Hard carbon composite material and preparation method thereof, negative electrode material, sodium ion battery and electric equipment

Through the preparation of hard carbon composite materials, the combination of porous hard carbon matrix and tin-containing compounds, combined with the hard carbon coating layer, solves the energy density and cycle stability problems of hard carbon materials in sodium ion batteries, and achieves high embedding Sodium capacity and long cycle life effects.

CN118748244AActive Publication Date: 2024-10-08BYD CO LTD

Patent Information

Application Number
CN202410833903.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The application of hard carbon materials in sodium-ion batteries has inherent low specific capacity, prone to capillary adsorption and volume expansion problems, which limits its energy density and cycle stability.

Method used

A hard carbon composite material is used, including a porous hard carbon matrix and a tin-containing compound filled in it, plus a hard carbon coating layer. It is prepared through hydrothermal reaction and carbon coating treatment to form a carbon-tin inner layer material and a coating outer layer. Buffer volume expands and increases sodium/desodium capacity.

Benefits of technology

It achieves high embedded sodium capacity and long cycle life, while improving the problems of capillary adsorption and drying and dehydration, and improving the energy density and stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748244A_ABST
    Figure CN118748244A_ABST
Patent Text Reader

Abstract

The invention discloses a hard carbon composite material and a preparation method thereof, a negative electrode material, a sodium ion battery and electric equipment. The hard carbon composite material comprises a carbon tin inner layer material and a coating outer layer, the carbon tin inner layer material comprises a porous hard carbon matrix and a tin-containing compound filled in holes of the porous hard carbon matrix, and the coating outer layer is a hard carbon coating layer. The invention also discloses a preparation method of the material, and the hard carbon composite material prepared by the method effectively buffers the volume expansion of the negative electrode material, and improves the sodium intercalation / sodium removal capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sodium ion batteries, and in particular to a hard carbon composite material and a preparation method thereof, a negative electrode material, a sodium ion battery and electrical equipment. Background Art

[0002] At present, sodium-ion batteries are considered to be a highly cost-effective secondary ion battery system. The wide availability and low cost of sodium resources can greatly alleviate the cost anxiety caused by the shortage of lithium ore resources and the high price of lithium carbonate raw materials. Its research and development and industrialization progress have received widespread attention at home and abroad. As one of the negative electrode materials for sodium-ion batteries, hard carbon materials have good cycle stability and feasibility of industrial mass production. However, hard carbon materials also have certain application shortcomings: 1) Due to the low inherent specific capacity of hard carbon materials, which is often less than 300mAh / g, it greatly limits the improvement of the energy density of the whole battery; 2) Due to the presence of a large number of mesoporous micropores in hard carbon materials, the inherent properties of the porous structure make it very easy to produce capillary adsorption during storage and use, absorbing moisture in the environment, seriously affecting the production process stability and cycle stability of sodium-ion batteries.

[0003] Tin-based materials are a kind of electrode materials with great potential and are favored by researchers. Tin-based materials are less studied as negative electrode materials for sodium-ion batteries. They have high theoretical capacity but poor cycle stability, mainly because they have a large volume expansion problem during the charge and discharge process. Summary of the invention

[0004] Based on this, the present invention provides a hard carbon composite material and a preparation method thereof, a negative electrode material, a sodium ion battery and electrical equipment. The hard carbon composite material includes a carbon-tin inner layer material and a coating outer layer. The carbon-tin inner layer material includes a porous hard carbon matrix and a tin-containing compound filled in the pores of the porous hard carbon matrix. The coating outer layer is a hard carbon coating layer. The hard carbon composite material effectively buffers the volume expansion of the negative electrode material and improves the sodium insertion / de-sodiumization capacity and cycle performance.

[0005] In one embodiment, the particle size distribution of the porous hard carbon matrix is: 1um≤D50≤20um.

[0006] In one embodiment, the BET specific surface area of ​​the porous hard carbon matrix is ​​1-20 m 2 / g, the tap density of porous hard carbon matrix is ​​≥0.7g / cm 3 , the carbon content of the porous hard carbon matrix is ​​≥99.10%.

[0007] In one embodiment, the tin-containing compound includes one or more of SnO, Sn3P4 and SnS.

[0008] In one embodiment, the particle diameter of the tin-containing compound satisfies 5nm≤D50≤200nm.

[0009] In one embodiment, the mass proportion of the tin-containing compound is 1% to 2% based on the total mass of the hard carbon composite material.

[0010] In one embodiment, the thickness of the outer coating layer is 20 to 800 nm, and based on the total mass of the hard carbon composite material, the mass of the outer coating layer accounts for 0.5% to 1%.

[0011] The hard carbon composite material provided in the first aspect of the present invention has a high capacity, and the porous internal structure provides a fast transfer channel for the diffusion transfer of ions. At the same time, the porous carbon skeleton can serve as a buffer structure to alleviate the volume expansion during the charging and discharging process. The introduced tin-containing compound has a good theoretical capacity and can improve the capacity of the hard carbon-based material. The hard carbon composite material of the present invention can achieve a high sodium embedding capacity while achieving a longer cycle life.

[0012] In a second aspect, the present invention further provides a method for preparing a hard carbon composite material, characterized in that it comprises the following steps:

[0013] S1, performing a first carbonization treatment on the first carbon source and then pickling it;

[0014] S2, subjecting the acid-washed first carbon source and the activated pore-forming agent to an activation reaction;

[0015] S3, performing a second carbonization on the activated first carbon source to obtain a porous hard carbon matrix;

[0016] S4, subjecting the porous hard carbon matrix and the tin source to a hydrothermal reaction to obtain a carbon-tin inner layer material;

[0017] S5. Carry out carbon coating treatment on the carbon-tin inner layer material to obtain a hard carbon composite material.

