Method for producing bisphenol, method for producing regenerated polycarbonate resin, method for producing epoxy resin, method for producing cured epoxy resin, and method for producing bisphenol-alkyl carbonate condensate

By using a catalyst system of dialkyl carbonate and aliphatic monohydric alcohols, polycarbonate resin is decomposed under mild conditions to produce bisphenol with good color, which solves the problems of high temperature and high pressure and complex operation in the existing technology, and realizes efficient industrial production and recycling of polycarbonate resin.

CN118748990APending Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380022650.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-29
Filing Date
2023-02-22
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing methods for decomposing polycarbonate resins require high temperature and high pressure conditions or are complicated to operate, and the catalyst is difficult to remove, resulting in low reaction efficiency and complicated purification steps, making them unsuitable for industrial production, especially for optical materials where high color tone requirements are required.

Method used

Dialkyl carbonate and aliphatic monohydric alcohols are used as catalysts to decompose polycarbonate resin under mild conditions. Alkali metal hydroxides, alkali metal carbonates and other catalysts are used to generate bisphenol through alcoholysis reaction, and the polycarbonate resin and epoxy resin are recovered and regenerated.

Benefits of technology

It achieves efficient decomposition of polycarbonate resin under mild conditions to generate bisphenol with good color, simplifies the operation process, is suitable for industrial production, and improves the quality of recycled polycarbonate resin and epoxy resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000577670000041
    Figure BDA0005000577670000041
  • Figure BDA0005000577670000042
    Figure BDA0005000577670000042
  • Figure BDA0005000577670000061
    Figure BDA0005000577670000061
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for producing a bisphenol by decomposing a polycarbonate resin with high reactivity even under mild and low environmental load conditions using a highly versatile catalyst. A method for producing a bisphenol, in which a decomposition reaction of a polycarbonate resin is performed in a reaction solution containing the polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol, and a catalyst, the molar ratio of the dialkyl carbonate used in the decomposition reaction to 1 mol of a bisphenol-derived repeating unit in the polycarbonate resin used in the decomposition reaction is 1.8 or more; the catalyst is any one selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal alkoxides, alkali metal oxides, chain alkylamines, and pyridines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing bisphenol and a method for producing a bisphenol-alkyl carbonate condensate. Specifically, it relates to a method for producing bisphenol and a method for producing a bisphenol-alkyl carbonate condensate by decomposing a polycarbonate resin. It also relates to a method for producing a recycled polycarbonate resin and a method for producing an epoxy resin using the bisphenol obtained by the bisphenol production method. It also relates to a method for producing a cured epoxy resin using the epoxy resin obtained by the epoxy resin production method. Background Art

[0002] Plastics are produced in large quantities not only in Japan but also around the world because they are simple, durable, and cheap. Most of these plastics are used in a "disposable" manner, so there are cases where they are not properly handled and flow into the environment. Specifically, plastic waste flows into the ocean from rivers, and in the process it is degraded by waves and ultraviolet rays to less than 5 mm. This small plastic waste is called microplastics. Animals and fish may accidentally eat these microplastics. In this way, plastic waste has a great impact on the ecosystem, and in recent years, it has been regarded as a problem worldwide as a marine plastic problem. Polycarbonate resins are used in a wide range of fields due to their transparency, mechanical properties, flame retardancy, dimensional stability, and electrical properties, and this polycarbonate resin is no exception.

[0003] One of the methods for recycling polycarbonate resins is chemical recycling in which the polycarbonate resins are chemically decomposed and returned to bisphenol for recycling. Alcoholysis is known as one of the methods for decomposing polycarbonate resins.

[0004] For example, Patent Document 1 discloses a method in which an aromatic polycarbonate dissolved in a monohydroxy compound other than methanol is contact-esterified with methanol in a distillation column to continuously ring-open the aromatic polycarbonate into a dihydroxy compound and dimethyl carbonate.

[0005] In addition, Patent Document 2 discloses a method for recovering useful materials from waste plastics, comprising: adding a specific tertiary amine as a catalyst to a solution containing waste plastics and monohydric alcohols or monohydric phenols to chemically decompose the polycarbonate resin in the waste plastics; and recovering the decomposition products as useful materials.

[0006] Non-patent document 1 discloses a method of obtaining bisphenol A as a reaction liquid by metathesis of a polycarbonate resin using a guanidine derivative or an amidine derivative as a catalyst. Non-patent document 2 discloses methanolysis of a polycarbonate resin using methyl carbonate (tetramethylammonium) as a catalyst.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 6-340591

[0010] Patent Document 2: Japanese Patent Application Publication No. 2004-51620

[0011] Non-patent literature

[0012] Non-patent literature 1: Polymer, 2018, vol143, p106-114

[0013] Non-patent document 2: Green Chemistry, 2020, vol22, Issue12, p3721-3726. Summary of the invention

[0014] Problems to be solved by the invention

[0015] In the decomposition method of polycarbonate resin by alcoholysis, aliphatic monohydric alcohol is generally used. However, in order to dissolve the polycarbonate resin and to increase the decomposition rate, it is necessary to carry out the reaction under high decomposition temperature and high pressure conditions, and since aliphatic monohydric alcohol with a small number of carbon atoms has a low boiling point, a pressure-resistant container is required.

[0016] In addition, according to Example 1 of Patent Document 1, a polycarbonate resin is dissolved in phenol at 150° C. and decomposed by convection contact with vapor composed of methanol and dimethyl carbonate. However, since this is carried out at normal pressure, there are problems such as complicated control of the apparatus and difficulty in controlling the decomposition of the polycarbonate resin.

[0017] In the method of Patent Document 2, amines are used as solvents and catalysts because polycarbonate resins are difficult to dissolve in methanol. However, when the amount of amine is small, there are problems such as low reactivity and prolonged reaction time.

[0018] Furthermore, the method of non-patent document 1 uses guanidine derivatives and amidine derivatives as catalysts to decompose polycarbonate resin. These guanidine derivatives and amidine derivatives have high affinity with oil and water, so they cannot be easily removed by water washing. In addition, these compounds have a boiling point of more than 150°C, which is relatively high, so they are not easy to distill off. Furthermore, these compounds are colored light yellow, so column chromatography purification and extraction with diethyl ether with a low flash point are required for purification. Therefore, in order to obtain bisphenol A from polycarbonate resin, complicated steps are required, so there is a problem of being unsuitable for industry.

[0019] The method of Non-Patent Document 2 also requires the use of a special catalyst, and like the method of Non-Patent Document 1, complicated steps are required to obtain bisphenol A from a polycarbonate resin, thus causing a problem of being unsuitable for industrial use.

[0020] Any of the above-mentioned methods for decomposing polycarbonate resins using aliphatic monohydric alcohols requires high temperature and high pressure decomposition conditions, or lacks reactivity, or the operation is complicated, and further improvement is required.

[0021] Bisphenol A is also used as a raw material for optical materials such as optical polycarbonate resins. Optical materials are required to have excellent color tone (transparency), and therefore bisphenol A as a raw material thereof is also required to have excellent color tone.

[0022] The present invention has been made in view of such circumstances, and its object is to provide a method for producing bisphenol, which produces bisphenol with good color tone by using a decomposition method, wherein the decomposition method uses a highly versatile catalyst and can decompose polycarbonate resin with high reactivity even under mild conditions with low environmental load. Furthermore, the object is to provide a method for producing a recycled polycarbonate resin and an epoxy resin using the obtained bisphenol. In addition, the object is to provide a method for producing an epoxy resin cured product using the epoxy resin obtained by the epoxy resin production method.

[0023] Another object of the present invention is to provide a method for producing a bisphenol-alkyl carbonate condensate, which method comprises producing a bisphenol-alkyl carbonate condensate by using a decomposition method for decomposing the polycarbonate resin.

[0024] Means for solving problems

[0025] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result, have discovered a decomposition method for decomposing a polycarbonate resin using a general catalyst, a dialkyl carbonate and an aliphatic monohydric alcohol. In addition, a method for producing bisphenol using the polycarbonate resin decomposition method has been discovered. Furthermore, a method for producing a regenerated polycarbonate resin and an epoxy resin using the obtained bisphenol has been discovered. In addition, a method for producing an epoxy resin cured product using the epoxy resin obtained by the epoxy resin production method has been discovered.

[0026] In addition, a method for producing a bisphenol-alkyl carbonate condensate has been discovered.

[0027] That is, the present invention relates to the following inventions.

[0028] <1> A method for producing bisphenol, comprising performing a decomposition reaction of a polycarbonate resin in a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst, wherein the molar ratio of the dialkyl carbonate used in the decomposition reaction to 1 mol of a repeating unit derived from bisphenol in the polycarbonate resin used in the decomposition reaction is 1.8 or more, and the catalyst is any one selected from the group consisting of an alkali metal hydroxide, an alkali metal carbonate, an alkali metal alkoxide, an alkali metal oxide, a chain alkylamine and pyridine.

[0029] <2> According to the above <1> In the method for producing bisphenol, the reaction liquid is in a slurry state.

[0030] <3> According to the above <1> or <2> In the method for producing bisphenol, the dialkyl carbonate includes dialkyl carbonate not derived from the polycarbonate resin.

[0031] <4> According to the above <1> to <3> The method for producing bisphenol according to any one of the above aspects, wherein the reaction liquid is prepared by mixing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol, and the catalyst.

[0032] <5> According to the above <1> to <4> The method for producing bisphenol according to any one of the preceding claims, wherein the alkali metal hydroxide is sodium hydroxide or potassium hydroxide, the alkali metal carbonate is sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate, the alkali metal alkoxide is sodium phenolate or sodium methoxide, and the alkali metal oxide is sodium oxide or potassium oxide.

[0033] <6> According to the above <1> to <5> The method for producing bisphenol according to any one of the preceding claims, wherein the chain alkylamine is represented by the following formula (I) or the following formula (II),

[0034] [Chemistry 1]

[0035]

[0036] In formula (I), R A represents an alkyl group having 1 to 3 carbon atoms, R B ~R C Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms,

[0037] [Chemistry 2]

[0038]

[0039] In formula (II), R D ~R G Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and m represents an integer of 1 to 6.

[0040] <7> According to the above <1> to <6> The method for producing bisphenol according to any one of the above, wherein the dialkyl carbonate is dimethyl carbonate, diethyl carbonate or dibutyl carbonate.

[0041] <8> According to the above <1> to <7> The method for producing bisphenol according to any one of the preceding claims, wherein the bisphenol is 2,2-bis(4-hydroxyphenyl)propane.

[0042] <9> According to the above <1> to <8> The method for producing bisphenol according to any one of the preceding claims, wherein the aliphatic monohydric alcohol is methanol, ethanol or butanol.

[0043] <10> According to the above <1> to <9> The method for producing bisphenol according to any one of the preceding claims comprises the following steps A, B1 and C1,

[0044] Step A: a step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a non-slurry polycarbonate decomposition solution containing bisphenol,

[0045] Step B1: a step of concentrating the polycarbonate decomposition liquid obtained in the step A to obtain a concentrated liquid,

[0046] Step C1: A step of supplying an aromatic hydrocarbon to the concentrated liquid obtained in the step B1 to precipitate bisphenol by crystallization to obtain a slurry containing bisphenol, and subjecting the obtained slurry to solid-liquid separation to obtain bisphenol.

[0047] <11> According to the above <1> to <9> The method for producing bisphenol according to any one of the preceding claims comprises the following steps A, B2 and C2,

[0048] Step A: a step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a non-slurry polycarbonate decomposition solution containing bisphenol,

[0049] Step B2: a step of removing the dialkyl carbonate and the aliphatic monohydric alcohol from the solution containing the polycarbonate decomposition liquid obtained in the step A and the aromatic monohydric alcohol to obtain a solution containing bisphenol and the aromatic monohydric alcohol,

[0050] Step C2: a step of recovering bisphenol from the solution containing bisphenol and aromatic monohydric alcohol obtained in the step B2.

[0051] <12> According to the above <1> to <10> The method for producing bisphenol according to any one of the preceding claims, comprising a first decomposition step and a second decomposition step,

[0052] A first decomposition step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a first decomposition solution containing bisphenol;

[0053] a second decomposition step of mixing the first decomposition liquid with water to hydrolyze the dialkyl carbonate, regenerate the aliphatic monohydric alcohol, and decompose the polycarbonate resin to generate bisphenol;

[0054] The first decomposition step and the second decomposition step are performed continuously.

[0055] <13> According to the above <12> In the method for producing bisphenol, the amount of water mixed with the first decomposition liquid is 0.5 mol or more and 1.5 mol or less per 1 mol of the repeating unit derived from bisphenol in the polycarbonate resin used in the decomposition reaction.

[0056] <14> According to the above <12> or <13> In the bisphenol production method, the aliphatic monohydric alcohol regenerated in the second decomposition step is separated from the bisphenol in the form of a mixture with the dialkyl carbonate, and the mixture of the aliphatic monohydric alcohol and the dialkyl carbonate is reused in the first decomposition step.

[0057] <15> According to the above <12> to <14> The method for producing bisphenol according to any one of the above aspects, wherein the reaction liquid is in a slurry state, and the first decomposition liquid is not in a slurry state.

[0058] <16> According to the above <1> to <10> The method for producing bisphenol according to any one of the preceding claims, wherein the bisphenol-alkyl carbonate condensate represented by the following formula (III) produced as a by-product during the decomposition of the polycarbonate resin is further recovered.

[0059] [Chemistry 3]

[0060]

[0061] In formula (III), R is methyl, ethyl or butyl.

[0062] <17> According to the above <16> The method for producing bisphenol, wherein in the formula (III), R is a methyl group.

[0063] <18> A method for producing recycled polycarbonate resin, comprising: <1> to <17> After obtaining bisphenol by the method for producing bisphenol described in any one of the above, a recycled polycarbonate resin is produced using a bisphenol raw material containing the bisphenol.

[0064] <19> A method for producing epoxy resin, comprising: <1> to <17> After obtaining bisphenol by the method for producing bisphenol described in any one of the above, an epoxy resin is produced using a polyhydroxy compound raw material containing the bisphenol.

[0065] <20> A method for producing epoxy resin, comprising: <19> After obtaining the epoxy resin, the epoxy resin manufacturing method further reacts the epoxy resin raw material containing the epoxy resin with a polyhydroxy compound raw material to manufacture the epoxy resin.

[0066] <21> A method for producing epoxy resin cured product, comprising: <19> or <20> The epoxy resin is obtained by the epoxy resin production method, and an epoxy resin composition containing the epoxy resin and a curing agent is obtained, and then the epoxy resin composition is cured to obtain an epoxy resin cured product.

[0067] <22> A method for producing a bisphenol-alkyl carbonate condensate, which comprises decomposing a polycarbonate resin in a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst, wherein the catalyst is any one selected from the group consisting of an alkali metal hydroxide, an alkali metal carbonate, an alkali metal alkoxide, an alkali metal oxide, a chain alkylamine and pyridine.

[0068] [Chemistry 4]

[0069]

[0070] In formula (III), R is methyl, ethyl or butyl.

[0071] Effects of the Invention

[0072] According to the present invention, there is provided a method for producing bisphenol, which uses a decomposition method that can decompose polycarbonate resin with high reactivity using a general-purpose catalyst even under mild conditions with low environmental load. According to the method for producing bisphenol of the present invention, bisphenol with good color tone can be obtained.

[0073] Furthermore, a method for producing a recycled polycarbonate resin and a method for producing an epoxy resin using the obtained bisphenol are provided.

[0074] In addition, a method for producing a bisphenol-alkyl carbonate condensate is provided, wherein the method comprises producing a bisphenol-alkyl carbonate condensate by decomposing the polycarbonate resin. DETAILED DESCRIPTION

[0075] The following is a detailed description of the embodiments of the present invention, but the description of the constituent elements described below is an example of the embodiments of the present invention, and the present invention is not limited to the following description as long as it does not exceed its main purpose. It should be noted that when the expression "to" is used in this specification, it is used as an expression containing the numerical values ​​or physical property values ​​before and after it.

[0076] <Bisphenol Production Method>

[0077] The present invention relates to a method for producing bisphenol (hereinafter sometimes described as "the method for producing bisphenol of the present invention"), which is a method for producing bisphenol in which a decomposition reaction of a polycarbonate resin is carried out in a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst, wherein the catalyst is any one selected from the group consisting of an alkali metal hydroxide, an alkali metal carbonate, an alkali metal alkoxide, an alkali metal oxide, a chain alkylamine and pyridine.

[0078] The bisphenol production method of the present invention is to decompose a polycarbonate resin in the presence of a dialkyl carbonate, an aliphatic monohydric alcohol and a specific catalyst. By using a dialkyl carbonate and an aliphatic alcohol in combination, the dialkyl carbonate swells the polycarbonate resin, and the contact area with the aliphatic monohydric alcohol increases, thereby accelerating the dissolution rate and the decomposition rate, so it is believed that the polycarbonate resin is easily decomposed even under mild conditions.

[0079] In addition, in the bisphenol production method of the present invention, the molar ratio of the dialkyl carbonate used in the decomposition reaction to 1 mol of the repeating unit derived from bisphenol of the polycarbonate resin used in the decomposition reaction (i.e., the input molar ratio) is 1.8 or more. As described later, the dissolution rate and decomposition rate of the polycarbonate resin are not reduced, and the reaction can be carried out efficiently.

[0080] In addition, the dispersibility of polycarbonate resin in dialkyl carbonate is very good. By using dialkyl carbonate, polycarbonate resin can be simply crushed, micronized and dispersed while swelling. The dispersed polycarbonate resin slowly dissolves in dialkyl carbonate and is decomposed. Compared with the solvent in which the polycarbonate resin remains in a block state, the decomposition reaction of dialkyl carbonate at the solid-liquid interface is easy to proceed. Therefore, the bisphenol manufacturing method of the present invention preferably prepares a slurry-like reaction solution in which polycarbonate resin is dispersed, and decomposes the polycarbonate resin in the slurry-like reaction solution.

[0081] By decomposing the polycarbonate resin in a slurry-like reaction solution, only the polycarbonate resin dissolved in an amount corresponding to the solubility will participate in the decomposition reaction, so it is easy to control the reaction and the polycarbonate resin can be stably decomposed. Moreover, as the decomposition reaction proceeds, the polycarbonate resin is completely dissolved, and in the reaction solution (decomposition solution) at the end of the decomposition reaction, the slurry state in which the polycarbonate resin is dispersed disappears, and the generated bisphenol is dissolved in a non-slurry-like liquid. It should be noted that in the present application, as the range of the slurry state at the beginning of the decomposition of polycarbonate, it is preferred to use a filter with a pore size of 1 mm or less to filter the reaction solution, and the solid concentration of the polycarbonate resin filtered out is 5% by mass or more relative to the reaction solution. In addition, as the range of the non-slurry state at the end of the decomposition reaction, it is preferred to use a filter with a pore size of 1 mm or less to filter the decomposition solution, and the solid concentration of the polycarbonate resin filtered out is less than 5% by mass relative to the decomposition solution.

[0082] (Polycarbonate resin (PC))

[0083] The polycarbonate resin used in the method for producing bisphenol of the present invention comprises a polymer composition containing a carbonate bond (-OC(=O)-O-). Specifically, the polycarbonate resin used in the method for producing bisphenol of the present invention comprises a polymer containing a repeating unit derived from bisphenol represented by the general formula (1) (hereinafter, sometimes simply referred to as a "repeating unit").

[0084] [Chemistry 5]

[0085]

[0086] As R 1 ~R 4 , each independently includes a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, an aryl group, etc. For example, a hydrogen atom, a fluoro group, a chloro group, a bromo group, an iodo group, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentyl group, an isopentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclododecyl group, a benzyl group, a phenyl group, a tolyl group, and a 2,6-dimethylphenyl group may be mentioned.

[0087] As R 5 and R 6, each independently includes a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, etc. For example, a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, a 2-ethylhexyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentyl group, an isopentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclododecyl group, a benzyl group, a phenyl group, a tolyl group, and a 2,6-dimethylphenyl group may be mentioned.

[0088] R 5 and R 6 Two groups may be bonded or cross-linked to form cycloalkylene, fluorenylene (fluorenyl 9,9-diyl), xanthenylidene (xanthene 9,9-diyl), thioxanthenylidene (thioxanthene 9,9-diyl), etc. For example, examples of cycloalkylene include cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, 3,3,5-trimethylcyclohexylene, cycloheptylene, cyclooctylene, cyclononylene, cyclodecylene, cycloundecylene, and cyclododecylene.

[0089] In the method for producing bisphenol of the present invention, it is preferred to use R 1 ~R 4 is a hydrogen atom, R 5 , R 6 A methyl polycarbonate resin (bisphenol A type polycarbonate resin) is used as a raw material.

[0090] That is, the method for producing bisphenol of the present invention is suitable as a method for producing 2,2-bis(4-hydroxyphenyl)propane (hereinafter, sometimes referred to as "bisphenol A").

[0091] In the general formula (1), n ​​is not particularly limited and is, for example, 2 to 1,000.

[0092] As the raw material of the bisphenol manufacturing method of the present invention, not only the raw material of polycarbonate resin alone can be used, but also a composition containing a resin other than polycarbonate resin, such as a copolymer or a polymer alloy, can be used. As the composition containing a resin other than polycarbonate resin, for example, polycarbonate / polyester copolymers, polycarbonate / polyester alloys, polycarbonate / polyarylate copolymers, polycarbonate / polyarylate alloys, etc. can be cited. When using a composition containing a resin other than polycarbonate resin, a composition containing polycarbonate resin as the main component (containing more than 50% by mass of polycarbonate resin in the composition) can be suitably used.

[0093] The polycarbonate resin may be a mixture of two or more different polycarbonate resins. In addition, a single polycarbonate resin may be simply referred to as polycarbonate.

[0094] From the viewpoint of chemical recycling, polycarbonate resin is preferably the polycarbonate resin contained in waste plastics. Polycarbonate resin is molded into various molded products such as optical components such as headlights, optical recording media such as optical disks, and used. As waste plastics containing polycarbonate resin, scraps, defective products, used molded products, etc. when polycarbonate resin is molded into these molded products can be used.

[0095] Waste plastics that have been washed, crushed, pulverized, etc. can be used appropriately. As a crushing method for waste plastics, it is to use a jaw crusher, a gyratory crusher to crush to a coarse crushing of less than 20 cm, to use a gyratory crusher, a cone crusher, a mill to crush to a medium crushing of less than 1 cm, to use a mill to crush to a pulverizing of less than 1 mm, etc., as long as it can be reduced to a size that can be supplied to a decomposition tank. In addition, in the case where the waste plastics are thin plastics such as CDs and DVDs, they can be cut using a shredder and the like and then supplied to the decomposition tank. In addition, it is also possible to use a portion formed by components other than polycarbonate resins such as other resins of copolymers and polymer alloys, and layers on the surface or back of optical disks that are removed in advance.

[0096] (Dialkyl carbonate)

[0097] One of the characteristics of the method for producing bisphenol of the present invention is the use of a dialkyl carbonate. The dialkyl carbonate is preferably dimethyl carbonate, diethyl carbonate or dibutyl carbonate.

[0098] Among them, dimethyl carbonate and diethyl carbonate are preferred because they have relatively low boiling points and are easily removed after the decomposition reaction, thereby reducing the purification load.

[0099] The dialkyl carbonate includes dialkyl carbonate not derived from the polycarbonate resin. That is, when the polycarbonate resin is decomposed in the presence of an aliphatic monohydric alcohol, dialkyl carbonate is generated along with the decomposition of the polycarbonate resin, but in the bisphenol production method of the present invention, a dialkyl carbonate different from the dialkyl carbonate generated in the reaction is supplied to the reaction tank for decomposing the polycarbonate resin for use.

[0100] It should be noted that "dialkyl carbonate not derived from polycarbonate resin" refers to dialkyl carbonate not derived from polycarbonate resin used simultaneously, and is dialkyl carbonate supplied to the reaction tank. In the bisphenol production method of the present invention, dialkyl carbonate generated by decomposition of polycarbonate resin can also be reused in the next decomposition reaction as dialkyl carbonate not derived from polycarbonate resin used simultaneously.

[0101] Relative to the amount of the polycarbonate resin used, when the amount of the dialkyl carbonate used is small, the amount of the solid (polycarbonate resin) relative to the initial reaction liquid becomes more, and there is a tendency that the mixing is poor or the dissolution rate and the decomposition rate of the polycarbonate resin slow down. Therefore, the molar ratio of the dialkyl carbonate used relative to 1 mole of the repeating unit of the polycarbonate resin used is more than 1.8. More preferably, more than 1.9, more preferably, more than 2.0. In addition, relative to the polycarbonate resin used, when the amount of the dialkyl carbonate used is large, there is a tendency that the manufacturing efficiency deteriorates. