the upper and lower heating temperatures of each heating stage and the soaking stage are controlled separately; the total heating time of the continuous casting billet is 10-12min / mm; the starting rolling temperature is 950-1000℃, and the single pass reduction rate is ≥15% except the widening pass; the second stage starting rolling temperature is 720-760℃, the single pass reduction rate is ≥11%, and the final rolling temperature is 680-720℃; 3) Controlled cooling; After final rolling, the steel plate is directly cooled by DQ+ACC rapid cooling system, with an average cooling rate of ≥10℃ / s and a red-return temperature of 200~300℃; 4) Offline quenching and tempering heat treatment; Quenching: The steel plate is subjected to quenching heat treatment, the quenching heating temperature is 860-910°C, the heating rate is 1.3-2min / mm, the holding time is 20-40min, and the steel plate is quenched in water to room temperature after being taken out of the furnace; Tempering: The steel plate is tempered at a temperature of 580-630°C and a furnace time of 3-4.5 min / mm. After being taken out of the furnace, it is air-cooled to obtain a finished steel plate.
3. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: In the step 2), the lower heating temperature of the first heating section is 1000-1120°C, and the upper heating temperature of the first heating section is 1050-1180°C; the lower heating temperature of the second heating section is 1130-1180°C, and the upper heating temperature of the second heating section is 1180-1220°C; the lower heating temperature of the third heating section is 1150-1200°C, and the upper heating temperature of the third heating section is 1200-1250°C; the lower heating temperature of the soaking section is 1050-1150°C, and the upper heating temperature of the soaking section is 1150-1200°C.
4. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: In the step 2), after the continuous casting billet is taken out of the furnace, high-pressure water is used to remove phosphorus for 2 to 3 times.
5. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: In the step 2), the intermediate billet thickness is 2 to 2.5 times the thickness of the finished steel plate, and the intermediate billet is water-cooled at a cooling rate of ≥4°C / s.
6. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: The microstructure of the finished steel plate is tempered martensite + bainite, and the grain size is ≥ grade 7.
7. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: The yield strength of the finished steel plate is ≥690MPa, the tensile strength is 770~940MPa, the section elongation is ≥14%, the Z-direction section shrinkage is ≥65%, the -40℃ Charpy impact energy of the steel plate core is ≥100J, and the -10℃ low-temperature fracture CTOD characteristic value is ≥0.5mm.
8. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: The maximum thickness of the finished steel plate is 60mm.
9. The method for manufacturing EH690 grade marine engineering steel according to claim 2, characterized in that: The unevenness of the finished steel plate is ≤4mm / 2m.
Citation Information
Patent Citations
High-strength steel plate for 800MPa hydropower station pressure pipeline and production method thereof
CN103290339A
FQ70-level ultrahigh-strength extra-thickness steel plate for ocean engineering and manufacturing method thereof
CN103938110A
Large-thickness high-strength steel plate for F690 ocean engineering and manufacturing method of steel plate
CN104711488A
800 MPa-level high-strength-tenacity steel plate used for engineering machine in extremely cold environment and manufacturing method for 800 MPa-level high-strength-tenacity steel plate
CN105779899A
Easily-welded high-strength steel with excellent low-temperature toughness and 800 MPa-grade tensile strength and production method thereof