[0018] In one embodiment, in step S1, the first carbon source includes biomass waste and coal, the biomass waste includes one or more of crop straw and crop husk, and the coal includes one or more of anthracite, bituminous coal and lignite.

[0019] In one embodiment, step S1 further includes coarsely crushing, washing and drying the first carbon source, and the particle size of the first carbon source after drying is 1 mm≤D50≤5 mm.

[0020] In one embodiment, the method for preparing the hard carbon composite material further comprises:

[0021] In step S1, the temperature of the first carbonization treatment is 300-600°C, the treatment time is 10-12 hours, and the pickling uses one or more of hydrochloric acid, sulfuric acid, and hydrofluoric acid, and the pickling temperature is 40-70°C;

[0022] In step S2, the activation reaction temperature is 600-1000° C., and the activation reaction time is 2-6 hours;

[0023] In step S3, the second carbonization temperature is 1000-1700° C., and the second carbonization time is 2-10 hours;

[0024] In step S4, the temperature of the hydrothermal reaction is 120-180° C., and the hydrothermal reaction time is 4-8 hours.

[0025] In one embodiment, in step S5, the carbon coating treatment step includes: mixing the carbon-tin inner layer material, the second carbon source and the first solvent, performing a third carbonization, grinding and screening to obtain a hard carbon composite material.

[0026] In one embodiment, in step S5, the third carbonization temperature is 1000-1300° C., and the third carbonization time is 3-5 hours.

[0027] The preparation method of the hard carbon composite material provided in the second aspect of the present invention has a simple process, uses a low-cost carbon source, has high repeatability, short cycle, low energy consumption, saves production costs, is suitable for large-scale production needs, and has good application prospects in the field of sodium ion batteries.

[0028] In a third aspect, the present invention provides a negative electrode material, comprising the hard carbon composite material provided in the first aspect of the present invention. The negative electrode material provided by the present invention has a small volume change during the cycle, a high cycle capacity and a long cycle life.

[0029] In a fourth aspect, the present invention provides a sodium ion battery, comprising the negative electrode material provided in the third aspect of the present invention. The sodium ion battery provided by the present invention has a high cycle capacity and a long cycle life.

[0030] In a fifth aspect, the present invention provides an electric device, which includes a sodium ion battery. Specifically, the electric device can be an electric car, an electric motorcycle, an electric bicycle, a mobile power supply, an unmanned aerial vehicle, a mobile phone, a computer, a camera, an electric tool, a smart home or a wearable device. The sodium ion battery has a long cycle life and a high capacity, so that the electric device can be used stably for a long time, which is conducive to improving the performance of the electric device. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the embodiments or the prior art description. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0032] Figure 1A schematic cross-sectional view of a hard carbon composite material provided in one embodiment of the present invention.

[0033] Figure 2 This is a scanning electron microscope image of the hard carbon material provided in Comparative Example 1 of the present invention.

[0034] Figure 3 This is a scanning electron microscope image of the hard carbon composite material provided in Example 1 of the present invention.

[0035] Figure 4 This is a TGA curve chart of the hard carbon composite material provided in Example 1.

[0036] Description of labels:

[0037] A porous hard carbon matrix-11, a tin-containing compound-12, and a coating outer layer-13. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.

[0040] Some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0041] The application of hard carbon materials in sodium-ion batteries has attracted increasing attention. Their high specific capacity can effectively improve the energy density of the battery, and their excellent cycle stability ensures the long-term use of the battery. At the same time, their good conductivity enhances the charging and discharging efficiency of the battery. In addition, hard carbon materials are relatively low in cost and have the potential for large-scale application.

[0042] However, despite the advantages of hard carbon materials in sodium-ion batteries, there are still many technical challenges and defects. For example, the preparation process of hard carbon materials is complicated and costly, and their electrochemical performance is affected by many factors such as preparation conditions, structural defects and surface properties, which limits their large-scale application in sodium-ion batteries. In addition, the volume expansion and contraction problems of hard carbon materials during charging and discharging also need to be solved to further improve their cycle stability and energy density.

[0043] Based on this, the present invention provides a hard carbon composite material, which includes a carbon-tin inner layer material and a coating outer layer, wherein the carbon-tin inner layer material includes a porous hard carbon matrix and a tin-containing compound filled in the pores of the porous hard carbon matrix, and the coating outer layer is a hard carbon coating layer. The introduced tin-containing compound has a good theoretical capacity, which can significantly improve the capacity of the hard carbon-based material; secondly, the tin-containing compound load is compounded with the porous hard carbon material, and the hard carbon material with a certain conductivity can provide a good electron transmission path, and the porous internal structure provides a fast transfer channel for the diffusion transfer of ions, and the porous carbon skeleton can be used as a buffer structure to alleviate the volume expansion of the tin-containing compound during the charge and discharge process, so as to achieve a high sodium embedding capacity and a long cycle life; finally, a layer of carbon material is coated on the surface of the porous hard carbon / tin-containing compound composite material. The carbon coating layer can block the open pore structure on the surface, reduce the area of ​​contact with the electrolyte, thereby improving the first coulomb efficiency, and can improve the problem of strong water absorption and difficulty in drying and dehydration caused by capillary adsorption of the hard carbon material itself.

