Steel rail near tread plane strain fracture toughness KIC test method
Through the combination of C-shaped tensile specimen and MTS810 material testing machine, the problem in the existing technology of detecting the fracture toughness KIC of the hardened layer of the rail head is solved, and the accurate fracture toughness of the hardened layer near the tread of the quenched rail head is achieved. The test overcomes the limitations of the three-point bending fixture on the sample size, and the test results are true and effective.
Patent Information
- Application Number
- CN202410848904.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
AI Technical Summary
The existing technology is difficult to effectively detect the fracture toughness KIC of the hardened layer of the rail head, especially due to the limitation of the sample size by the three-point bending fixture, which makes it impossible to accurately detect the fracture toughness of the hardened layer near the tread of the quenched rail head.
A C-shaped tensile specimen was used to conduct the plane strain fracture toughness KIC test. By adjusting the specimen width W and the notch position, combined with the MTS810 material testing machine, the KQ value was calculated to determine the KIC to meet specific validity criteria.
It achieves accurate detection of the fracture toughness KIC of the rail head near the tread, avoids the limitation of the sample size by the three-point bending fixture, and can detect the fracture toughness of smaller ligament heights. The method is simple, easy to operate and the results are real and effective.
Smart Images

Figure CN118746490A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of railway transportation and metal material detection, and in particular relates to a plane strain fracture toughness K of a rail near the tread surface. IC Test method. Background Art
[0002] With the increase in speed and heavy-duty of railway transportation, the damage of rails is becoming more and more serious. It is particularly important to improve the comprehensive performance of rails, especially the toughness of rail heads. Domestic and foreign practices have shown that the combination of alloy strengthening and heat treatment can produce high-strength and high-toughness rails with high strength and good plasticity. In particular, the heat treatment method has low cost and good effect. However, different quenching processes have different effects on the performance of rail heads. It is required to test the shape and depth of the quenched hardened layer (hat shape), the refinement of the structure, the reasonable distribution of hardness and other indicators of the rail head, especially the fracture toughness K of the hardened layer of the rail head. IC The detection of the hardened layer of the quenched rail tread has always troubled the inspectors, because the depth of the hardened layer on the tread of the quenched rail is about 10-15mm, and the strength and hardness of the hardened layer at different depths are different. IC According to the standard of TB / T2344-2020, a 25×40×180mm SEB specimen is used to test the ligament below 20±2mm below the rail head tread. IC To detect the defect, it is necessary to change the notch position and orientation and reduce the sample size, but this cannot be achieved due to the limitations of the three-point bending fixture.
[0003] In order to truly reflect the fracture toughness of the hardened layer at different depths of the rail head of the quenched rail, we have calculated the fracture toughness of the hardened layer at different depths according to the national standard GB / T4161-2007 "Plane Strain Fracture Toughness K of Metallic Materials". IC Test Method》A plane strain fracture toughness K of the rail near the tread surface was designed IC Test method. Summary of the invention
[0004] The purpose of the present invention is to provide a plane strain fracture toughness K of a rail near the tread surface. IC The test method has simple principle, convenient operation, strong practicability and true and effective results.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A plane strain fracture toughness K of a rail near the tread surface of the present invention IC The test method comprises: preparing a test specimen using a C-shaped tensile specimen with W / B=2, a ratio X / W=0.5, and no restriction on r1 / r2; the fracture toughness K of the C-shaped tensile specimen ICThe test was carried out on an MTS810 material testing machine (imported from the United States). The pre-cracked C-shaped tensile specimen was clamped onto the U-shaped fixture, and then the clamping end of the U-shaped fixture was installed onto the upper and lower chucks of the MTS810 material testing machine, tightened. Set the loading rate to 100 N / second, zero the extensometer, and then the plane strain fracture toughness K IC test can be started;
[0007] The K of the test data of the C-shaped tensile specimen Q is calculated by the following formula:
[0008] K Q =(F Q / BW 1 / 2 )[3X / W + 1.9 + 1.1a / W][1 + 0.25(1 - a / W) 2 (1 - r1 / r2)]f(a / W);
[0009] where: f(a / W)=[(a / W) 1 / 2 / (1 - a / W) 3 / 2 ×[3.74 - 6.30a / W + 6.32(a / W) 2 - 2.43(a / W) 3 ;
[0010] W is the specimen width in mm, B is the specimen thickness in mm, r1 / r2 is the ratio of the inner and outer radii of the specimen; a is the crack length of the specimen in mm, and X is the offset dimension of the loading hole.
