Corrosion-resistant functional textile yarn and preparation method thereof
By coating composite polyethylene fiber with modified polyurethane and drawing and blending it with polydopamine-modified polyimide fiber, a tightly cross-linked structure is formed, which solves the problem of insufficient corrosion resistance of yarn in special environments and significantly improves mechanical performance. Strength and corrosion resistance.
Patent Information
- Application Number
- CN202410983632.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing textile yarns have insufficient corrosion resistance in special environments. The uneven mechanical properties of polyimide fibers and polyethylene fibers lead to uneven stress distribution, weak interface bonding, and easy corrosion.
Composite polyethylene fiber is coated with modified polyurethane and drawn and blended with polydopamine-modified polyimide fiber. It is activated with sodium hydroxide/ethanol solution to promote the mutual adhesion of the fibers to form a tight cross-linked structure and strengthen the Mechanical strength and corrosion resistance of yarns.
It improves the overall performance and service life of the yarn, reduces the gaps and voids between fibers, enhances the interface bonding force, and significantly improves the corrosion resistance of the yarn.
Smart Images

Figure BDA0004956773500000041 
Figure BDA0004956773500000061 
Figure BDA0004956773500000202
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of yarn processing, and in particular to a corrosion-resistant functional textile yarn and a preparation method thereof. Background Art
[0002] Textile yarns play a vital role in various applications and are widely used in clothing, household items, industrial materials and other fields. With the rapid development of the textile industry and technological progress, functional textiles have become an important part of the textile market. The application scope of textiles is becoming more and more extensive, especially under some special environmental conditions, especially in specific industrial environments such as the chemical industry, marine engineering, aerospace and other fields. The performance requirements for textiles are increasing day by day. Among them, corrosion resistance is one of the important properties that textiles in these special fields must have.
[0003] In traditional textile technology, textile yarn products with corrosion resistance mostly adopt the method of coating the yarn surface with corrosion-resistant coating to improve their corrosion resistance. However, this method has the following disadvantages: first, the coating is easy to peel off or wear, resulting in a decrease in corrosion resistance; second, the use of coating will change the original properties of the yarn, such as softness and air permeability; third, the preparation process of the coating is complicated and costly. Therefore, it is necessary to find a more effective and economical method to prepare functional textile yarns with excellent corrosion resistance.
[0004] Polyimide fiber has good mechanical strength and corrosion resistance and is usually used to prepare corrosion-resistant yarn. However, the cost of polyimide is high, and other fibers are usually added to polyimide fiber for drawing and blending to prepare yarn. Although polyethylene fiber has high mechanical strength, the mechanical properties of polyimide fiber are higher than those of polyethylene fiber. As a result, when polyimide fiber is mixed with polyethylene fiber to prepare yarn, due to the imbalance of mechanical properties, the stress distribution between different fibers is uneven when the yarn is subjected to external force, affecting the overall performance of the yarn. In addition, there are differences in chemical structure and surface properties between polyimide fiber and polyethylene fiber, which will result in weak interfacial bonding between fibers when the two fibers are mixed to prepare yarn. There are a large number of gaps and voids between fibers, and corrosive media can easily enter the yarn and directly contact the fibers, causing corrosion to the yarn. The corrosion resistance of the yarn needs to be further improved. Summary of the invention
[0005] The object of the present invention is to provide a corrosion-resistant functional textile yarn and a preparation method thereof, so as to solve the technical problem in the prior art that the mechanical strength and corrosion resistance of polyamide fiber composite textile yarn need to be further improved.
[0006] The purpose of the present invention can be achieved by the following technical solution: A method for preparing a corrosion-resistant functional textile yarn comprises the following steps:
[0007] S1, adding modified polyurethane and isopropanol into a reactor and stirring, raising the temperature of the reactor to 60-80°C, and stirring at this temperature until the system is dissolved to obtain a modified polyurethane solution;
[0008] S2, immersing the composite polyethylene fiber in a modified polyurethane solution at a temperature of 60-80°C, keeping the temperature for 30-50 seconds, dispersing the composite polyethylene fiber in a promoting liquid at a temperature of 50-60°C, keeping the temperature for 20-30 minutes, and post-treating to obtain a modified composite polyethylene fiber;
[0009] The synthetic reaction principle of modified composite polyethylene is:
[0010] The modified polyurethane is dissolved to prepare a modified polyurethane solution, and the modified polyurethane is coated on the outside of the composite polyethylene fiber in an impregnated manner. A compact modified polyurethane coating layer is formed on the outside of the composite polyethylene fiber by promoting the formation of a modified polyurethane coating layer by a promoter, thereby preparing the modified composite polyethylene fiber.
[0011] S3, adding the modified polyimide fiber and the modified composite polyethylene fiber into a drawing frame for drawing to prepare a coarse yarn;
[0012] S4, transferring the coarse yarn to an activation solution at a temperature of 70-80°C, steaming at the temperature for 30-50 minutes, and post-treating to obtain textile yarn.
[0013] Furthermore, in step S1, the amount ratio of the modified polyurethane to isopropanol is 1g:5mL; in step S2, the promoting liquid is composed of isopropanol and 1mol / L hydrochloric acid in a volume ratio of 3:2, and the post-treatment includes: after the heat preservation and dispersion are completed, the filter cake is filtered, washed with purified water for 3 times and then dried, and the filter cake is transferred to a drying oven at a temperature of 65-75°C, and dried to constant weight to obtain modified composite polyethylene; in step S3, the weight ratio of the modified polyimide fiber to the modified composite polyethylene fiber is 2:3; in step S4, the activation solution is composed of 10wt% sodium hydroxide solution and ethanol in a volume ratio of 2:3, and the post-treatment includes: after the reaction is completed, the coarse yarn is taken out from the activation solution, washed with purified water to neutrality and then drained, and then transferred to a drying oven at a temperature of 70-80°C and dried to constant weight to obtain textile yarn.
[0014] Further, the modified polyurethane is obtained by processing through the following steps:
[0015] A1. Add polytetrahydrofuran, 1H,1H,9H,9H-perfluoro-1,9-nonanediol and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 55-60° C., add isophorone diisocyanate solution into the reactor, keep the temperature for 90-120 min, add a chain extender into the reactor, keep the temperature for 2-3 h, add 3-aminopropyltriethoxysilane into the reactor, keep the temperature for 60-80 min, and perform post-treatment to obtain polyurethane.