[0044] In one embodiment, the particle size distribution of the porous hard carbon matrix is: 1um≤D50≤20um. Particle size distribution within this range helps to optimize the structure and performance of the electrode. Smaller particles can be more evenly dispersed in the electrode, increasing the contact area between the electrode and the electrolyte, thereby increasing the diffusion rate and reaction efficiency of sodium ions; secondly, smaller particles can shorten the transmission path of electrons in the electrode, reduce resistance, and thus improve the conductivity of the electrode. This helps to reduce the energy loss of the battery during the charging and discharging process and improve the efficiency and cycle life of the battery. Optionally, the particle size D50 of the porous hard carbon matrix can be 1um, 5um, 10um, 15um, 20um, 25um, 30um, 40um, 50um.

[0045] In one embodiment, the BET specific surface area of ​​the porous hard carbon matrix is ​​1-20 m 2 / g, powder tap density ≥0.7g / cm 3 The carbon content of the porous hard carbon matrix is ​​≥99.10%. The BET specific surface area is controlled within 1 to 20 m 2 / g helps to enhance the contact between the electrolyte and the electrode and improve the sodium ion reaction efficiency. Optionally, the BET specific surface area of ​​the porous hard carbon matrix can be 1m2 / g, 2m 2 / g, 4m 2 / g, 6m 2 / g, 8m 2 / g, 10m 2 / g, 12m 2 / g, 14m 2 / g, 16m 2 / g, 18m 2 / g, 20m 2 / g; tap density ≥0.7g / cm 3 This ensures that the materials are tightly stacked, improving electrode conductivity and energy density; at the same time, a carbon content of ≥99.10% ensures the high purity of the material, reduces side reactions, and improves battery cycle stability.

[0046] In one embodiment, the tin-containing compound includes one or more of SnO, Sn3P4 and SnS. These tin-containing compounds can significantly improve the electrochemical properties of hard carbon materials. Since they have a higher theoretical capacity, the storage capacity of sodium ion batteries can be increased after doping, thereby increasing the energy density of the battery. Secondly, tin-containing compounds have good sodium ion embedding and extraction capabilities during the charge and discharge process, which helps to improve the cycle stability and rate performance of the battery. After the hard carbon material is doped with these compounds, it can more effectively accommodate sodium ions, reduce the volume expansion and contraction of the material during the charge and discharge process, and extend the service life of the battery.

[0047] In one embodiment, the particle size diameter of the tin-containing compound satisfies 5nm≤D50≤200nm. The particle size diameter of the tin-containing compound within this range helps the tin-containing compound to be more evenly dispersed in the hard carbon material, reduces the local concentration difference in the material, and is conducive to the full mixing of the tin-containing compound with the hard carbon material and other components to form a uniform electrode structure, thereby improving the diffusion efficiency of sodium ions in the electrode, thereby enhancing the electrochemical performance of the battery. Optionally, the particle size diameter D50 of the tin-containing compound can be 5nm, 10nm, 20nm, 30nm, 50nm, 70nm, 90nm, 110nm, 130nm, 150nm, 170nm, 200nm.

[0048] In one embodiment, based on the total mass of the hard carbon composite material, the mass proportion of the tin-containing compound is 1% to 2%. In the present invention, the mass proportion of the tin-containing compound of 1% to 2% is conducive to the optimization and balance of material properties. At this time, the tin-containing compound can be evenly distributed in the hard carbon matrix and form a good synergistic effect with the hard carbon material. It can not only improve the conductivity and ion diffusion rate of the electrode, but also reduce the polarization phenomenon of the electrode during the charging and discharging process, and improve the power density and energy conversion efficiency of the battery. Optionally, based on the total mass of the hard carbon composite material, the mass proportion of the tin-containing compound can be 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%.

[0049] In one embodiment, the thickness of the outer coating layer is 20 to 800 nm, and the mass of the outer coating layer accounts for 0.5% to 1% based on the total mass of the hard carbon composite material. The thickness of the outer coating layer affects the electrochemical properties and physical stability of the hard carbon composite material. The thickness range of 20 to 800 nm can ensure that the coating layer is neither too thick to reduce the overall performance of the material, nor too thin to effectively protect the internal material. The appropriate thickness not only helps to improve the conductivity and ion diffusion rate of the electrode, but also prevents the structural damage of the hard carbon material during the charge and discharge process, thereby improving the cycle life and stability of the battery. Optionally, the thickness of the coating outer layer can be 20nm, 50nm, 1000nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm; secondly, the mass proportion of the coating outer layer of 0.5% to 1% can provide sufficient protection without affecting the main performance of the hard carbon composite material, improve the interface contact between the electrode and the electrolyte, and improve the embedding and extraction efficiency of sodium ions, thereby further improving the overall performance of the sodium ion battery. Optionally, based on the total mass of the hard carbon composite material, the mass proportion of the coating outer layer can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1.0%.

[0050] The hard carbon composite material provided by the present invention has a high capacity, and the porous internal structure provides a fast transfer channel for the diffusion transfer of ions. At the same time, the porous carbon skeleton can be used as a buffer structure to alleviate the volume expansion during the charge and discharge process, which can achieve a high sodium embedding capacity while achieving a long cycle life.

[0051] The present invention also provides a method for preparing a hard carbon composite material, which is characterized by comprising the following steps:

[0052] S1, performing a first carbonization treatment on the first carbon source and then pickling it;

[0053] S2, subjecting the acid-washed first carbon source and the activated pore-forming agent to an activation reaction;

[0054] S3, performing a second carbonization on the activated first carbon source to obtain a porous hard carbon matrix;

[0055] S4, subjecting the porous hard carbon matrix and the tin source to a hydrothermal reaction to obtain a carbon-tin inner layer material;

[0056] S5. Carry out carbon coating treatment on the carbon-tin inner layer material to obtain a hard carbon composite material.

