Neodymium-iron-boron magnet and preparation method and application thereof
By dividing and controlling the content and diffusion zone of Tb and Dy in NdFeB magnets, the problems of insufficient anti-demagnetization performance and lack of heavy rare earth resources in NdFeB magnets in high temperature environments are solved, achieving more efficient magnet performance matching and The utilization of rare earth resources improves the coercive force and thermal stability of magnets.
Patent Information
- Application Number
- CN202410921512.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing NdFeB magnets have insufficient anti-demagnetization performance in high-temperature environments, and the scarcity of heavy rare earth resources has restricted their application. Traditional grain boundary diffusion technology is difficult to meet the performance needs of different regions.
By setting a three-dimensional rectangular coordinate system in the NdFeB magnet, the easy demagnetization zone, the transition zone and the non-easy demagnetization zone are divided, and the content ratio and diffusion increment of Tb and Dy are controlled in each zone, and the crystal structure parallel to the orientation direction is used. Boundary diffusion technology applies a diffusion source to form a gradient structure to improve anti-demagnetization performance.
On the premise of ensuring residual magnetism, the attenuation of surface magnetism and magnetic flux of NdFeB magnets is reduced, the resistance to demagnetization is improved, the coercive force and thermal stability of the magnets are improved, and the use of heavy rare earths is reduced.
Smart Images

Figure CN118748112A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a neodymium iron boron magnet and a preparation method and application thereof. Background Art
[0002] Since the advent of NdFeB permanent magnet materials, they have been widely used in the fields of automobiles, wind power, home appliances, industrial robots, etc. Due to the different working conditions in various fields, the performance requirements of magnetic steel for products in their fields are also different. In recent years, new energy vehicles have flourished, and the demand for magnetic steel in the main drive motor has increased sharply. Since the normal operating temperature of the main drive motor is mainly concentrated in the range of 120-180°C, NdFeB requires higher coercive force and thermal stability. In order to improve the temperature resistance of rare earth permanent magnets, a large amount of heavy rare earth Dy and Tb is usually added to increase the main phase magnetocrystalline anisotropy field. However, the scarcity of heavy rare earth resources and high prices have seriously restricted the application of NdFeB magnets in various industries.
[0003] With the increasing demand for high-performance magnets, grain boundary diffusion technology has gradually become known and accepted by everyone. Conventional grain boundary diffusion technology uses a physical vapor deposition method to deposit the diffusion source on the surface of the magnet and then penetrate the diffusion source into the interior of the magnet along the grain boundary under high temperature and a certain pressure. The biggest advantage of this technology is that it only uses a small amount of heavy rare earth and can greatly improve the coercive force while keeping its remanence almost unchanged. In terms of the effective utilization rate of heavy rare earth, traditional grain boundary diffusion products have been greatly improved compared with non-grain boundary diffusion products.
[0004] However, in the actual use of NdFeB, the performance requirements for each part of the magnet are not the same. For example, in the motor, the reverse magnetic field generated by the motor coil after power is turned on is not a uniform magnetic field. Therefore, how to design a NdFeB magnet according to the needs of different regions to meet the needs of different applications, while ensuring coercive force and remanence, and also having good anti-demagnetization ability. Summary of the invention
[0005] In order to solve the defects in the prior art, the present invention provides a NdFeB magnet and a preparation method and application thereof. The NdFeB magnet of the present invention can reduce the attenuation of the surface magnetism and magnetic flux of the NdFeB magnet while ensuring the residual magnetism, and has good anti-demagnetization performance.
[0006] In a first aspect, the present invention provides a NdFeB magnet, and establishes a three-dimensional rectangular coordinate system, with the orientation direction being the Z-axis direction, and the origin of the three-dimensional rectangular coordinate system is located inside the NdFeB magnet;
[0007] The NdFeB magnet comprises a non-demagnetization zone, a transition zone and an easy demagnetization zone; the easy demagnetization zone is an outer annular zone located on the NdFeB magnet along the Z-axis direction, and the non-demagnetization zone is a central zone located on the NdFeB magnet along the Z-axis direction; the transition zone is a boundary zone between the easy demagnetization zone and the non-demagnetization zone;
[0008] The Tb content ratio of the non-demagnetization-prone region, the transition region and the demagnetization-prone region is (0-0.05):(0.95-1):1;
[0009] The Dy content ratio among the non-demagnetization-prone region, the transition region and the demagnetization-prone region is 1:1:1.
[0010] In the present invention, in the “outer edge annular region along the Z-axis direction”, the central axis of the “outer edge annular region” is parallel to the Z-axis.
[0011] About parameters
[0012] In the present invention, preferably, the content of heavy rare earth at each position in the easily demagnetized region is the same.
[0013] In the present invention, preferably, the diffusion increment of heavy rare earth at the same XY position along the Z axis in the transition zone is the same. Preferably, the diffusion content of Tb in the transition zone along the X axis or Y axis and away from the easy demagnetization zone decreases.
[0014] In the present invention, preferably, the contents of Tb at any two locations with the same XY position in the easy demagnetization region are the same.
[0015] In the present invention, preferably, the contents of Dy at any two positions in the easily demagnetized region, the transition region, and the non-easy demagnetized region are the same.
[0016] In the present invention, the diffusion increment of the heavy rare earth means the percentage of the mass of Tb introduced into a certain area by diffusion to the total mass of the magnet in the area. Specifically, the diffusion increment of Tb means the percentage of the mass of Tb introduced into a certain area by diffusion to the total mass of the magnet in the area; the diffusion increment of Dy means the percentage of the mass of Dy introduced into a certain area by diffusion to the total mass of the magnet in the area.
[0017] In the present invention, the "same diffusion increment of heavy rare earth" means that the types of heavy rare earth introduced by diffusion at various positions in a certain area are the same, and the diffusion increment of each heavy rare earth is the same. Specifically, the same diffusion increment of Tb means that the diffusion increment of Tb introduced by diffusion is the same; the same diffusion increment of Dy means that the diffusion increment of Dy introduced by diffusion is the same.
[0018] In the present invention, the Tb content ratio of the transition region to the easily demagnetized region may be 0.8:1 or 0.9:1.
[0019] In the present invention, the Tb content ratio of the transition region to the non-demagnetized region may be 1:(0-0.1), preferably 1:(0-0.05).
[0020] In the present invention, the Tb content ratio of the non-demagnetized region and the easily demagnetized region may be (0-0.9):1, for example, 0.1:1, 0.2:1 or 0.7:1.
[0021] In the present invention, the ratio of the diffusion increment of Tb in the easily demagnetized region to the diffusion increment of Tb in the non-easy demagnetized region may be (1-100):1, for example, 9:1, 36:1 or 55:1.
[0022] In the present invention, the ratio of the diffusion increment of Tb in the easy demagnetization zone to the diffusion increment of Tb in the transition zone may be (1-1.1):1, for example, 1:1, 36:34 or 55:52.
[0023] In the present invention, the diffusion increment of Tb in the easily demagnetized region may be 0.1 wt%-1 wt%, for example, 0.35 wt%, 0.36 wt%, 0.45 wt% or 0.55 wt%.
[0024] In the present invention, the diffusion increment of Tb in the non-demagnetization-prone region may be 0-0.1 wt %, preferably 0-0.05 wt %, such as 0, 0.01 wt % or 0.05 wt %.
[0025] In the present invention, the diffusion increment of Tb in the transition zone may be 0.1 wt%-1 wt%, for example, 0.34 wt%, 0.45 wt% or 0.52 wt%.
[0026] In the present invention, the diffusion increment of Dy in the easily demagnetized area may be 0.1 wt%-1 wt%, for example, 0.55 wt%.
[0027] In the present invention, the diffusion increment of Dy in the non-demagnetizable region may be 0.1wt%-1wt%, preferably 0.4wt%-0.7wt%, for example 0.55wt%.
[0028] In the present invention, the diffusion increment of Dy in the transition zone may be 0.1 wt%-1 wt%, for example, 0.55 wt%.
[0029] In the present invention, an interface A exists between the transition zone and the easily demagnetized zone, and the content of heavy rare earth at each position of the interface A is the same.
[0030] The diffusion increment of Tb at the interface A may be 0.3wt%-0.7wt%, for example, 0.36wt%, 0.45wt% or 0.55wt%.
[0031] The diffusion increment ratio of the interface A to the Tb in the easily demagnetized zone is preferably (0.95-1):1.
[0032] The diffusion increment of Dy at the interface A may be 0.4wt%-0.7wt%, for example 0.55wt%.
[0033] In the present invention, an interface B exists between the transition zone and the non-easily demagnetized zone, and the content of heavy rare earth at each position of the interface B is the same.
[0034] The diffusion increment of Tb at the interface B may be 0.3wt%-0.7wt%, for example, 0.34wt%, 0.43wt% or 0.52wt%.
[0035] The diffusion increment ratio of the interface B to the Tb in the non-demagnetization-prone region is preferably (6-60):1, such as 43:5, 34:1 or 52:1.
[0036] The diffusion increment of Dy at the interface B may be 0.4wt%-0.7wt%, for example 0.55wt%.
[0037] In the present invention, the coercivity ratio of the easily demagnetized region to the non-easily demagnetized region may be 1:(0.7-0.96), for example, 1:0.876, 1:0.909 or 1:0.957.
[0038] In the present invention, the coercivity ratio of the easy demagnetization region to the transition region may be 1:(0.93-1), for example, 1:0.930, 1:0.959 or 1:0.970.
[0039] In the present invention, the coercive force at each position of the easy demagnetization region may be the same.
[0040] In the present invention, the coercive force at each position of the transition zone along the Z-axis direction may be the same. Preferably, the coercive force in the transition zone along the X-axis or the Y-axis and away from the easy demagnetization zone decreases.
[0041] In the present invention, the remanence at various positions of the easily demagnetized area may be the same.
[0042] In the present invention, the remanence at each position of the transition zone along the Z-axis direction may be the same. Preferably, the remanence in the transition zone along the X-axis or Y-axis and away from the easy demagnetization zone decreases gradually.
[0043] About composition
[0044] In the present invention, the NdFeB magnet can be represented by the chemical formula R1-R2-TBM, wherein R1 can be one or more of Pr, Nd, Ce, Er, Tm, Y, Lu, Gd and Ho; R2 can be Dy and / or Tb; T can be one or more of Fe, Zn, Si, V, Cr, Mn, Ni, Ge, Nb, Mo, Pd, Ag, Cd, Sb, Hf, Ta, W, O, C, N, S, F and P; M can be one or more of Cu, Al, Co, Ga, Zr and Ti.
[0045] In certain embodiments of the present invention, all of the M elements are derived from the NdFeB matrix.
[0046] In certain embodiments of the present invention, the M element comprises an M element introduced by diffusion, wherein the mass percentage of the M element introduced by diffusion in the NdFeB magnet is preferably 0-0.4%.
[0047] In certain embodiments of the present invention, the microstructure of the NdFeB magnet includes Re2Fe 14 B main phase grains and Re-rich phase grain boundaries; the Re2Fe 14 The B main phase grains include a core layer and a shell layer; the Re is one or more of Nd, Dy and Tb.