[0016] The synthetic reaction formula of polyurethane is:
[0017]
[0018] Where:
[0019] The synthetic reaction principle of polyurethane is:
[0020] The isocyanate group on isophorone diisocyanate reacts with the hydroxyl groups on polytetrahydrofuran and 1H,1H,9H,9H-perfluoro-1,9-nonanediol to form a polyurethane prepolymer. The isocyanate group on the polyurethane prepolymer further condenses with the amino group on the chain extender, and 3-aminopropyltriethoxysilane is used as a capping agent to prepare a polyurethane having a triethoxysilane-capped polytetrahydrofuran chain segment and a perfluoroalkane chain segment copolymerized with a hydrogen-containing silane as a chain extender.
[0021] A2. Add polyurethane, glycidyl methacrylate, toluene and catalyst into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 70-80°C and keep the reaction temperature for 4-6 hours. Post-treat to obtain modified polyurethane.
[0022] The synthetic reaction principle of modified polyurethane is:
[0023] Under the action of a catalyst, the olefin double bond on glycidyl methacrylate reacts with the active hydrogen (such as silicon hydrogen) on the polyurethane molecule to introduce an alkylene oxide bond into the polyurethane molecule to prepare a modified polyurethane.
[0024] Further, in step A1, the molecular weight of the polytetrahydrofuran is 650±25, the polytetrahydrofuran, 1H,1H,9H,9H-perfluoro-1,9-nonanediol 412, tetrahydrofuran, isophorone diisocyanate solution 222.23, chain extender and 3-aminopropyltriethoxysilane are used in a ratio of 10g:6g:50mL:8g:1g:4g, and the isophorone diisocyanate solution is composed of isophorone diisocyanate and tetrahydrofuran in a ratio of 2g:3mL. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is reduced to room temperature, and the reaction solution is transferred to The method comprises the following steps: placing a dialysis bag with a molecular weight cutoff of 1000 in a tetrahydrofuran solution, dialyzing for 2 days, replacing the tetrahydrofuran solution every 6 hours, and then transferring the solution in the dialysis bag to a rotary evaporator, setting the water bath temperature to 50-60° C., and removing the solvent under reduced pressure to obtain a polyurethane; in step A2, the polyurethane, glycidyl methacrylate, toluene and catalyst are used in a ratio of 10 g:1-2 g:50 mL:0.1 g, the catalyst is chloroplatinic acid, and the post-treatment comprises: after the reaction is completed, raising the temperature of the reactor to 90-100° C., and removing the solvent under reduced pressure to obtain a modified polyurethane.
[0025] Furthermore, the preparation method of the chain extender is: 3-aminopropyltriethoxysilane, dimethoxysilane, triethoxysilane, and anhydrous ethanol are added to a reactor and stirred, the temperature of the reactor is increased to 50-60°C, 1 mol / L ammonia water is added to the reactor, the reaction is kept warm for 4-6 hours, and the chain extender is obtained by post-treatment.
[0026] The synthetic reaction formula of the chain extender is:
[0027]
[0028] The synthetic reaction principle of the chain extender is:
[0029] In an alkaline environment, the siloxane bonds on 3-aminopropyltriethoxysilane, dimethoxysilane and triethoxysilane are hydrolyzed and then self-assembled to prepare a polysiloxane network cross-linked chain extender with amino group and silicon-hydrogen bond modification.
[0030] Furthermore, the molar ratio of the 3-aminopropyltriethoxysilane, dimethoxysilane and triethoxysilane is 2:7:3, the dosage ratio of the 3-aminopropyltriethoxysilane, anhydrous ethanol and 1 mol / L ammonia water is 1 g:15 mL:5 mL, and the post-treatment includes: after the reaction is completed, the reactor is kept at 50-60°C, and the low-boiling point solvent is evaporated under reduced pressure, the temperature of the reactor is increased to 70-80°C, and distilled under reduced pressure until no liquid is distilled out, and the reactor is cooled to room temperature using nitrogen purge to obtain a chain extender.
[0031] Furthermore, the composite polyethylene fiber is obtained by processing the following steps:
[0032] B1. Add polyethylene powder, reinforcing modifier and white oil into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 70-80°C, keep warm and stir for 8-12 hours, add initiator and additives into the reactor to obtain a mixed solution.
[0033] B2, adding the mixed solution into a twin-screw extruder, after being extruded by the twin-screw extruder, spraying it from a spinneret into a low-temperature curing liquid, and post-processing to obtain a composite polyethylene fiber precursor;
[0034] B3. Thermally stretching the composite polyethylene fiber precursor to prepare composite polyethylene fibers with a fineness of 20-25 tex.
[0035] The synthetic reaction principle of composite polyethylene fiber is:
[0036] White oil has good compatibility with polyethylene. When white oil comes into contact with polyethylene, its molecules penetrate between the molecular chains of polyethylene, thereby causing the volume expansion of polyethylene to a certain extent and improving the reaction activity of polyethylene. 5-hexenyltrimethoxysilane is used as an active agent to promote the uniform distribution of the system. Under the action of an initiator, the unsaturated double bonds on 5-hexenyltrimethoxysilane react with polyethylene through addition reaction, while the multi-active oxygen-containing groups on the carboxylated multi-walled carbon nanotubes react with the siloxane bonds on 5-hexenyltrimethoxysilane through condensation under high temperature. 5-hexenyltrimethoxysilane is used as a cross-linking agent to improve the cross-linking degree between multi-walled carbon nanotubes and polyethylene, thereby preparing composite polyethylene. After being ejected from a spinneret, the composite polyethylene is stretched at high temperature to prepare a composite polyethylene fiber reinforced with a high cross-linking degree by multi-walled carbon nanotubes.