[0057] The method provided by the present invention prepares a hard carbon composite material with excellent electrochemical properties through the steps of carbonization treatment, acid washing, activation pore formation, re-carbonization, introduction of tin source by hydrothermal reaction and final carbon coating treatment. The hard carbon composite material prepared by the present invention not only has high storage capacity and cycle stability, but also has good conductivity and ion diffusion performance, which provides strong support for the performance improvement and application expansion of sodium ion batteries.

[0058] In one embodiment, in step S1, the first carbon source includes biomass waste and coal, the biomass waste includes one or more of crop straw and crop shells, and the coal includes one or more of anthracite, bituminous coal and lignite. The utilization of biomass waste such as crop straw and crop shells not only realizes the recycling of resources, reduces environmental pollution, but also reduces production costs. These biomass wastes are rich in carbon elements and can be converted into carbon materials with good performance after carbonization treatment, providing a sustainable source of raw materials for the preparation of hard carbon composite materials. In addition, using biomass waste and coal as a composite carbon source can give full play to the advantages of both and realize the complementary performance of carbon materials. The porous structure and rich functional groups of biomass waste help to improve the specific surface area and electrochemical activity of hard carbon materials, while the high carbon content and stability of coal help to improve the conductivity and cycle stability of hard carbon materials.

[0059] In one embodiment, in step S1, the first carbon source is coarsely broken, cleaned, and dried, and the particle size of the first carbon source after coarse breaking is 1mm≤D50≤5mm. The coarse breaking process can break the original first carbon source into smaller particles, which helps the uniformity and efficiency of subsequent processing steps. Larger particles may cause uneven reactions, affecting the carbonization effect and the performance of the final product. The cleaning step can remove impurities and contaminants on the surface of the first carbon source. These impurities may affect the quality of carbonization, introduce unnecessary defects or reduce the purity of the material. The purity of the first carbon source can be ensured by cleaning, providing high-quality raw materials for subsequent steps. The drying step is to remove moisture from the first carbon source. Excessive moisture content may cause bubbles or cracks to form during the carbonization process, affecting the structure and performance of the carbon material. Therefore, drying can ensure that the first carbon source has a lower moisture content before carbonization. The particle size of the first carbon source after drying is controlled to be 1mm≤D50≤5mm in order to ensure that the first carbon source can have a suitable reaction speed and uniformity in the subsequent carbonization and other processing steps. Too large a particle size may lead to incomplete reaction, while too small a particle size may increase the preparation cost and processing difficulty. Therefore, by controlling the particle size range, the preparation efficiency can be improved and the cost can be reduced while ensuring the material performance. Optionally, the particle size D50 of the first carbon source after coarse crushing can be 1mm, 2mm, 3mm, 4mm, or 5mm.

[0060] In one embodiment, in step S1, the temperature of the first carbonization treatment is 300-600° C., and the first carbonization treatment time is 10-12 hours. The first carbonization can be carried out in a box furnace. Optionally, the first carbonization treatment temperature is in the temperature range of 300-600°C. At this time, the first carbon source can be gradually pyrolyzed and carbonized to form a carbon material with a certain degree of graphitization. This temperature range can not only ensure the progress of the carbonization reaction, but also avoid excessive graphitization or burning of the carbon material caused by excessive temperature, thereby maintaining its porous structure and high specific surface area. Optionally, the first carbonization temperature can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C; the first carbonization treatment time of 10-12 hours can ensure that the first carbon source is fully carbonized to form a stable carbon structure. At the same time, appropriate treatment time can also avoid structural damage or performance degradation of the carbon material caused by too long a time. Optionally, the first carbonization treatment time can be 10h, 10.5h, 11h, 11.5h, 12h.

[0061] In one embodiment, in step S1, pickling uses one or more of hydrochloric acid, sulfuric acid, and hydrofluoric acid, and the pickling temperature is 40-70°C. The main purpose of pickling is to remove impurities in the first carbon source, such as metal oxides, inorganic salts, etc., to improve the purity of the carbon material. Hydrochloric acid, sulfuric acid, and hydrofluoric acid are all strong acids that can effectively dissolve these impurities, thereby achieving deep cleaning of the carbon source. At the same time, their combined use can be flexibly adjusted according to the specific composition and impurity type of the carbon source to achieve the best cleaning effect. Secondly, the choice of pickling temperature has an important influence on the pickling effect. The temperature range of 40-70°C can ensure that the pickling reaction is carried out under relatively mild conditions, avoiding the destruction of the carbon material structure caused by excessively high temperatures or the acid volatilization too fast. At the same time, the appropriate temperature can also accelerate the pickling reaction rate and improve the pickling efficiency. Optionally, the pickling temperature can be 40°C, 50°C, 60°C, or 70°C.

[0062] In one embodiment, in step S2, the activation reaction temperature is 600-1000°C, and the activation reaction time is 2-6 hours. The activation method can be one of KOH activation, water vapor activation, and CO2 activation. The activation reaction temperature is within the temperature range of 600-1000°C, and the reaction between the activator and the carbon material can be fully carried out, thereby effectively introducing pores into the carbon material, while avoiding excessive ablation or structural damage of the carbon material caused by excessive temperature, and maintaining its stability and integrity. Optionally, the activation reaction temperature can be 600°C, 700°C, 800°C, 900°C, and 1000°C. Secondly, the activation reaction time within the range of 2-6 hours can promote the full reaction of the activator and the carbon material to form a uniform pore distribution. Optionally, the activation reaction time can be 2h, 3h, 4h, 5h, and 6h.

[0063] In one embodiment, in step S3, the second carbonization temperature is 1000-1700°C, and the second carbonization time is 2-10 hours. The carbonization temperature in the range of 1000-1700°C helps the non-carbon elements in the carbon source material to further escape, thereby improving the purity of the carbon material. At this time, the carbon source can fully carry out the graphitization reaction, so that the graphitization degree of the carbon material is moderate, which not only retains sufficient pore structure and specific surface area, but also improves the conductivity and structural stability of the material. Optionally, the second carbonization temperature can be 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C. At the same time, controlling the carbonization time between 2-10 hours can ensure the complete progress of the carbonization reaction and avoid excessive graphitization or structural damage of the carbon material. Optionally, the second carbonization time can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h.

[0064] In one embodiment, in step S4, the temperature of the hydrothermal reaction is 120-180°C, and the hydrothermal reaction time is 4-8 hours. The temperature of the hydrothermal reaction is within the temperature range of 120-180°C, and the tin source can be preferably dissolved or dispersed in the hydrothermal medium, and then interact with the hard carbon matrix, which can ensure the full dissolution or dispersion of the tin source, and avoid the volatilization of the tin source or the destruction of the hard carbon matrix structure caused by excessive temperature. Optionally, the temperature of the hydrothermal reaction can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C. At the same time, the reaction time of 4-8 hours of hydrothermal reaction can promote the tin source to fully diffuse and be evenly loaded on the hard carbon matrix, avoid the agglomeration of the tin source or the change of the hard carbon matrix structure, and form a stable carbon-tin inner layer structure. Optionally, the time of the hydrothermal reaction can be 4h, 5h, 6h, 7h, 8h.

[0065] In one embodiment, in step S5, the carbon coating treatment step includes: mixing the carbon-tin inner layer material, the second carbon source and the first solvent, and then performing a third carbonization, grinding, and screening to obtain a hard carbon composite material. In this embodiment, the mixture will be subjected to a third carbonization at a high temperature to convert the second carbon source into carbon and coat the surface of the carbon-tin inner layer material. After the carbonization is completed, the material is refined by grinding to increase its specific surface area and reaction activity, and then the oversized or undersized particles are removed by screening to ensure that the particle size distribution of the final product is uniform. Through a series of carbon coating treatment steps, a hard carbon composite material with excellent performance is obtained. This material not only has a high specific capacity and good cycle stability, but also has excellent conductivity and ion diffusion properties, providing an ideal electrode material for applications such as sodium ion batteries. In one embodiment of the present invention, the second carbon source is asphalt and the first solvent is petroleum ether.

[0066] The preparation method of the hard carbon composite material provided by the present invention has a simple process, uses a low-cost carbon source, has high repeatability, a short cycle, low energy consumption, saves production costs, is suitable for large-scale production needs, and has good application prospects in the field of sodium ion batteries.

[0067] The present invention provides a negative electrode material, comprising the hard carbon composite material provided by the first aspect of the present invention. The negative electrode material provided by the present invention has a small volume change during the cycle, a high cycle capacity and a long cycle life.

[0068] The present invention provides a sodium ion battery, comprising the negative electrode material provided by the third aspect of the present invention. The sodium ion battery provided by the present invention has high cycle capacity and long cycle life.

[0069] The present invention provides an electric device, which comprises a sodium ion battery. The sodium ion battery has a long cycle life and a high capacity, so that the electric device can be used stably for a long time, which is beneficial to improving the performance of the electric device.

[0070] The technical solution of the present invention is further illustrated below through specific embodiments and comparative examples.

[0071] Example 1

[0072] This embodiment provides a hard carbon composite material and a preparation method thereof, wherein the synthesis process comprises the following steps:

[0073] (1) The waste coconut shells were rinsed with deionized water for three times to remove the sludge and other impurities on the surface, and then dried in an oven at 120°C for 12 h;

[0074] (2) After drying, the coconut shell is roughly broken, and the sample particle size control range is: D50 = 2 mm;

[0075] (3) The coarsely crushed coconut shell samples were pre-carbonized at 450 °C for 10 h;

[0076] (4) Grinding the sample after the pre-carbonization treatment in the above step (3) in a jet mill to control the particle size of the output sample to: D50≈5um;

[0077] (5) The sample after the grinding treatment in the above step (4) is subjected to acid washing and purification, and the volume ratio of each component in the mixed acid used is hydrochloric acid: sulfuric acid: hydrofluoric acid = 7:2:1; the volume of the mixed acid used per 100g is 500ml, and the acid washing reaction temperature is 50°C. After the acid washing is completed, it is repeatedly washed with deionized water and then dried;

[0078] (6) subjecting the sample subjected to the acid-washing and purification treatment in step (5) to an activation reaction with an activation pore-forming agent KOH at a high temperature, the reaction temperature being 600° C. and the reaction time being 5 h;

[0079] (7) subjecting the sample activated in step (6) to a carbonization reaction at a high temperature of 1300° C. for 6 h; and obtaining a porous hard carbon skeleton material after natural cooling;

[0080] (8) 500 g of the porous hard carbon powder prepared in step (7) above was mixed with 10.86 g of SnCl2·2H2O, and then dispersed in deionized water. After sufficient stirring, the mixture was transferred to a polytetrafluoroethylene reactor and subjected to a hydrothermal reaction at 120°C for 6 hours. The product obtained after the reaction was completed was washed by centrifugation, filtered and dried to obtain a hard carbon / SnO composite material.

[0081] (9) Dissolve asphalt in petroleum ether, then add a certain amount of asphalt and stir until it is completely dissolved, then add the hard carbon / SnO composite material in the above step (8) to the petroleum ether solution dissolved with asphalt, continue stirring for 2 hours, and raise the temperature to 80°C until the petroleum ether is completely evaporated. Carbonize the asphalt-coated hard carbon / SnO composite material at 1000°C for 3 hours under a nitrogen atmosphere, and take it out after the temperature drops to room temperature.

[0082] Example 2

[0083] This embodiment provides a hard carbon composite material and a preparation method thereof, wherein the synthesis process comprises the following steps:

[0084] (1) The waste coconut shells were rinsed with deionized water for three times to remove the sludge and other impurities on the surface, and then dried in an oven at 120°C for 12 h;

[0085] (2) After drying, the coconut shell is roughly broken, and the sample particle size control range is: D50 = 2 mm;

[0086] (3) The coarsely crushed coconut shell samples were pre-carbonized at 450 °C for 11 h;

[0087] (4) Grinding the sample after the pre-carbonization treatment in the above step (3) in a jet mill to control the particle size of the output sample to: D50≈8um;

[0088] (5) The sample after the grinding treatment in the above step (4) is subjected to acid washing and purification, and the volume ratio of each component in the mixed acid used is hydrochloric acid: sulfuric acid: hydrofluoric acid = 7:2:1; the volume of the mixed acid used per 100g is 500ml, and the acid washing reaction temperature is 50°C. After the acid washing is completed, it is repeatedly washed with deionized water and then dried;

[0089] (6) subjecting the sample subjected to the acid-washing and purification treatment in step (5) to an activation reaction with an activation pore-forming agent KOH at a high temperature, the reaction temperature being 600° C. and the reaction time being 5 h;

[0090] (7) subjecting the sample activated in step (6) to a carbonization reaction at a high temperature of 1300° C. for 6 h; and obtaining a porous hard carbon skeleton material after natural cooling;

[0091] (8) 500 g of the porous hard carbon powder of step (7) above was mixed with 7.848 g of SnCl2·2H2O, and then dispersed in deionized water. After sufficient stirring, the mixture was transferred to a polytetrafluoroethylene reactor and subjected to a hydrothermal reaction at 120° C. for 6 hours. After the reaction was completed, the product was washed by centrifugation, filtered and dried to obtain a hard carbon / SnO composite material.

[0092] (9) Dissolve asphalt in petroleum ether, then add a certain amount of asphalt and stir until it is completely dissolved, then add the hard carbon / SnO composite material in the above step (8) to the petroleum ether solution dissolved with asphalt, continue stirring for 2 hours, and raise the temperature to 80°C until the petroleum ether is completely evaporated. Carbonize the asphalt-coated hard carbon / SnO composite material at 1000°C for 3 hours under a nitrogen atmosphere, and take it out after the temperature drops to room temperature.

[0093] Example 3

[0094] The difference from Example 1 is that the mass of SnCl2·2H2O in step (8) is 9.81 g, and the other steps are consistent with Example 1.

[0095] Example 4

[0096] The difference from Example 1 is that the mass of SnCl2·2H2O in step (8) is 13.08 g, and the other steps are consistent with Example 1.

[0097] Example 5

[0098] (Compared with Example 3, anthracite is used as the precursor raw material and steam is used as the activator)

[0099] In this embodiment, the carbon-coated and SnO-loaded co-modified porous hard carbon negative electrode material and its preparation method, the synthesis process of which comprises the following steps:

[0100] (1) Rinse the anthracite with deionized water three times to remove surface dirt and other impurities, and then dry it in an oven at 100°C for 24 hours;

[0101] (2) After drying, the anthracite is roughly crushed, and the sample particle size control range is: D50 = 1mm;

[0102] (3) Pre-carbonizing the coarsely crushed anthracite at 550°C for 3 hours;

[0103] (4) Grinding the sample after the pre-carbonization treatment in the above step (3) in a jet mill to control the particle size of the output sample to: D50≈5um;

[0104] (5) The sample after the grinding treatment in the above step (4) is subjected to acid washing and purification, and the volume ratio of each component in the mixed acid used is hydrochloric acid: sulfuric acid: hydrofluoric acid = 7:2:1; the volume of the mixed acid used per 100g is 600ml, and the acid washing reaction temperature is 60°C. After the acid washing is completed, it is repeatedly washed with deionized water and then dried;

[0105] (6) subjecting the sample subjected to the acid washing and purification treatment in step (5) to an activation reaction with high-temperature steam at a high temperature, the reaction temperature being 600° C. and the reaction time being 4 h;

[0106] (7) subjecting the sample activated in step (6) to a carbonization reaction at a high temperature of 1200° C. for 6 h; and obtaining a porous hard carbon skeleton material after natural cooling;

[0107] (8) The porous hard carbon powder of step (7) is mixed with SnCl2·2H2O, and then dispersed in deionized water. After being fully stirred, the mixture is transferred to a polytetrafluoroethylene reactor and subjected to a hydrothermal reaction at 120°C for 6 hours. After the reaction is completed, the product is washed by centrifugation, filtered and dried to obtain a hard carbon / SnO composite material.

[0108] (9) Dissolve asphalt in petroleum ether, then add a certain amount of asphalt and stir until it is completely dissolved, then add the hard carbon / SnO composite material in the above step (8) to the petroleum ether solution dissolved with asphalt, continue stirring for 2 hours, and raise the temperature to 80°C until the petroleum ether is completely evaporated. Carbonize the asphalt-coated hard carbon / SnO composite material at 1000°C for 3 hours under a nitrogen atmosphere, and take it out after the temperature drops to room temperature.

[0109] Example 6

[0110] (Compared with Example 3, lignite is used as the precursor raw material and CO2 is used as the activator)

[0111] In this embodiment, the carbon-coated and SnO-loaded co-modified porous hard carbon negative electrode material and its preparation method are characterized in that the synthesis process comprises the following steps:

[0112] (1) The lignite was rinsed with deionized water for three times to remove surface dirt and other impurities, and then dried in an oven at 85°C for 24 h;

[0113] (2) After drying, the lignite is roughly broken, and the sample particle size control range is: D50 = 1 mm;

[0114] (3) pre-carbonizing the coarsely crushed lignite at 550°C for 3 h;

[0115] (4) Grinding the sample after the pre-carbonization treatment in the above step (3) in a jet mill to control the particle size of the output sample to: D50≈5um;

[0116] (5) The sample after the grinding treatment in the above step (4) is subjected to acid washing and purification, and the volume ratio of each component in the mixed acid used is hydrochloric acid: sulfuric acid: hydrofluoric acid = 7:2:1; the volume of the mixed acid used per 100g is 600ml, and the acid washing reaction temperature is 60°C. After the acid washing is completed, it is repeatedly washed with deionized water and then dried;

[0117] (6) The sample after acid washing and purification in the above step (5) is activated with an activated pore-forming agent CO2 at a high temperature, the reaction temperature is 900° C., and the reaction time is 4 h;

[0118] (7) subjecting the sample activated in step (6) to a carbonization reaction at a high temperature of 1250° C. for 6 h; and obtaining a porous hard carbon skeleton material after natural cooling;

[0119] (8) The porous hard carbon powder of step (7) is mixed with SnCl2·2H2O, and then dispersed in deionized water. After being fully stirred, the mixture is transferred to a polytetrafluoroethylene reactor and subjected to a hydrothermal reaction at 120°C for 6 hours. After the reaction is completed, the product is washed by centrifugation, filtered and dried to obtain a hard carbon / SnO composite material.

[0120] (9) Dissolve asphalt in petroleum ether, then add a certain amount of asphalt and stir until it is completely dissolved, then add the hard carbon / SnO composite material in the above step (8) to the petroleum ether solution dissolved with asphalt, continue stirring for 2 hours, and raise the temperature to 80°C until the petroleum ether is completely evaporated. Carbonize the asphalt-coated hard carbon / SnO composite material at 1000°C for 3 hours under a nitrogen atmosphere, and take it out after the temperature drops to room temperature.

[0121] Comparative Example 1

[0122] Commercially available Japanese Kuraray hard carbon product Type-2. The specific surface area and particle size of the composite material prepared in this comparative example were tested, and its specific surface area was 4.5 m 2 / g, average particle size D50 = 5um.

[0123] Comparative Example 2

[0124] 39.84 g of SnCl2·2H2O was mixed and then dispersed in deionized water. After sufficient stirring, it was transferred to a polytetrafluoroethylene reactor and subjected to a hydrothermal reaction at a reaction temperature of 120°C for 6 hours. After the reaction was completed, the product was washed by centrifugation and filtered to obtain SnO material.

[0125] Test method:

[0126] (1) Electrochemical sodium storage performance test

[0127] The composite materials obtained in the embodiment and the comparative example were used as the negative electrode (the mass ratio of the materials in the formula was hard carbon composite material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR): conductive carbon black (SP) = 100: 1.5: 2.5: 1), the sodium sheet was used as the positive electrode, the electrolyte was NaPF6 / (PC+EMC) (the volume ratio of the electrolyte solvent PC: EMC = 1: 1), the diaphragm was a glass fiber diaphragm, and the button half-cell was assembled in a glove box filled with high-purity argon. The electrochemical performance was carried out on a Wuhan Blue Electric CT2001A battery tester, the charge and discharge voltage range was controlled at 0-2V, the charge and discharge rate was 0.1C, the first-cycle sodium insertion capacity and sodium removal capacity and the number of cycles were recorded (the sodium removal capacity decayed to 80% of the first-cycle sodium removal capacity), and the first-cycle coulomb efficiency was calculated (first-cycle coulomb efficiency = first-cycle sodium removal capacity / first-cycle sodium insertion capacity).

[0128] (2) Specific surface area test

[0129] According to the provisions of GB / T 19587, the specific surface area of ​​the material was measured using a Quantachrome NOVA2000e specific surface area analyzer.

[0130] (3) Particle size test

[0131] According to Appendix A of GB / T 24533-2019, the particle size of the material was detected using a Malvern laser particle size analyzer.

[0132] (4) TGA thermogravimetric test

[0133] Use a special crucible to weigh a small amount of powder sample, record its mass and place it in a thermogravimetric analyzer. Perform a heating test in an air atmosphere at a heating rate of 5°C / min. The temperature range is from room temperature to 900°C. The remaining mass percentage is the mass percentage of SnO.

[0134] (5) TEM test

[0135] A small amount of sample was ultrasonically dispersed in anhydrous ethanol, and then a small amount was taken with a pipette and dropped onto a carbon film or microgrid. After natural drying, the test was performed. The instruments used were Hitachi-7650 (Japan, 80 kV), and HRTEM, JEOL JEM-3000F.

[0136] Table 1 Hard carbon composite material components and preparation, battery test results

[0137]

[0138] By comparing Examples 1-6 with Comparative Example 1, it can be found that after activation and SnO composite, the capacity is significantly improved. Thanks to the activation pore formation providing more active sites, SnO as an active material and porous hard carbon composite provides more capacity. The battery cycle stability of Comparative Example 2 using only SnO as the negative electrode material is poor. At the same time, in Examples 1-6, the first coulomb efficiency is also improved to a certain extent, which is mainly due to the optimization of the surface structure of the coating layer, which reduces the contact area with the electrolyte. Furthermore, when the SnO content further meets the range of 1 to 2% in the present invention, the sodium ion battery containing this hard carbon composite material has high capacity, high first-cycle coulomb efficiency and long cycle life.

[0139] The above are preferred embodiments of the present application, but they should not be construed as limiting the scope of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. A hard carbon composite material, characterized in that: It comprises a carbon-tin inner layer material and a coating outer layer, wherein the carbon-tin inner layer material comprises a porous hard carbon matrix and a tin-containing compound filled in the pores of the porous hard carbon matrix, and the coating outer layer is a hard carbon coating layer.

2. The hard carbon composite material according to claim 1, characterized in that The particle size diameter of the porous hard carbon matrix is: 1um≤D50≤20um.

3. The hard carbon composite material according to claim 1, characterized in that The BET specific surface area of ​​the porous hard carbon matrix is ​​1-20 m 2 / g, the powder tap density of the porous hard carbon matrix is ​​≥0.7g / cm 3 , the carbon content of the porous hard carbon matrix is ​​≥99.10%.

4. The hard carbon composite material according to claim 1, characterized in that The tin-containing compound includes one or more of SnO, Sn3P4 and SnS.

5. The hard carbon composite material according to claim 1 or 4, characterized in that: The particle diameter of the tin-containing compound satisfies 5nm≤D50≤200nm.

6. The hard carbon composite material according to claim 1, characterized in that Based on the total mass of the hard carbon composite material, the mass proportion of the tin-containing compound is 1% to 2%.

7. The hard carbon composite material according to claim 1, characterized in that The thickness of the outer coating layer is 20 to 800 nm, and based on the total mass of the hard carbon composite material, the mass proportion of the outer coating layer is 0.5% to 1%.

8. A method for preparing a hard carbon composite material, characterized in that: The following steps are involved: S1, performing a first carbonization treatment on the first carbon source and then pickling it; S2, subjecting the acid-washed first carbon source and the activated pore-forming agent to an activation reaction; S3, performing a second carbonization on the activated first carbon source to obtain a porous hard carbon matrix; S4, subjecting the porous hard carbon matrix and the tin source to a hydrothermal reaction to obtain a carbon-tin inner layer material; S5. Carry out carbon coating treatment on the carbon-tin inner layer material to obtain a hard carbon composite material.

9. The method for preparing a hard carbon composite material according to claim 8, characterized in that: In step S1, the first carbon source includes biomass waste and coal, the biomass waste includes one or more of crop straw and crop husk, and the coal includes one or more of anthracite, bituminous coal and lignite.

10. The method for preparing a hard carbon composite material according to claim 8, characterized in that: Step S1 further includes coarsely crushing, washing and drying the first carbon source, wherein the particle size of the first carbon source after coarsely crushing is 1 mm≤D50≤5 mm.

11. The method for preparing a hard carbon composite material according to claim 8, characterized in that: include: In step S1, the temperature of the first carbonization treatment is 300-600°C, the treatment time is 10-12 hours, the pickling uses one or more of hydrochloric acid, sulfuric acid, and hydrofluoric acid, and the pickling temperature is 40-70°C; In step S2, the activation reaction temperature is 600-1000° C., and the activation reaction time is 2-6 hours; In step S3, the second carbonization temperature is 1000-1700° C., and the second carbonization time is 2-10 hours; In step S4, the temperature of the hydrothermal reaction is 120-180° C., and the hydrothermal reaction time is 4-8 hours.

12. The method for preparing a hard carbon composite material according to claim 8, characterized in that: In step S5, the carbon coating treatment step includes: mixing the carbon-tin inner layer material, the second carbon source and the first solvent, performing a third carbonization, grinding and screening to obtain the hard carbon composite material.

13. The method for preparing a hard carbon composite material according to claim 12, characterized in that: In step S5, the third carbonization temperature is 1000-1300° C., and the third carbonization time is 3-5 hours.

14. A negative electrode material, characterized in that: The negative electrode material includes the hard carbon composite material as described in any one of claims 1 to 7 or the hard carbon composite material prepared by the preparation method of the hard carbon composite material as described in any one of claims 8 to 13.

15. A sodium ion battery, characterized in that: The sodium ion battery comprises the negative electrode material as claimed in claim 14.

16. An electrical equipment, characterized in that: The electrical equipment comprises the negative electrode material according to claim 14 or the sodium ion battery according to claim 15.

Citation Information

Patent Citations

  • Negative electrode material, negative electrode and preparation method of negative electrode

    CN110556517A

  • Composite hard carbon material and preparation method and application thereof

    CN115911320A

  • Porous hard carbon negative electrode material and preparation method and application thereof

    CN116404128A

  • Tin-carbon sodium ion battery negative electrode material as well as preparation method and application thereof

    CN116706019A

  • Hard carbon composite material and preparation method and application thereof

    CN116960294A

Cited By

  • Preparation method of sodium ion battery hard carbon negative electrode material

    CN120398026A