[0048]
【Re2Fe 14 B main phase grains
[0049] Wherein, the Re2Fe 14 The difference in the grain size of the B main phase grains may not exceed 8 μm.
[0050] Among them, the Re2Fe 14 The difference in the grain size of the B main phase grains may not exceed 8 μm.
[0051] Among them, the Re2Fe 14 The grain sizes of the B main phase grains may be equal, wherein the surface layer refers to the surface perpendicular to the orientation direction.
[0052] Among them, the Re2Fe 14 The grain sizes of the B main phase grains may be equal, wherein the center means the median plane along the orientation direction.
[0053] In some specific embodiments of the present invention, in the easily demagnetized region, the transition region and the non-easy demagnetized region, the surface layer of Re2Fe 14The grain size of the B main phase grains is preferably 1-1.5 times the grain size of the central main phase grains.
[0054] In a specific embodiment of the present invention, the Re2Fe 14 The grain size ratio of the B main phase grains is 1:1:1.
[0055] In some specific embodiments of the present invention, the Re2Fe 14 The particle size of the B main phase grains is preferably 1-12 μm.
[0056] In the above text, the grain size refers to the average size of all grains in a certain area. 14 The grain size of the B main phase grains means that all Re2Fe 14 The average value of the grain size of the B main phase grains.
[0057]
Re-rich phase grain boundary
[0058] In the present invention, the Re-rich phase grain boundary has the conventional meaning in the art, that is, the grain boundary region between two particles with Re>95%.
[0059] The thickness of the Re-rich phase grain boundaries in the easy demagnetization zone may be equal, that is, the thickness of the Re-rich phase grain boundaries in each region in the easy demagnetization zone remains unchanged.
[0060] The thickness of the Re-rich phase grain boundaries in the transition zone may be equal, that is, the thickness of the Re-rich phase grain boundaries in various regions in the transition zone remains unchanged.
[0061] In certain specific embodiments of the present invention, the thickness of the Re-rich phase grain boundary in the easily demagnetized region is 0.4-1 μm, such as 0.5 μm or 0.55 μm.
[0062] In certain specific embodiments of the present invention, the thickness of the Re-rich phase grain boundary in the transition zone is 0.4-1 μm, such as 0.5 μm or 0.52 μm.
[0063] In certain specific embodiments of the present invention, the thickness of the Re-rich phase grain boundary in the non-easily demagnetized region is 0.2-0.5 μm, such as 0.20 μm, 0.23 μm or 0.25 μm.
[0064] [Core and Shell]
[0065] In certain embodiments of the present invention, the shell layer is conventional Re2Fe 14 B hard magnetic layer.
[0066] In certain embodiments of the present invention, the shell layer of the easily demagnetized region is (Nd, Dy, Tb)2Fe 14 B hard magnetic layer.
[0067] In some embodiments of the present invention, the shell layer of the non-demagnetized region is (Nd, Dy)2Fe 14 B hard magnetic layer.
[0068] Among them, the core layer and shell layer in the easily demagnetized zone, the transition zone and the non-easy demagnetized zone can each independently meet the following conditions: the R1 content in the core layer is not less than the R1 content in the shell layer; the R2 content in the core layer is less than the R2 content in the shell layer.
[0069] Wherein, the R2 is Tb, and the content of R2 in the easily demagnetized region, the transition region and the non-easy demagnetized region may satisfy the following condition: easily demagnetized region ≥ transition region > non-easy demagnetized region.
[0070] Wherein, the R2 is Dy, and the content of R2 in the easily demagnetized region, the transition region and the non-easy demagnetized region may satisfy the following condition: non-easy demagnetized region=transition region=easy demagnetized region.
[0071] The thickness of the shell layer of the easily demagnetized region may be equal, that is, the thickness of the shell layer of each region in the easily demagnetized region remains unchanged.
[0072] The thickness of the shell layer in the transition zone may be equal, that is, the thickness of the shell layer in each area in the transition zone remains unchanged.
[0073] In certain specific embodiments of the present invention, the thickness of the shell layer of the easily demagnetized region is 2-3 μm, such as 2 μm, 2.1 μm or 2.5 μm.
[0074] In certain specific embodiments of the present invention, the thickness of the shell layer of the main phase grains in the transition zone is 2-2.5 μm, for example, 2 μm or 2.38 μm.
[0075] In certain specific embodiments of the present invention, the thickness of the shell layer of the main phase grains in the non-easily demagnetized region is 0.5-2 μm, such as 0.95 μm, 1.0 μm or 1.1 μm.
[0076] In certain specific embodiments of the present invention, the thickness ratio of the shell layer of the easily demagnetized region and the Re-rich phase grain boundary is preferably (2-3):(0.4-1), for example, 4:1, 2.1:0.5 or 2.5:0.55.
[0077] In certain specific embodiments of the present invention, the thickness ratio of the shell layer in the transition zone and the Re-rich phase grain boundary is preferably (2-2.5):(0.4-1), for example 4:1 or 2.38:0.52.
[0078] In certain specific embodiments of the present invention, the thickness ratio of the shell layer of the main phase grains in the non-easily demagnetized zone and the Re-rich phase grain boundary is preferably (0.5-2):(0.2-0.5), for example, 1.1:0.25, 1.0:0.23 or 0.95:0.20.
[0079] About structure
[0080] In the present invention, the NdFeB magnet may be a rectangular parallelepiped, the origin may be located at the center of the upper surface of the rectangular parallelepiped, and the X-axis of the three-dimensional rectangular coordinate system may be parallel to one side of the upper surface.
[0081] In the present invention, the specific position of the upper surface is not specifically limited. Those skilled in the art can generally understand that the upper surface refers to the surface opposite to a plane when the magnet is placed on the plane.