[0037] Further, in step B1, the molecular weight of the polyethylene powder is 1.5 million to 2.5 million, the amount ratio of the polyethylene powder, the reinforcing modifier, the white oil, the initiator and the additive is 10-15g:3-5g:40-50mL:0.1-0.2g:0.1g, and the reinforcing modifier is composed of carboxylated multi-walled carbon nanotubes and 5-hexenyltrimethoxysilane in a weight ratio of 3:1; in step B2, the temperature of the 8 temperature intervals of the twin-screw extruder from the feed end to the discharge end is 90°C, 150°C, 230°C, 230°C, 230°C, 230°C, 200°C, and 180°C, and the pore size of the spinneret on the spinneret is 0.9-1. 1mm, the aspect ratio is 8:1, the temperature of the low-temperature curing liquid is 5-10°C, the curing liquid is composed of dichloromethane and nonylphenol polyoxyethylene ether in a dosage ratio of 10mL:0.2g, and the post-treatment includes: after curing with the curing liquid, washing the fiber 3 times with dichloromethane, transferring it to a drying oven at a temperature of 50-60°C, and drying it to constant weight to obtain a composite polyethylene fiber precursor; in step B3, the hot stretching includes primary stretching, secondary stretching and tertiary stretching, the primary stretching temperature is 80-85°C, the stretching ratio is 15 times, the secondary stretching temperature is 100°C, the stretching ratio is 2 times, and the tertiary stretching temperature is 115°C, and the stretching ratio is 1.5 times.
[0038] Furthermore, the modified polyimide fiber is obtained by processing the following steps:
[0039] C1. Add the polyimide fiber and the pretreatment solution into a reactor and stir, raise the temperature of the reactor to 70-80° C., keep the temperature for 20-30 minutes, and perform post-treatment to obtain the pre-treated polyimide fiber;
[0040] C2. Add the pretreated polyimide fiber and Tris-HCl aqueous solution into the reactor and stir. The temperature of the reactor is raised to 55-65° C., and dopamine hydrochloride solution is added into the reactor. The mixture is stirred for 12-14 hours at the temperature maintained. The modified polyimide fiber is obtained by post-treatment.
[0041] The synthetic reaction principle of modified polyimide fiber is:
[0042] The modified polyimide fiber is prepared by pre-treating the polyimide fiber to improve the surface activity of the polyimide fiber and then depositing a polydopamine layer on the outside of the fiber.
[0043] Further, in step C1, the fineness of the polyimide fiber is 20-30tex, the amount ratio of the polyimide fiber to the pretreatment solution is 1g:10mL, the pretreatment solution is composed of 2mol / L hydrochloric acid and 10wt% hydrogen peroxide in a volume ratio of 3:1, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with purified water until neutral and then dried, the filter cake is transferred to a drying oven at a temperature of 70-80°C, and vacuum dried to constant weight to obtain the pre-treated polyimide fiber; in step C2, the The pH value of the Tris-HCl aqueous solution is 8.5. The usage ratio of the pre-treated polyimide fiber, the Tris-HCl aqueous solution and the dopamine hydrochloride solution is 10g:500mL:5-10g. The dopamine hydrochloride solution is composed of dopamine hydrochloride and purified water in a weight ratio of 1g:10mL. The post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filter cake is filtered, the filter cake is washed with purified water until it is neutral and then dried, the filter cake is transferred to a drying oven with a temperature of 60-70°C, and dried to constant weight to obtain the modified polyimide fiber.
[0044] A corrosion-resistant functional textile yarn is prepared by a corrosion-resistant functional textile yarn preparation method.
[0045] The present invention has the following beneficial effects:
[0046] 1. The corrosion-resistant functional textile yarn of the present invention is prepared by reinforcing high-molecular polyethylene with multi-walled carbon nanotubes to obtain highly cross-linked high-molecular composite polyethylene fibers, and then coating and modifying the high-molecular composite polyethylene fibers with modified polyurethane to obtain modified composite polyethylene fibers, which are then blended with polyimide fibers coated with polydopamine and activated with sodium hydroxide / ethanol solution to promote mutual adhesion between the fibers to obtain textile yarns; the strength of the polyethylene fibers is increased and the difference in mechanical properties between the polyethylene fibers and the polyimide fibers is reduced, so that when the yarn is subjected to external forces, the stress received by the yarn is evenly distributed, thereby improving the overall performance and service life of the yarn; and the surface of the composite polyethylene fibers and the polyimide fibers is modified to reduce the difference in surface properties between the polyethylene fibers and the polyimide fibers, thereby enhancing the interfacial bonding force of the yarns, reducing the separation or damage between the fibers caused by acid or alkali corrosion, and improving the corrosion resistance of the textile fibers.
[0047] 2. The corrosion-resistant functional textile yarn of the present invention is prepared by using high molecular weight polyethylene as a raw material, and reinforcing polyethylene with polyhydroxy carbon nanotubes and 5-hexenyltrimethoxysilane as reinforcing materials to prepare composite polyethylene. After melt spinning, the composite polyethylene is stretched at a ratio to increase the orientation of the fiber, so that the fiber molecular chain is arranged more closely, the defects and gaps inside the fiber are reduced, and the mechanical properties of the fiber are increased. A layer of polyurethane is tightly coated on the outside of the composite polyethylene fiber to further improve the corrosion resistance of the composite polyethylene fiber. In addition, under the action of the activation liquid, The epoxy groups modified on the polyurethane layer undergo condensation cross-linking with the imine or other oxygen-containing groups on the polydopamine layer modified on the modified polyimide fiber to form cross-linking bonds within the fibers, thereby enhancing the connection and stability between the fibers, increasing the proportion of macromolecular chain breaks, and improving the overall mechanical strength of the yarn. Stable chemical bonds are formed between the fibers that make up the yarn. The chemical bonds fill or seal the gaps and voids between the fibers, reducing the area of direct contact between the corrosive medium and the fiber, resisting the penetration and erosion of external corrosive media (such as acid, alkali, water, etc.), thereby further improving the corrosion resistance of the yarn. DETAILED DESCRIPTION
[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] This embodiment provides a method for preparing a corrosion-resistant functional textile yarn, comprising the following steps:
[0051] S1. Preparation of composite polyethylene fibers
[0052] The carboxylated multi-walled carbon nanotubes and 5-hexenyltrimethoxysilane are uniformly mixed in a weight ratio of 3:1 to obtain a reinforcing modifier;
[0053] Weigh: 100 g of polyethylene powder with a molecular weight of 1.5 million to 2.5 million, 30 g of a reinforcing modifier and 400 mL of white oil, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 70° C., keep warm and stir for 8 hours, add 1 g of benzoyl peroxide and 1 g of an antioxidant 1010 into the reactor to obtain a mixed solution;
[0054] Mix dichloromethane and nonylphenol polyoxyethylene ether in a ratio of 10 mL:0.2 g to obtain a solidified liquid;
[0055] The mixed solution is added into a twin-screw extruder, and the temperatures of the eight temperature zones of the twin-screw extruder from the feed end to the discharge end are 90°C, 150°C, 230°C, 230°C, 230°C, 200°C, and 180°C, respectively. After being extruded by the twin-screw extruder, the mixed solution is sprayed from a spinneret into a curing liquid at a temperature of 5°C. After being cured by the curing liquid, the fiber is washed three times with dichloromethane, and the fiber is transferred into a drying oven at a temperature of 50°C, and dried to a constant weight to obtain a composite polyethylene fiber precursor, wherein the diameter of the spinneret hole on the spinneret is 0.9 mm, and the aspect ratio is 8:1;
[0056] The composite polyethylene fiber precursor is placed in a stretching machine at a temperature of 80°C, the stretching ratio is set to 15 times, and the first-stage stretching is performed. Then the temperature of the stretching machine is increased to 100°C, the stretching ratio is set to 2 times, and the second-stage stretching is performed. The temperature of the stretching machine is increased to 115°C, the stretching ratio is set to 1.5 times, and the third-stage stretching is performed to prepare a composite polyethylene fiber with a fineness of 20-25tex.