[0011] Further, the W value of the C-shaped tensile specimen is selected according to the depth of the hardened layer on the tread of the quenched rail to be detected, or the W value is selected according to the distance from the rail tread height to be detected, so as to determine the thickness of the detected fracture ligament.
[0012] Further, the C-shaped tensile specimen is taken from the cross-section of the rail head. The specimen is processed by using a sawing machine to saw the blank of the specimen shape from the rail head, and after machining by a lathe and a milling machine, it is finally processed by a grinding machine.
[0013] Further, after being processed by a grinding machine, the surface roughness of the C-shaped tensile specimen is ≤1.6 μm, and the parallelism and perpendicularity of the specimen are not less than 0.2%W.
[0014] Further, the notch offset of the C-shaped tensile specimen is within ±2°, the width is within 0.1W, but not less than 1.6 mm; the root radius of the V-shaped notch of the specimen is not more than 0.1 mm, and it is processed by molybdenum wire cutting.
[0015] Further, the C-shaped tensile specimen is symmetrically cut with dovetail grooves at a distance of 6 mm from the center line outside the notch by wire cutting for clamping the extensometer.
[0016] Furthermore, the corresponding fixture is a U-clamp. When clamping, the C-shaped tensile specimen should be located in the center of the U-shaped hook with a deviation within 0.76 mm, and the center line deviation of the upper and lower force rods should be within 0.76 mm.
[0017] Furthermore, the C-shaped tensile specimen prefabricated fatigue crack was carried out on an MTS810 material testing machine imported from the United States, with an expansion of at least 0.025W, or 1.3mm, whichever is greater, and the sum of the notch and the prefabricated fatigue crack length was 0.5W.
[0018] Furthermore, the plane strain fracture toughness K IC Criteria for validity of test results:
[0019] Fmax / F Q ≤1.10;
[0020] W≥2.5(K Q / R p0.2 ) 2 ;
[0021] B≥2.5(K Q / R p0.2 ) 2 ;
[0022] Wa≥2.5(K Q / R p0.2 ) 2 .
[0023] All the above conditions must be met, K Q Then it is equal to K IC , otherwise it is not a valid K IC test;
[0024] Where: Fmax is the maximum force value in MPa, F Q is the specific force value kN, K Q为 K IC The conditional value Mpam 1 / 2 , K IC K I Critical value Mpam 1 / 2 , K I is the opening stress intensity factor, R p0.2 is the tensile yield strength and Wa is the ligament length.
[0025] Compared with the prior art, the beneficial technical effects of the present invention are:
[0026] The present invention abandons the SEB specimen adopted in the TB / T2344-2020 standard and adopts a C-shaped tensile specimen, which avoids the SEB specimen plane strain fracture toughness K ICThe three-point bending fixture used in the test limits the sample size, which can detect the fracture toughness K of smaller ligament heights. IC .
[0027] Using a C-shaped tensile specimen, the fracture toughness K can be changed by changing the specimen width W. IC Ligament height, solve the problem of testing the fracture toughness K of the rail head near the tread surface IC problem.
[0028] The present invention provides a plane strain fracture toughness K of a rail near the tread surface. IC The test method has simple principle, convenient operation, strong practicability and true and effective results. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The present invention will be further described below in conjunction with the accompanying drawings.
[0030] Figure 1 Schematic diagram of C-shaped tensile specimen for plane strain fracture toughness KIC test;
[0031] Figure 2 Schematic diagram of detecting different heights of rail head near tread surface by selecting different W;
[0032] Figure 3 Schematic diagram of the dovetail groove of the extensometer clamped at the notch of the specimen during wire cutting;
[0033] Figure 4 Symbols and illustrations;
[0034] Figure 5 Schematic diagram of ligament location testing according to national standard GB / T4161-2007. DETAILED DESCRIPTION
[0035] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0036] A plane strain fracture toughness K of a rail near the tread surface of the present invention IC The test method is mainly used to solve the problem that the plane strain fracture toughness K of the hardened layer of the rail head of the quenched rail cannot be tested according to the SEB specimen adopted in the TB / T2344-2020 standard due to the limitation of the specimen size by the three-point bending fixture. IC The test specimen is a C-shaped tensile specimen with W / B=2, a ratio of X / W=0.5, no restriction on r1 / r2, and the shape, size and notch of the specimen are as follows: Figure 1 The C-shaped tensile test specimen selects the W value according to the depth of the hardened layer of the quenched rail tread to be tested, or selects the W value according to the distance of the rail tread to be tested, so as to determine the thickness of the tested fracture ligament, for example Figure 2 h1, h2 and h3 shown.
[0037] The C-shaped tensile specimen is taken from the cross section of the rail head. Figure 2 As shown, the sample is processed by using a sawing machine to cut the sample shape blank from the rail head, and then processed by a lathe and a milling machine, and finally completed by an internal cylindrical grinder and a surface grinder.
[0038] After the C-shaped tensile specimen is processed by a grinder, the surface roughness of the specimen is ≤1.6 μm, and the parallelism and verticality of the specimen are not less than 0.2%W.
[0039] The notch offset of the C-shaped tensile specimen is within ±2°, and the width is within 0.1W, but not less than 1.6mm. The root radius of the V-shaped notch of the specimen is not greater than 0.1mm, and molybdenum wire cutting is used.
[0040] The C-shaped tensile specimen is cut symmetrically with a dovetail groove at the outside of the notch and 6 mm from the center line by wire cutting to clamp the extensometer. Figure 3 shown.
[0041] The corresponding fixture is a U-clamp. When clamping, the C-shaped tensile specimen should be located in the center of the U-shaped hook with a deviation within 0.76 mm, and the center line deviation of the upper and lower force rods should be within 0.76 mm.
[0042] The C-shaped tensile specimen prefabricated fatigue crack was carried out on an MTS810 material testing machine imported from the United States, with an expansion of at least 0.025W, or 1.3mm, whichever is greater, and the sum of the notch and the prefabricated fatigue crack length was 0.5W.
[0043] The fracture toughness K of the C-shaped tensile specimen IC The test was carried out on an MTS810 material testing machine. The C-shaped tensile specimen with prefabricated cracks was clamped on the U-clamp, and then the clamping end of the U-clamp was installed on the upper and lower chucks of the MTS810 material testing machine. After clamping, the loading rate was set to 100N / s, the extensometer was cleared, and the plane strain fracture toughness KIC test could be started.
[0044] The K of the C-shaped tensile specimen test data Q Calculated by the following formula:
[0045] K Q =(F Q / BW 1 / 2 )[3X / W+1.9+1.1a / W][1+0.25(1-a / W) 2 (1-r1 / r2)]f(a / W)
[0046] Among them: f(a / W)=[(a / W) 1 / 2 / (1-a / W) 3 / 2×[3.74 - 6.30a / W + 6.32(a / W) 2 -2.43(a / W) 3
[0047] The plane strain fracture toughness K IC Criterion conditions for the validity of test results:
[0048] Fmax / F Q ≤1.10;
[0049] W ≥ 2.5(K Q / R p0.2 ) 2 ;
[0050] B ≥ 2.5(K Q / R p0.2 ) 2 ;
[0051] W - a ≥ 2.5(K Q / R p0.2 ) 2 .
[0052] All of the above conditions must be satisfied, and K Q is then equal to K IC , otherwise it is not a valid K IC test.
[0053] For the notations used in the calculation formula and criterion conditions, see Figure 4 .
[0054] Just record the experimental data in the original data record book and issue the test report in the format required by GB / T 4161 - 2007 "Test Method for Plane Strain Fracture Toughness KIC of Metallic Materials".