[0082] Among them, the ratio of the length to the width of the NdFeB magnet is (2-5):1, preferably (2.42-3.7):1, for example 3:1, 3.65:1 or 39:10.7, the length refers to the extension distance of one side of the upper surface along the positive direction of the X-axis; the width refers to the extension distance of the cuboid from the upper surface along the positive direction of the Y-axis.
[0083] In the present invention, the widths of the easily demagnetized regions may be equal, that is, the distances of the easily demagnetized regions extending from the edges of the NdFeB magnets along the X-axis or the Y-axis remain unchanged.
[0084] Preferably, the width of the easily demagnetized area is not greater than 5 mm, for example, 2-4 mm.
[0085] In the present invention, on any plane perpendicular to the orientation direction, the shape of the non-demagnetization region may be an ellipse.
[0086] The ratio of the major axis a to the minor axis b of the non-demagnetizable region may be (2-15):1, for example, 17.5:3.35.
[0087] In the present invention, the widths of the transition zones may be equal, that is, the distances of the transition zones extending from the edges of the NdFeB magnets along the X-axis or the Y-axis remain unchanged.
[0088] Preferably, the width of the transition zone is 0-2 mm, not 0, for example 0.5 mm.
[0089] In the present invention, the volume of the easily demagnetized area may account for 40%-90% of the volume of the NdFeB magnet, for example, 47.85%.
[0090] In the present invention, the percentage of the volume of the transition zone to the volume of the NdFeB magnet may be 0-28.4%, for example 8.04%.
[0091] In the present invention, the percentage of the volume of the non-demagnetized area to the volume of the NdFeB magnet may be 15.7%-44.11%.
[0092] In the present invention, the non-demagnetization-prone region, transition region and demagnetization-prone region can be obtained by simulating cloud maps under working conditions.
[0093] In the present invention, the thickness of the NdFeB magnet may be no greater than 5 mm, for example, 3 mm.
[0094] In a second aspect, the present invention also provides a method for preparing a NdFeB magnet, which comprises the following steps: applying diffusion sources on the upper surface and / or lower surface perpendicular to the Z-axis direction on the NdFeB substrate, respectively, to carry out grain boundary diffusion parallel to the orientation direction; wherein, the diffusion source Dy is applied to the entire area of the upper surface and the lower surface, and the diffusion source Tb is applied to the outer edge annular area along the Z-axis direction to form the easily demagnetized zone, the transition zone and the non-easy demagnetized zone.
[0095] In the present invention, it is known to those skilled in the art that during grain boundary diffusion, Dy or Tb in the diffusion source is not completely diffused into the magnet, and its utilization rate is generally 85%-95%. Therefore, in the actual preparation process, a larger amount of Dy or Tb is generally applied.
[0096] In the present invention, it is known to those skilled in the art that different grain boundary diffusion methods will result in different coating thicknesses when diffusing the same amount of Dy or Tb into the magnet. Therefore, in the actual preparation process, the coating thickness is not limited as long as the corresponding Dy or Tb diffusion amount is achieved.
[0097] In the present invention, the diffusion source can be applied by conventional methods in the art, such as coating.
[0098] The coating method is preferably spraying or printing. The dewaxing temperature of the spraying can be 200-400°C. The dewaxing temperature of the printing can be 100-500°C.
[0099] In the present invention, when the diffusion source is applied by coating, the diffusion source is generally mixed with a solvent and a binder in a certain proportion to form a slurry. The solvent can be water, alcohol, ketone or ester. The mass percentage of Dy or Tb in the diffusion source in the slurry can be 0.3%-1%.
[0100] In the present invention, the diffusion source Dy may be a single substance of Dy.
[0101] In the present invention, the diffusion source Dy may be a Dy-M alloy, and M may be one or more of Cu, Al, Co, Ga, Zr and Ti. The mass percentage of M in the Dy-M alloy may not exceed 40%.
[0102] In the present invention, the diffusion source Dy may be a hydride of Dy or a fluoride of Dy.
[0103] In the present invention, the diffusion source Tb may be a single substance of Tb.
[0104] In the present invention, the diffusion source Tb may be a Tb-M alloy, and M may be one or more of Cu, Al, Co, Ga, Zr and Ti. The mass percentage of M in the Tb-M alloy may not exceed 40%.
[0105] In the present invention, the diffusion source Tb may be a hydride of Tb or a fluoride of Tb.
[0106] In the present invention, the temperature of the grain boundary diffusion may be 750-950°C, for example, 900°C.
[0107] In the present invention, the grain boundary diffusion time may be 5-30 hours, for example, 10 hours.
[0108] In the present invention, an aging treatment may be further included after the grain boundary diffusion.
[0109] The aging treatment temperature may be 300-600°C, for example 500°C.
[0110] The aging treatment time may be 1-10 hours, for example 3 hours.
[0111] In a third aspect, the present invention also provides a NdFeB magnet prepared by the method for preparing a NdFeB magnet as described above.
[0112] In a fourth aspect, the present invention also provides a use of the NdFeB magnet as described above in magnetic steel.
[0113] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0114] The reagents and raw materials used in the present invention are commercially available.
[0115] The positive and progressive effects of the present invention are:
[0116] The NdFeB magnet of the present invention includes a transition zone, and by controlling the coordination of the Tb and Dy contents introduced by diffusion in the transition zone, the easy demagnetization zone, and the non-easy demagnetization zone, it is possible to reduce the cross-zone mutual diffusion of Tb or Dy caused by the Tb concentration gradient difference in the transition zone, thereby reducing the problem of gradient decline in the performance of the boundary zone and weakening the anti-demagnetization effect. It is possible to reduce the attenuation of the surface magnetism and magnetic flux of the NdFeB magnet while ensuring the remanence of the NdFeB magnet, and improve the anti-demagnetization ability of the NdFeB magnet. In addition, the present invention sets the easy demagnetization zone, the non-easy demagnetization zone, and the transition zone as an inner ellipse and an outer square, which can improve the anti-demagnetization ability of the four long sides of the NdFeB magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0117] Figure 1 It is a schematic diagram of the structure of each area of the NdFeB magnet of the present invention;
[0118] Figure 2 The NdFeB magnet of Example 3 is Figure 1 Schematic diagram of the coercive force of test lines 1 to 4 is shown.
[0119] Figure 3 The NdFeB magnet of Example 3 is Figure 1 Schematic diagram of the diffusion increment of Tb from test line 1 to test line 4 is shown. DETAILED DESCRIPTION
[0120] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0121] Examples 1-3 and Comparative Examples 1-2
[0122] On the upper and lower surfaces of the NdFeB substrate along the Z-axis direction, Dy is sprayed on the entire area of the two surfaces, and Tb is sprayed on the outer annular area along the Z-axis direction. The dewaxing temperature of the spraying is 200°C, and the grain boundary diffusion parallel to the orientation direction is performed to obtain the NdFeB magnet, such as Figure 1 As shown; wherein the utilization rate of Dy or Tb in the diffusion source is 85%-95%.
[0123] The heat treatment temperature in the grain boundary diffusion is 900° C., and the heat treatment time is 10 h. After the heat treatment, an aging treatment is also included. The aging treatment temperature is 500° C., and the aging treatment time is 3 h.
[0124] The parameters of each region of the NdFeB magnets of Examples 1-3 and Comparative Examples 1-2 are listed in Tables 1-3 below. Figure 1 The change of Tb content from test line 1 to test line 4 is shown as Figure 3As shown. Test line 1 is parallel to the X-axis direction, and passes through the easy demagnetization area, transition area and non-easy demagnetization area, and overlaps with the long axis of the non-easy demagnetization area. Test line 2 is parallel to the X-axis direction, and passes through the easy demagnetization area, transition area and non-easy demagnetization area. Test line 3 is parallel to the X-axis direction, and passes through the easy demagnetization area and transition area. Test line 4 is parallel to the X-axis direction and passes through the easy demagnetization area. The element contents of the NdFeB substrates used in Examples 1-3 and Comparative Examples 1-2 are shown in Table 4.
[0125] The thickness of the NdFeB magnets of Examples 1-3 and Comparative Examples 1-2 is 3 mm. The shells of the main phase grains in the easy demagnetization zone and the transition zone both include an inner shell and an outer shell, and the main phase grains in the non-easy demagnetization zone only include an inner shell. The main phase and Re phase grain sizes and shells of each region of the NdFeB magnets of Examples 1-3 and Comparative Examples 1-2 are shown in Tables 5-6.
[0126] Table 1 Diffusion increments of Dy and Tb in each region of the NdFeB magnets obtained in Examples 1-3 and Comparative Examples 1-2
[0127]
[0128] Table 2 Diffusion increment of Dy and Tb at the interface of NdFeB magnets prepared in Examples 1-3 and Comparative Examples 1-2
[0129]
[0130] Table 3 Dimension ratios of each region of the NdFeB magnets obtained in Examples 1-3 and Comparative Examples 1-2
[0131]
[0132] Table 4 Mass concentration of each element in the NdFeB substrate of Examples 1-3 and Comparative Examples 1-2 (wt%)
[0133]
[0134] Table 5 Main phase and Re phase particle size and shell of NdFeB in each region of Example 1-3 and Comparative Example 1-2
[0135]
[0136] Table 6 Main phase particle size and shell conditions of each region of NdFeB in Examples 1-3 and Comparative Examples 1-2
[0137]
[0138] Effect Example
[0139] 1. Test objects: NdFeB magnets of Examples 1-3 and Comparative Examples 1-2;
[0140] 2. Test method:
[0141] 1. Coercive force test: Examples 1-3 and Comparative Examples 1-2 were prepared with samples of W2~3±0.1*L19±0.1*T4±0.1 mm in specification. Two samples were stacked for testing. A coil with size W3*L19~20*T2.7 mm was used in the permanent magnet precision measurement system NIM-62000 for room temperature testing (temperature ≤ 200°C).
[0142] 2. Demagnetization rate test: Use electromagnetic simulation software, model Ansys Workbench, input speed 13000rpm, then adjust its temperature to the corresponding temperature condition, collect the back electromotive force data of the motor under the same time and observe the change of magnetic steel cloud map to identify whether the magnetic steel has demagnetized. The calculation formula of demagnetization rate is: demagnetization rate = (high temperature back electromotive force - normal temperature back electromotive force) / normal temperature back electromotive force.
[0143] 3. Line scan test: The magnet surface of the selected area was microscopically photographed under the EMMA equipment. The equipment model was JEOL 8530f, and the shooting magnification was X3000. The two main phases were scanned by pulling wires to characterize the distribution of elements such as Dy / Nd.