[0057] S2. Preparation of modified polyurethane
[0058] Weigh: 44.3 g of 3-aminopropyltriethoxysilane, 74.3 g of dimethoxysilane, 49.3 g of triethoxysilane, and 664.5 mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 50° C., add 221.5 mL of 1 mol / L ammonia water into the reactor, and keep the temperature for 4 hours. After the reaction is completed, keep the reactor at 50° C., remove the low boiling point solvent under reduced pressure, raise the temperature of the reactor to 70° C., distill under reduced pressure until no liquid is distilled out, and purge the reactor with nitrogen to cool it down to room temperature to obtain a chain extender;
[0059] Isophorone diisocyanate and tetrahydrofuran were mixed uniformly in a ratio of 2 g:3 mL to obtain an isophorone diisocyanate solution;
[0060] Weigh: 100 g of polytetrahydrofuran with a molecular weight of 650±25, 60 g of 1H,1H,9H,9H-perfluoro-1,9-nonanediol and 500 mL of tetrahydrofuran, add them to a nitrogen-protected reactor and stir, raise the temperature of the reactor to 55°C, add 80 g of isophorone diisocyanate solution to the reactor, keep warm for 90 minutes, add 10 g of chain extender to the reactor, keep warm for 2 hours, add 40 g of 3-aminopropyltriethoxysilane to the reactor, keep warm for 60 minutes, after the reaction is completed, lower the temperature of the reactor to room temperature, transfer the reaction solution to a dialysis bag with a molecular weight cutoff of 1000, place the dialysis bag in a tetrahydrofuran solution, dialyze for 2 days, replace the tetrahydrofuran solution every 6 hours, then transfer the solution in the dialysis bag to a rotary evaporator, set the water bath temperature to 50°C, and evaporate the solvent under reduced pressure to obtain a polyurethane;
[0061] Weigh: 100 g of polyurethane, 10 g of glycidyl methacrylate, 500 mL of toluene and 1 g of chloroplatinic acid, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 70°C, and keep the reaction for 4 hours. After the reaction is completed, raise the temperature of the reactor to 90°C, and evaporate the solvent under reduced pressure to obtain modified polyurethane.
[0062] S3. Preparation of modified composite polyethylene fiber
[0063] Add modified polyurethane and isopropanol in a ratio of 1 g:5 mL into a reactor and stir, raise the temperature of the reactor to 60° C., and keep stirring until the system is dissolved to obtain a modified polyurethane solution;
[0064] Isopropyl alcohol and 1 mol / L hydrochloric acid were mixed evenly in a volume ratio of 3:2 to obtain a promoting solution;
[0065] The composite polyethylene fiber is immersed in a modified polyurethane solution at a temperature of 60°C and kept warm for 30 seconds. The composite polyethylene fiber is dispersed in a promoting liquid at a temperature of 50°C and kept warm for 20 minutes. After the heat preservation and dispersion are completed, it is filtered and the filter cake is washed with purified water three times and then dried. The filter cake is transferred to a drying oven at a temperature of 65°C and dried to constant weight to obtain a modified composite polyethylene.
[0066] S4. Preparation of modified polyimide fiber
[0067] 2 mol / L hydrochloric acid and 10 wt % hydrogen peroxide were mixed uniformly in a volume ratio of 3:1 to obtain a pretreatment solution for later use;
[0068] The polyimide fiber and the pretreatment solution are added to the reactor in a dosage ratio of 1g:10mL and stirred, the temperature of the reactor is raised to 70°C, and the temperature is kept for 20 minutes. After the reaction is completed, the temperature of the reactor is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 70°C and vacuum dried to constant weight to obtain the pretreated polyimide fiber, wherein the fineness of the polyimide fiber is 20-30tex;
[0069] Dopamine hydrochloride and purified water were mixed uniformly at a weight ratio of 1 g:10 mL to obtain a dopamine hydrochloride solution;
[0070] Weigh: 100 g of pretreated polyimide fiber and 5000 mL of Tris-HCl aqueous solution with pH = 8.5 are added to the reactor and stirred. The temperature of the reactor is raised to 55°C, 50 g of dopamine hydrochloride solution is added to the reactor, and the mixture is kept warm and stirred for 12 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 60°C and dried to constant weight to obtain modified polyimide fiber.
[0071] S5. Preparation of textile yarn
[0072] The modified polyimide fiber and the modified composite polyethylene fiber were added into a drawing frame at a weight ratio of 2:3 for drawing to prepare a coarse yarn with a twist of 350 twists / m;
[0073] 10 wt % sodium hydroxide solution and ethanol were mixed uniformly in a volume ratio of 2:3 to obtain an activation solution;
[0074] The coarse yarn is transferred to an activation solution at a temperature of 70°C and kept warm for 30 minutes. After the reaction is completed, the coarse yarn is taken out from the activation solution, washed with purified water until it is neutral, drained, and then transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain textile yarn.
[0075] Example 2
[0076] This embodiment provides a method for preparing a corrosion-resistant functional textile yarn, comprising the following steps:
[0077] S1. Preparation of composite polyethylene fibers
[0078] The carboxylated multi-walled carbon nanotubes and 5-hexenyltrimethoxysilane are uniformly mixed in a weight ratio of 3:1 to obtain a reinforcing modifier;
[0079] Weigh: 125 g of polyethylene powder with a molecular weight of 1.5 million to 2.5 million, 40 g of a reinforcing modifier and 450 mL of white oil, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 75° C., keep warm and stir for 10 hours, add 1.5 g of benzoyl peroxide and 1 g of an antioxidant 1010 into the reactor to obtain a mixed solution;
[0080] Mix dichloromethane and nonylphenol polyoxyethylene ether in a ratio of 10 mL:0.2 g to obtain a solidified liquid;
[0081] The mixed solution is added into a twin-screw extruder, wherein the temperatures of the eight temperature zones from the feed end to the discharge end of the twin-screw extruder are 90°C, 150°C, 230°C, 230°C, 230°C, 200°C, and 180°C, respectively; after being extruded by the twin-screw extruder, the mixed solution is sprayed out from a spinneret into a curing liquid at a temperature of 5-10°C; after being cured by the curing liquid, the fiber is washed three times with dichloromethane, and the fiber is transferred into a drying oven at a temperature of 55°C, and dried to a constant weight to obtain a composite polyethylene fiber precursor, wherein the diameter of the spinneret hole on the spinneret is 1.0 mm, and the aspect ratio is 8:1;
[0082] The composite polyethylene fiber precursor is placed in a stretching machine at a temperature of 83°C, the stretching ratio is set to 15 times, and the first-stage stretching is performed. Then the temperature of the stretching machine is increased to 100°C, the stretching ratio is set to 2 times, and the second-stage stretching is performed. The temperature of the stretching machine is increased to 115°C, the stretching ratio is set to 1.5 times, and the third-stage stretching is performed to prepare a composite polyethylene fiber with a fineness of 20-25tex.
[0083] S2. Preparation of modified polyurethane
[0084] Weigh: 44.3 g of 3-aminopropyltriethoxysilane, 74.3 g of dimethoxysilane, 49.3 g of triethoxysilane, and 664.5 mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 55° C., add 221.5 mL of 1 mol / L ammonia water into the reactor, and keep the temperature for 5 hours. After the reaction is completed, keep the reactor at 55° C., evaporate the low-boiling point solvent under reduced pressure, raise the temperature of the reactor to 75° C., distill under reduced pressure until no liquid is distilled out, and purge the reactor with nitrogen to cool it down to room temperature to obtain a chain extender;
[0085] Isophorone diisocyanate and tetrahydrofuran were mixed uniformly in a ratio of 2 g:3 mL to obtain an isophorone diisocyanate solution;
[0086] Weigh: 100 g of polytetrahydrofuran with a molecular weight of 650±25, 60 g of 1H,1H,9H,9H-perfluoro-1,9-nonanediol and 500 mL of tetrahydrofuran, add them to a nitrogen-protected reactor and stir, raise the temperature of the reactor to 57°C, add 80 g of isophorone diisocyanate solution to the reactor, keep warm for 105 min, add 10 g of chain extender to the reactor, keep warm for 2.5 h, add 40 g of 3-aminopropyltriethoxysilane to the reactor, keep warm for 70 min, after the reaction is completed, lower the temperature of the reactor to room temperature, transfer the reaction solution to a dialysis bag with a molecular weight cutoff of 1000, place the dialysis bag in a tetrahydrofuran solution, dialyze for 2 days, replace the tetrahydrofuran solution every 6 h, then transfer the solution in the dialysis bag to a rotary evaporator, set the water bath temperature to 55°C, and evaporate the solvent under reduced pressure to obtain a polyurethane;
[0087] Weigh: 100 g of polyurethane, 15 g of glycidyl methacrylate, 500 mL of toluene and 1 g of chloroplatinic acid, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 75°C, and keep the reaction for 5 hours. After the reaction is completed, raise the temperature of the reactor to 95°C, and evaporate the solvent under reduced pressure to obtain modified polyurethane.
[0088] S3. Preparation of modified composite polyethylene fiber
[0089] Add modified polyurethane and isopropanol in a ratio of 1 g:5 mL into a reactor and stir, raise the temperature of the reactor to 70° C., and keep stirring until the system is dissolved to obtain a modified polyurethane solution;
[0090] Isopropyl alcohol and 1 mol / L hydrochloric acid were mixed evenly in a volume ratio of 3:2 to obtain a promoting solution;
[0091] The composite polyethylene fiber is immersed in a modified polyurethane solution at a temperature of 70°C and kept warm for 40 seconds. The composite polyethylene fiber is dispersed in a promoting liquid at a temperature of 55°C and kept warm for 25 minutes. After the insulation and dispersion are completed, it is filtered and the filter cake is washed three times with purified water and then dried. The filter cake is transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain a modified composite polyethylene.
[0092] S4. Preparation of modified polyimide fiber
[0093] 2 mol / L hydrochloric acid and 10 wt % hydrogen peroxide were mixed uniformly in a volume ratio of 3:1 to obtain a pretreatment solution for later use;
[0094] The polyimide fiber and the pretreatment solution were added to the reactor in a dosage ratio of 1g:10mL and stirred, the temperature of the reactor was raised to 75°C, and the temperature was kept for 25 minutes. After the reaction was completed, the temperature of the reactor was lowered to room temperature, and the filter cake was washed with purified water until it was neutral and then dried. The filter cake was transferred to a drying oven at a temperature of 75°C and vacuum dried to constant weight to obtain the pretreated polyimide fiber, wherein the fineness of the polyimide fiber was 20-30tex;
[0095] Dopamine hydrochloride and purified water were mixed uniformly at a weight ratio of 1 g:10 mL to obtain a dopamine hydrochloride solution;
[0096] Weigh: 100 g of pretreated polyimide fiber and 5000 mL of Tris-HCl aqueous solution with pH = 8.5 are added to the reactor and stirred. The temperature of the reactor is raised to 60°C, 75 g of dopamine hydrochloride solution is added to the reactor, and the mixture is kept warm and stirred for 13 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 65°C and dried to constant weight to obtain modified polyimide fiber.
[0097] S5. Preparation of textile yarn
[0098] The modified polyimide fiber and the modified composite polyethylene fiber were added into a drawing frame at a weight ratio of 2:3 for drawing to prepare a coarse yarn with a twist of 380 twists / m;
[0099] 10 wt % sodium hydroxide solution and ethanol were mixed uniformly in a volume ratio of 2:3 to obtain an activation solution;
[0100] The coarse yarn is transferred to an activation solution at a temperature of 75°C and kept warm for 40 minutes. After the reaction is completed, the coarse yarn is taken out from the activation solution, washed with purified water until it is neutral, drained, and then transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain textile yarn.
[0101] Example 3
[0102] This embodiment provides a method for preparing a corrosion-resistant functional textile yarn, comprising the following steps:
[0103] S1. Preparation of composite polyethylene fibers
[0104] The carboxylated multi-walled carbon nanotubes and 5-hexenyltrimethoxysilane are uniformly mixed in a weight ratio of 3:1 to obtain a reinforcing modifier;
[0105] Weigh: 150g of polyethylene powder with a molecular weight of 1.5 million to 2.5 million, 50g of a reinforcing modifier and 500mL of white oil, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 80°C, keep warm and stir for 12h, add 2g of benzoyl peroxide and 1g of an antioxidant 1010 into the reactor to obtain a mixed solution;
[0106] Mix dichloromethane and nonylphenol polyoxyethylene ether in a ratio of 10 mL:0.2 g to obtain a solidified liquid;
[0107] The mixed solution is added into a twin-screw extruder, and the temperatures of the eight temperature zones of the twin-screw extruder from the feed end to the discharge end are 90°C, 150°C, 230°C, 230°C, 230°C, 200°C, and 180°C, respectively. After being extruded by the twin-screw extruder, the mixed solution is sprayed from a spinneret into a curing liquid at a temperature of 10°C. After being cured by the curing liquid, the fiber is washed three times with dichloromethane, and the fiber is transferred into a drying oven at a temperature of 60°C, and dried to a constant weight to obtain a composite polyethylene fiber precursor, wherein the diameter of the spinneret hole on the spinneret is 1.1 mm, and the aspect ratio is 8:1;
[0108] The composite polyethylene fiber precursor is placed in a stretching machine at a temperature of 85°C, the stretching ratio is set to 15 times, and the first-stage stretching is performed. Then the temperature of the stretching machine is increased to 100°C, the stretching ratio is set to 2 times, and the second-stage stretching is performed. The temperature of the stretching machine is increased to 115°C, the stretching ratio is set to 1.5 times, and the third-stage stretching is performed to prepare a composite polyethylene fiber with a fineness of 20-25tex.
[0109] S2. Preparation of modified polyurethane
[0110] Weigh: 44.3 g of 3-aminopropyltriethoxysilane, 74.3 g of dimethoxysilane, 49.3 g of triethoxysilane, and 664.5 mL of anhydrous ethanol, add them into a reactor and stir, raise the temperature of the reactor to 60°C, add 221.5 mL of 1 mol / L ammonia water into the reactor, and keep the temperature for 4-6 hours. After the reaction is completed, keep the reactor at 60°C, remove the low boiling point solvent under reduced pressure, raise the temperature of the reactor to 80°C, distill under reduced pressure until no liquid is distilled out, and purge the reactor with nitrogen to cool it down to room temperature to obtain a chain extender;
[0111] Isophorone diisocyanate and tetrahydrofuran were mixed uniformly in a ratio of 2 g:3 mL to obtain an isophorone diisocyanate solution;
[0112] Weigh: 100 g of polytetrahydrofuran with a molecular weight of 650±25, 60 g of 1H,1H,9H,9H-perfluoro-1,9-nonanediol and 500 mL of tetrahydrofuran, add them to a nitrogen-protected reactor and stir, raise the temperature of the reactor to 60°C, add 80 g of isophorone diisocyanate solution to the reactor, keep warm for 120 min, add 10 g of chain extender to the reactor, keep warm for 3 h, add 40 g of 3-aminopropyltriethoxysilane to the reactor, keep warm for 80 min, after the reaction is completed, lower the temperature of the reactor to room temperature, transfer the reaction solution to a dialysis bag with a molecular weight cutoff of 1000, place the dialysis bag in a tetrahydrofuran solution, dialyze for 2 days, replace the tetrahydrofuran solution every 6 h, then transfer the solution in the dialysis bag to a rotary evaporator, set the water bath temperature to 60°C, and evaporate the solvent under reduced pressure to obtain a polyurethane;
[0113] Weigh: 100 g of polyurethane, 20 g of glycidyl methacrylate, 500 mL of toluene and 1 g of chloroplatinic acid, add into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 80° C., and keep the reaction for 6 hours. After the reaction is completed, raise the temperature of the reactor to 100° C., and evaporate the solvent under reduced pressure to obtain a modified polyurethane.
[0114] S3. Preparation of modified composite polyethylene fiber
[0115] Add modified polyurethane and isopropanol in a ratio of 1 g:5 mL into a reactor and stir, raise the temperature of the reactor to 80° C., and keep stirring until the system is dissolved to obtain a modified polyurethane solution;
[0116] Isopropyl alcohol and 1 mol / L hydrochloric acid were mixed evenly in a volume ratio of 3:2 to obtain a promoting solution;
[0117] The composite polyethylene fiber is immersed in a modified polyurethane solution at a temperature of 80°C and kept warm for 50 seconds. The composite polyethylene fiber is dispersed in a promoting liquid at a temperature of 60°C and kept warm for 30 minutes. After the heat preservation and dispersion are completed, it is filtered and the filter cake is washed three times with purified water and then dried. The filter cake is transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain a modified composite polyethylene.
[0118] S4. Preparation of modified polyimide fiber
[0119] 2 mol / L hydrochloric acid and 10 wt % hydrogen peroxide were mixed uniformly in a volume ratio of 3:1 to obtain a pretreatment solution for later use;
[0120] The polyimide fiber and the pretreatment solution are added to the reactor in a dosage ratio of 1g:10mL and stirred, the temperature of the reactor is raised to 80°C, and the temperature is kept for 30 minutes. After the reaction is completed, the temperature of the reactor is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 80°C and vacuum dried to constant weight to obtain the pretreated polyimide fiber, wherein the fineness of the polyimide fiber is 20-30tex;
[0121] Dopamine hydrochloride and purified water were mixed uniformly at a weight ratio of 1 g:10 mL to obtain a dopamine hydrochloride solution;
[0122] Weigh: 100 g of pretreated polyimide fiber and 5000 mL of Tris-HCl aqueous solution with pH = 8.5 are added to the reactor and stirred. The temperature of the reactor is raised to 65°C, 100 g of dopamine hydrochloride solution is added to the reactor, and the mixture is kept warm and stirred for 14 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain modified polyimide fiber.
[0123] S5. Preparation of textile yarn
[0124] The modified polyimide fiber and the modified composite polyethylene fiber are added into a drawing frame at a weight ratio of 2:3 for drawing to prepare a coarse yarn with a twist of 400 twists / m;
[0125] 10 wt % sodium hydroxide solution and ethanol were mixed uniformly in a volume ratio of 2:3 to obtain an activation solution;
[0126] The coarse yarn is transferred to an activation solution at a temperature of 80°C and kept warm for 50 minutes. After the reaction is completed, the coarse yarn is taken out from the activation solution, washed with purified water until it is neutral, drained, and then transferred to a drying oven at a temperature of 80°C and dried to constant weight to obtain textile yarn.
[0127] Comparative Example 1
[0128] The difference between this comparative example and Example 3 is that, in step S1, 5-hexenyltrimethoxysilane is not added as the reinforcing modifier.
[0129] Comparative Example 2
[0130] The difference between this comparative example and Example 3 is that, in step S3, the modified polyurethane in step S3 is replaced by the polyurethane in step S2.
[0131] Comparative Example 3
[0132] The difference between this comparative example and Example 3 is that steps S2-S3 are eliminated, and the modified composite polyethylene fiber in step S5 is replaced by the composite polyethylene fiber prepared in step S1.
[0133] Comparative Example 4
[0134] The difference between this comparative example and Example 3 is that step S4 is eliminated, and the modified polyimide fiber in step S5 is replaced by the polyimide fiber in step S4.
[0135] Performance Test:
[0136] The mechanical strength and corrosion resistance of the textile yarns prepared in Examples 1-3 and Comparative Examples 1-4 were tested, wherein the mechanical strength was determined by referring to the standard GB / T 3916-2013 "Determination of the breaking strength and breaking elongation of a single yarn of textile packaged yarn (CRE method)" to determine the breaking strength and breaking elongation of the sample. The corrosion resistance test was performed by placing the sample in a 2wt% sodium hydroxide solution at a temperature of 80°C for 30 minutes, a 10wt% nitric acid solution at a temperature of 80°C for 6 hours, and a 30wt% sulfuric acid solution at a temperature of 80°C for 20 hours, respectively, and measuring the breaking strength and breaking elongation of the sample after corrosion immersion in sodium hydroxide, nitric acid, and sulfuric acid, and according to the formula Calculate the fracture strength retention rate and fracture elongation retention rate of the sample, where X 腐蚀后 is the fracture strength or elongation of the sample after corrosion, X 腐蚀前 It is the fracture strength or elongation of the sample before corrosion. The specific test results are shown in Table 1-4.
[0137] Table 1-Mechanical strength of the samples
[0138]
[0139]
[0140] Table 2 - Sodium hydroxide corrosion resistance of samples
[0141]
[0142] Table 3- Nitric Acid Corrosion Performance of Samples
[0143]
[0144]
[0145] Table 4 - Sulfuric acid corrosion resistance performance of samples
[0146]
[0147] Data Analysis:
[0148] A comparative analysis of the data in Tables 1-4 shows that the breaking strength of the textile yarn prepared by the present invention reaches 3.91 cN / tex, and the elongation at break reaches 10.9%. After being immersed and corroded by 2wt% sodium hydroxide solution, 10wt% nitric acid solution and 30wt% sulfuric acid solution, the breaking strength and elongation at break of the yarn have good retention rates, and various performance parameters are better than those of the comparative example, indicating that the present invention strengthens and modifies polyethylene, and then coats a polyurethane layer on the outside thereof to prepare a modified composite polyethylene fiber, which is then composited with a polyimide fiber modified with polydopamine to prepare a yarn with high cross-linking between fibers, which not only effectively improves the breaking strength and elongation at break of the yarn, but also improves the acid and alkali corrosion resistance of the fiber.
[0149] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing corrosion-resistant functional textile yarn, It is characterized in that The following steps are involved: S1, adding modified polyurethane and isopropanol into a reactor and stirring, raising the temperature of the reactor to 60-80°C, and stirring at this temperature until the system is dissolved to obtain a modified polyurethane solution; S2, immersing the composite polyethylene fiber in a modified polyurethane solution at a temperature of 60-80°C, keeping the temperature for 30-50 seconds, dispersing the composite polyethylene fiber in a promoting liquid at a temperature of 50-60°C, keeping the temperature for 20-30 minutes, and post-treating to obtain a modified composite polyethylene fiber; S3, adding the modified polyimide fiber and the modified composite polyethylene fiber into a drawing frame for drawing to prepare a coarse yarn; S4, transferring the coarse yarn to an activation solution at a temperature of 70-80°C, steaming at the temperature for 30-50 minutes, and post-treating to obtain textile yarn.
2. A method for preparing a corrosion-resistant functional textile yarn according to claim 1, It is characterized in that In step S1, the dosage ratio of the modified polyurethane to isopropanol is 1g:5mL; in step S2, the promoting solution is composed of isopropanol and 1mol / L hydrochloric acid in a volume ratio of 3:2; in step S3, the weight ratio of the modified polyimide fiber to the modified composite polyethylene fiber is 2:3; in step S4, the activation solution is composed of 10wt% sodium hydroxide solution and ethanol in a volume ratio of 2:
3.
3. A method for preparing a corrosion-resistant functional textile yarn according to claim 1, It is characterized in that The modified polyurethane is processed by the following steps: A1. Add polytetrahydrofuran, 1H,1H,9H,9H-perfluoro-1,9-nonanediol and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 55-60° C., add isophorone diisocyanate solution into the reactor, keep the temperature for 90-120 min, add a chain extender into the reactor, keep the temperature for 2-3 h, add 3-aminopropyltriethoxysilane into the reactor, keep the temperature for 60-80 min, and perform post-treatment to obtain polyurethane. A2. Add polyurethane, glycidyl methacrylate, toluene and catalyst into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 70-80°C and keep the reaction temperature for 4-6 hours. Post-treat to obtain modified polyurethane.
4. A method for preparing a corrosion-resistant functional textile yarn according to claim 3, It is characterized in that In step A1, the molecular weight of the polytetrahydrofuran is 650±25, the amount ratio of the polytetrahydrofuran, 1H,1H,9H,9H-perfluoro-1,9-nonanediol 412, tetrahydrofuran, isophorone diisocyanate solution 222.23, chain extender and 3-aminopropyltriethoxysilane is 10g:6g:50mL:8g:1g:4g, and the isophorone diisocyanate solution is composed of isophorone diisocyanate and tetrahydrofuran in an amount ratio of 2g:3mL; in step A2, the amount ratio of the polyurethane, glycidyl methacrylate, toluene and catalyst is 10g:1-2g:50mL:0.1g, and the catalyst is chloroplatinic acid.
5. A method for preparing a corrosion-resistant functional textile yarn according to claim 3, It is characterized in that The preparation method of the chain extender is as follows: 3-aminopropyltriethoxysilane, dimethoxysilane, triethoxysilane and anhydrous ethanol are added into a reaction kettle and stirred, the temperature of the reaction kettle is increased to 50-60° C., 1 mol / L ammonia water is added into the reaction kettle, the reaction is carried out by heat preservation for 4-6 hours, and the chain extender is obtained by post-treatment, wherein the molar ratio of the 3-aminopropyltriethoxysilane, dimethoxysilane and triethoxysilane is 2:7:
3.
6. A method for preparing a corrosion-resistant functional textile yarn according to claim 1, It is characterized in that The composite polyethylene fiber is obtained by processing the following steps: B1. Add polyethylene powder, reinforcing modifier and white oil into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 70-80°C, keep warm and stir for 8-12 hours, add initiator and additives into the reactor to obtain a mixed solution. B2, adding the mixed solution into a twin-screw extruder, after being extruded by the twin-screw extruder, spraying it from a spinneret into a low-temperature curing liquid, and post-processing to obtain a composite polyethylene fiber precursor; B3. Thermally stretching the composite polyethylene fiber precursor to prepare composite polyethylene fibers with a fineness of 20-25 tex.
7. A method for preparing a corrosion-resistant functional textile yarn according to claim 6, It is characterized in that In step B1, the molecular weight of the polyethylene powder is 1.5 million-2.5 million, the amount ratio of the polyethylene powder, the reinforcing modifier, the white oil, the initiator and the additive is 10-15g:3-5g:40-50mL:0.1-0.2g:0.1g, and the reinforcing modifier is composed of carboxylated multi-walled carbon nanotubes and 5-hexenyltrimethoxysilane in a weight ratio of 3:1; in step B2, the temperatures of the 8 temperature intervals of the twin-screw extruder from the feed end to the discharge end are 90°C, 150°C, 230°C, 230°C, 230°C, 230°C, 200°C, and 180°C, respectively, and the aperture of the spinneret hole on the spinneret is 0.9-1.1mm , the aspect ratio is 8:1, the temperature of the low-temperature solidifying liquid is 5-10°C, the solidifying liquid is composed of dichloromethane and nonylphenol polyoxyethylene ether in a dosage ratio of 10mL:0.2g, and the post-treatment includes: after being solidified by the solidifying liquid, washing the fiber 3 times with dichloromethane, transferring it to a drying oven at a temperature of 50-60°C, and drying it to constant weight to obtain a composite polyethylene fiber precursor; in step B3, the hot stretching includes primary stretching, secondary stretching and tertiary stretching, the primary stretching temperature is 80-85°C, the stretching ratio is 15 times, the secondary stretching temperature is 100°C, the stretching ratio is 2 times, and the tertiary stretching temperature is 115°C, and the stretching ratio is 1.5 times.
8. The method for preparing a corrosion-resistant functional textile yarn according to claim 1, It is characterized in that The modified polyimide fiber is processed by the following steps: C1. Add the polyimide fiber and the pretreatment solution into a reactor and stir, raise the temperature of the reactor to 70-80° C., keep the temperature for 20-30 minutes, and post-treat to obtain the pretreatment polyimide fiber; C2. Add the pretreated polyimide fiber and Tris-HCl aqueous solution into the reactor and stir. The temperature of the reactor is raised to 55-65° C., and dopamine hydrochloride solution is added into the reactor. The mixture is stirred for 12-14 hours at the temperature maintained. The modified polyimide fiber is obtained by post-treatment.
9. A method for preparing a corrosion-resistant functional textile yarn according to claim 8, It is characterized in that In step C1, the fineness of the polyimide fiber is 20-30tex, the dosage ratio of the polyimide fiber to the pretreatment solution is 1g:10mL, and the pretreatment solution consists of 2mol / L hydrochloric acid and 10wt% hydrogen peroxide in a volume ratio of 3:1; in step C2, the pH of the Tris-HCl aqueous solution is 8.5, the dosage ratio of the pretreated polyimide fiber, the Tris-HCl aqueous solution and the dopamine hydrochloride solution is 10g:500mL:5-10g, and the dopamine hydrochloride solution consists of dopamine hydrochloride and purified water in a weight ratio of 1g:10mL.
10. A corrosion-resistant functional textile yarn, It is characterized in that The corrosion-resistant functional textile yarn is prepared by the method for preparing a corrosion-resistant functional textile yarn as described in any one of claims 1 to 9.