[0055] The embodiments described above are only descriptions of the preferred embodiments of the present invention and do not limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations and improvements made by those of ordinary skill in the art to the technical solutions of the present invention shall fall within the protection scope determined by the claims of the present invention.
Claims
1. A plane strain fracture toughness K of rail near tread surface IC The test method is characterized in that include: The test specimens prepared were C-shaped tensile specimens with W / B=2, a ratio of X / W=0.5, and no restriction on r1 / r2; the fracture toughness K of the C-shaped tensile specimens IC The test was carried out on an MTS810 material testing machine. The C-shaped tensile specimen with prefabricated cracks was clamped on the U fixture, and then the clamping end of the U fixture was installed on the upper and lower chucks of the MTS810 material testing machine. The test was clamped and the loading rate was set to 100N / s. The extensometer was cleared to zero, and the plane strain fracture toughness K was tested. IC test; The K of the C-shaped tensile specimen test data Q Calculated by the following formula: K Q =(F Q / BW 1 / 2 )[3X / W+1.9+1.1a / W][1+0.25(1-a / W) 2 (1-r1 / r2)]f(a / W); Where: f(a / W) = [(a / W) 1 / 2 / (1-a / W) 3 / 2 ]×[3.74-6.30a / W+6.32(a / W) 2 -2.43(a / W) 3 ]; W is the width of the specimen in mm, B is the thickness of the specimen in mm, r1 / r2 is the ratio of the inner and outer radii of the specimen; a is the crack length of the specimen in mm, and X is the offset size of the force-adding hole.
2. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The C-shaped tensile test specimen selects a W value according to the depth of the hardened layer of the quenched rail tread to be tested, or selects a W value according to the height of the rail tread to be tested, so as to determine the thickness of the tested fracture ligament.
3. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The C-shaped tensile test specimen is taken from the cross section of the rail head. The specimen is processed by sawing the specimen shape blank from the rail head using a sawing machine, and then processed by a lathe and a milling machine, and finally completed by a grinder.
4. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that After the C-shaped tensile specimen is processed by a grinder, the surface roughness of the specimen is ≤1.6 μm, and the parallelism and verticality of the specimen are not less than 0.2%W.
5. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The notch offset of the C-shaped tensile specimen is within ±2°, and the width is within 0.1W, but not less than 1.6mm; the root radius of the V-shaped notch of the specimen is not greater than 0.1mm, and molybdenum wire cutting is used.
6. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The C-shaped tensile specimen is cut symmetrically with a dovetail groove at the outside of the notch and 6 mm away from the center line by wire cutting to clamp the extensometer.
7. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The corresponding fixture is a U-clamp. When clamping, the C-shaped tensile specimen should be located in the center of the U-shaped hook with a deviation within 0.76 mm, and the center line deviation of the upper and lower force rods should be within 0.76 mm.
8. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The C-shaped tensile specimen prefabricated fatigue crack was carried out on an MTS810 material testing machine imported from the United States, with an expansion of at least 0.025W, or 1.3mm, whichever is greater, and the sum of the notch and the prefabricated fatigue crack length was 0.5W.
9. The plane strain fracture toughness K of the rail near the tread surface according to claim 1 IC The test method is characterized in that The plane strain fracture toughness K IC Criteria for validity of test results: Fmax / F Q ≤1.10; W≥2.5(K Q / R p0.2 ) 2 ; B≥2.5(K Q / R p0.2 ) 2 ; W-a≥2.5(K Q / R p0.2 ) 2 。 All the above conditions must be met, K Q Then it is equal to K IC , otherwise it is not a valid K IC test; Where: Fmax is the maximum force value in MPa, F Q is the specific force value kN, K Q为 K IC The conditional value Mpam 1 / 2 , K IC K I Critical value Mpam 1 / 2 , K I is the opening stress intensity factor, R p0.2 is the tensile yield strength and Wa is the ligament length.
Citation Information
Cited By
Sample for detecting near-tread fatigue crack growth rate of rail head of steel rail
CN119147331A
A specimen for detecting the fatigue crack propagation rate of a rail head near the tread surface
CN119147331B