[0144] 3. Test results: listed in the following table 7-8:
[0145] Table 7 Coercive force and anti-demagnetization ability of each region in the magnets of Examples 1-3 and Comparative Examples 1-2
[0146]
[0147] Table 8 Coercivity ratio of each region in the magnets of Examples 1-3 and Comparative Examples 1-2
[0148] Coercivity ratio of easy demagnetization region, transition region and non-easy demagnetization region Example 1 1:0.959:0.957 Example 2 1:0.930:0.909 Example 3 1:0.970:0.876 Comparative Example 1 1:0.945:0.936 Comparative Example 2 1:0.900:0.668
[0149] As can be seen from the above table, the demagnetization rate of the NdFeB magnets of Examples 1-3 at 130°C is only 2.0%-5.2%. The coercive force ratio of the transition zone and the easy demagnetization zone of the NdFeB magnets prepared in Examples 1-3 is between (0.93-0.97):1, and the coercive force difference between the easy demagnetization zone and the non-easy demagnetization zone is between 0.75-1.67kOe, which has excellent anti-demagnetization ability. Figure 1 The coercivity variation of test line 1 to test line 4 is shown in FIG. Figure 2 shown.
[0150] The Tb diffusion increment in the easily demagnetized zone of Comparative Example 1 is too low, and the increment ratio of Tb to Dy in the non-easy demagnetized zone is 3:11. The coercive force ratio of the easily demagnetized zone to the non-easy demagnetized zone of the NdFeB magnet in Comparative Example 1 is about 1:0.936, and the coercive force difference between the easily demagnetized zone and the non-easy demagnetized zone is 1.5kOe. The anti-demagnetization ability of the NdFeB magnet prepared in Comparative Example 1 is poor, and its demagnetization rate at 130°C is 20.2%, which is higher than that of Examples 1-3.
[0151] The Dy diffusion increment in the non-demagnetization zone of comparative example 2 is too low; while the Tb diffusion increment in the demagnetization zone is slightly higher (specifically 1wt%); the Tb diffusion increment in the transition zone is too low, and the ratio of the Tb diffusion increment in the demagnetization zone to the demagnetization zone is 1:5; the Dy diffusion weight gain in the transition zone and the non-demagnetization zone is ≤0.1wt%, and the coercive force ratio between the non-demagnetization zone and the demagnetization zone of the obtained NdFeB magnet is 0.668:1, and the coercive force difference between the demagnetization zone and the non-demagnetization zone is 8.7kOe. The anti-demagnetization ability of the NdFeB magnet obtained in comparative example 2 is poor, and its demagnetization rate at 130°C is as high as 19.6%, which is much higher than that of Examples 1-3, and the coercive force of the transition zone and the non-demagnetization zone is lower than that of the demagnetization under this condition.
[0152] The above-described embodiments are only preferred embodiments of the present invention, which are convenient for those skilled in the art to understand and use the present invention. Obviously, any person skilled in the art can slightly modify or change the present embodiment and apply it to other embodiments without creative work. Therefore, the present invention is not limited to the above-described embodiments, and any equal changes, simple modifications and modifications made within the scope of the present invention still belong to the scope of the present invention.
Claims
1. A neodymium iron boron magnet, characterized in that: Establishing a three-dimensional rectangular coordinate system with the orientation direction as the Z-axis direction, wherein the origin of the three-dimensional rectangular coordinate system is located inside the NdFeB magnet; The NdFeB magnet includes a non-demagnetization zone, a transition zone, and an easy demagnetization zone; the easy demagnetization zone is an outer annular area located along the Z-axis of the NdFeB magnet, and the non-demagnetization zone is a central area located along the Z-axis of the NdFeB magnet; the transition zone is a boundary area between the easy demagnetization zone and the non-demagnetization zone; The Tb content ratio of the non-demagnetization-prone region, the transition region, and the demagnetization-prone region is (0-0.05):(0.95-1):1; The Dy content ratio among the non-easily demagnetized region, the transition region, and the easily demagnetized region is 1:1:
1.
2. The NdFeB magnet according to claim 1, wherein The content of heavy rare earth at each position in the easily demagnetized region is the same; And / or, the diffusion increment of heavy rare earth at the same XY position in the transition region along the Z axis is the same; preferably, the diffusion content of Tb in the transition region along the X axis or Y axis and away from the easily demagnetized region decreases; And / or, the Tb content at any two locations with the same XY position in the easily demagnetized region is the same; And / or, the Dy contents at any two locations in the easily demagnetized region, the transition region, and the non-easily demagnetized region are the same; And / or, the Tb content ratio of the transition region to the easily demagnetized region is 0.8:1 or 0.9:1; And / or, the Tb content ratio of the transition region to the non-easily demagnetized region is 1:(0-0.1), preferably 1:(0-0.05); And / or, the Tb content ratio between the non-easily demagnetized region and the easily demagnetized region is (0-0.9):1, for example, 0.1:1, 0.2:1 or 0.7:1; And / or, the ratio of the diffusion increment of Tb in the easily demagnetized region to the diffusion increment of Tb in the non-easily demagnetized region is (1-100):1, for example, 9:1, 36:1 or 55:1; And / or, the ratio of the diffusion increment of Tb in the easy demagnetization zone to the diffusion increment of Tb in the transition zone is (1-1.1):1, for example, 1:1, 36:34 or 55:52; and / or, the diffusion increment of Tb in the easily demagnetized region is 0.1 wt%-1 wt%, for example, 0.35 wt%, 0.36 wt%, 0.45 wt% or 0.55 wt%; and / or, the diffusion increment of Tb in the non-demagnetizable region is 0-0.1 wt %, preferably 0-0.05 wt %, for example 0, 0.01 wt % or 0.05 wt %; and / or, the diffusion increment of Tb in the transition zone is 0.1 wt%-1 wt%, such as 0.34 wt%, 0.45 wt% or 0.52 wt%; and / or, the diffusion increment of Dy in the easily demagnetized region is 0.1 wt%-1 wt%, for example, 0.55 wt%; And / or, the diffusion increment of Dy in the non-demagnetizable region is 0.1wt%-1wt%, preferably 0.4wt%-0.7wt%, for example 0.55wt%; and / or, the diffusion increment of Dy in the transition zone is 0.1 wt%-1 wt%, for example 0.55 wt%; And / or, an interface A exists between the transition zone and the easily demagnetized zone, and the content of heavy rare earth at each position of the interface A is the same; the Tb diffusion increment at the interface A is preferably 0.3wt%-0.7wt%, for example, 0.36wt%, 0.45wt% or 0.55wt%; the Tb diffusion increment ratio between the interface A and the easily demagnetized zone is preferably (0.95-1):1; the Dy diffusion increment at the interface A is preferably 0.4wt%-0.7wt%, for example, 0.55wt%; And / or, an interface B exists between the transition zone and the non-easily demagnetized zone, and the content of heavy rare earth at each position of the interface B is the same; the Tb diffusion increment at the interface B is preferably 0.3wt%-0.7wt%, for example, 0.34wt%, 0.43wt% or 0.52wt%; the Tb diffusion increment ratio between the interface B and the non-easily demagnetized zone is preferably (6-60):1, for example, 43:5, 34:1 or 52:1; the Dy diffusion increment at the interface B is preferably 0.4wt%-0.7wt%, for example, 0.55wt%; and / or, a coercivity ratio of the easily demagnetized region to the non-easily demagnetized region is 1:(0.7-0.96), for example, 1:0.876, 1:0.909 or 1:0.957; and / or, a coercivity ratio of the easily demagnetized region to the transition region is 1:(0.93-1), for example, 1:0.930, 1:0.959 or 1:0.970; and / or, the coercive force at each position of the easily demagnetized region is the same; And / or, the coercive force at each position of the transition region along the Z-axis is the same; preferably, the coercive force in the transition region along the X-axis or the Y-axis and away from the easily demagnetized region decreases; and / or, the remanence at each position of the easily demagnetized region is the same; And / or, the remanence at each position of the transition zone along the Z-axis direction is the same; preferably, the remanence in the transition zone along the X-axis or the Y-axis and away from the easily demagnetized zone decreases.
3. The NdFeB magnet according to claim 1, wherein The NdFeB magnet is represented by the chemical formula R1-R2-TBM, wherein R1 is one or more of Pr, Nd, Ce, Er, Tm, Y, Lu, Gd and Ho; R2 is Dy and / or Tb; T is one or more of Fe, Zn, Si, V, Cr, Mn, Ni, Ge, Nb, Mo, Pd, Ag, Cd, Sb, Hf, Ta, W, O, C, N, S, F and P; M is one or more of Cu, Al, Co, Ga, Zr and Ti; preferably, all M elements are derived from the NdFeB substrate; preferably, the M elements include M elements introduced by diffusion, wherein the mass percentage of the M elements introduced by diffusion in the NdFeB magnet is preferably 0-0.4%; And / or, the microstructure of the NdFeB magnet includes Re2Fe 14 B main phase grains and Re-rich phase grain boundaries; the Re2Fe 14 The B main phase grains include a core layer and a shell layer; the Re is one or more of Nd, Dy and Tb.
4. The NdFeB magnet according to claim 3, wherein The Re2Fe 14 The difference in the grain size of the B main phase grains does not exceed 8μm; and / or, Re2Fe in the transition region 14 The difference in the grain size of the B main phase grains does not exceed 8μm; and / or, the Re2Fe 14 The grain sizes of the B main phase grains are equal; and / or, the Re2Fe in the center of the easily demagnetized region, the transition region and the non-easily demagnetized region 14 The grain sizes of the B main phase grains are equal; And / or, in the easily demagnetized region, the transition region and the non-easy demagnetized region, the surface layer of Re2Fe 14 The particle size of the B main phase grains is 1-1.5 times the particle size of the central main phase grains; And / or, the Re2Fe 14 The grain size ratio of the B main phase grains is 1:1:1; and / or, the Re2Fe 14 The particle size of the B main phase grains is 1-12 μm; and / or, the thicknesses of the Re-rich phase grain boundaries in the easily demagnetized regions are equal; and / or, the thicknesses of the Re-rich phase grain boundaries in the transition zone are equal; And / or, the thickness of the Re-rich phase grain boundary in the easily demagnetized region is 0.4-1 μm, for example, 0.5 μm or 0.55 μm; and / or, the thickness of the Re-rich phase grain boundary in the transition zone is 0.4-1 μm, for example, 0.5 μm or 0.52 μm; And / or, the thickness of the Re-rich phase grain boundary in the non-easily demagnetized region is 0.2-0.5 μm, for example, 0.20 μm, 0.23 μm or 0.25 μm.
5. The NdFeB magnet according to claim 3, wherein: The shell layer of the easily demagnetized region is (Nd, Dy, Tb)2Fe 14 B hard magnetic layer; And / or, the shell layer of the non-demagnetizable region is (Nd, Dy)2Fe 14 B hard magnetic layer; And / or, the core layer and the shell layer in the easily demagnetized region, the transition region, and the non-easily demagnetized region each independently meet the following conditions: the R1 content in the core layer is not less than the R1 content in the shell layer; the R2 content in the core layer is less than the R2 content in the shell layer; And / or, the R2 is Tb, and the content of R2 in the easily demagnetized region, the transition region and the non-easily demagnetized region satisfies the following condition: easily demagnetized region ≥ transition region > non-easily demagnetized region; And / or, R2 is Dy, and the content of R2 in the easily demagnetized region, the transition region and the non-easily demagnetized region satisfies the following condition: non-easily demagnetized region = transition region = easily demagnetized region; and / or, the thickness of the shell layers of the easily demagnetized regions are equal; and / or, the thickness of the shell layers of the transition region may be equal; and / or, the thickness of the shell layer of the easily demagnetized region is 2-3 μm, for example, 2 μm, 2.1 μm or 2.5 μm; and / or, the thickness of the shell layer of the main phase grains in the transition zone is 2-2.5 μm, for example, 2 μm or 2.38 μm; And / or, the thickness of the shell layer of the main phase grains in the non-easily demagnetized region is 0.5-2 μm, for example, 0.95 μm, 1.0 μm or 1.1 μm; and / or, the thickness ratio of the shell layer of the easily demagnetized region to the Re-rich phase grain boundary is (2-3):(0.4-1), for example, 4:1, 2.1:0.5 or 2.5:0.55; and / or, the thickness ratio of the shell layer and the Re-rich phase grain boundary in the transition zone is (2-2.5):(0.4-1), for example, 4:1 or 2.38:0.52; And / or, the thickness ratio of the shell layer of the main phase grains and the Re-rich phase grain boundary in the non-easily demagnetized region is (0.5-2):(0.2-0.5), for example, 1.1:0.25, 1.0:0.23 or 0.95:0.
20.
6. The NdFeB magnet according to claim 1, wherein The NdFeB magnet is a rectangular parallelepiped; the origin is preferably located at the center of the upper surface of the rectangular parallelepiped; the X-axis of the three-dimensional rectangular coordinate system is preferably parallel to a side of the upper surface; the ratio of the length to the width of the NdFeB magnet is preferably (2-5):1, more preferably (2.42-3.7):1, for example, 3:1, 3.65:1, or 39:10.7; And / or, the widths of the easily demagnetized regions are equal; preferably, the widths of the easily demagnetized regions are not greater than 5 mm, for example, 2-4 mm; And / or, on any plane perpendicular to the orientation direction, the shape of the non-easily demagnetized region is elliptical; the ratio of the major axis a to the minor axis b of the non-easily demagnetized region is preferably (2-15):1, for example, 17.5:3.35; And / or, the widths of the transition zones are equal; preferably, the width of the transition zones is 0-2 mm, not 0, for example 0.5 mm; And / or, the volume of the easily demagnetized region accounts for 50%-90% of the volume of the NdFeB magnet, for example, 47.85%; And / or, the volume of the transition zone accounts for 0-28.4% of the volume of the NdFeB magnet, for example, 8.04%; And / or, the volume of the non-demagnetizable region accounts for 15.7%-44.11% of the volume of the NdFeB magnet; And / or, the thickness of the NdFeB magnet is not greater than 5 mm, for example, 3 mm.
7. A method for preparing a neodymium iron boron magnet, characterized in that: The method comprises the following steps: applying diffusion sources on the upper surface and / or lower surface perpendicular to the Z-axis direction on a NdFeB substrate to carry out grain boundary diffusion parallel to the orientation direction; wherein, applying diffusion source Dy on the entire area of the upper surface and the lower surface, and applying diffusion source Tb on the outer edge annular area along the Z-axis direction to form an easily demagnetized area, a transition area and a non-easy demagnetized area.
8. The method for preparing a NdFeB magnet according to claim 7, wherein: The diffusion source is applied by coating; the coating method is preferably spraying or printing; the dewaxing temperature of the spraying is preferably 200-400°C; the dewaxing temperature of the printing is preferably 100-500°C; when the diffusion source is applied by coating, the diffusion source is preferably mixed with a solvent and a binder to form a slurry; the solvent is preferably water, alcohol, ketone or ester; the mass percentage of Dy or Tb in the diffusion source in the slurry is preferably 0.3%-1%; And / or, the diffusion source Dy satisfies any one of the following conditions ①-③: ① The diffusion source Dy is a simple substance of Dy; ② The diffusion source Dy is a Dy-M alloy, and M is preferably one or more of Cu, Al, Co, Ga, Zr and Ti; the mass percentage of M in the Dy-M alloy is preferably no more than 40%; ③ The diffusion source Dy is Dy hydride or Dy fluoride; And / or, the diffusion source Tb satisfies any one of the following conditions ①-③: ① The diffusion source Tb is Tb elemental; ② The diffusion source Tb is a Tb-M alloy, and M is preferably one or more of Cu, Al, Co, Ga, Zr and Ti; the mass percentage of M in the Tb-M alloy is preferably no more than 40%; ③ The diffusion source Tb is Tb hydride or Tb fluoride; And / or, the temperature of the grain boundary diffusion is 750-950° C., for example, 900° C.; And / or, the grain boundary diffusion time is 5-30 hours, for example 10 hours; And / or, an aging treatment is further included after the grain boundary diffusion; the temperature of the aging treatment is preferably 300-600° C., for example, 500° C.; the time of the aging treatment is preferably 1-10 h, for example, 3 h.
9. A NdFeB magnet prepared by the method for preparing a NdFeB magnet according to claim 7 or 8.
10. Use of the NdFeB magnet according to any one of claims 1 to 6 and 9 in magnetic steel.
Citation Information
Patent Citations
RFeB-based magnet and method for producing RFeB-based magnet
CN104517696A
Gradient neodymium iron boron magnet and manufacturing method thereof
CN108899190A
Gradient distribution neodymium-iron-boron magnet and preparation method thereof
CN111653407A
Neodymium iron boron material and preparation method thereof
CN112735717A
Preparation method of high-temperature-resistant neodymium iron boron magnet and high-temperature-resistant neodymium iron boron magnet
CN115440492A
Cited By
High-temperature-resistant neodymium-iron-boron magnet and preparation process thereof
CN120149005A
Neodymium-iron-boron magnet and preparation method thereof
CN120261096A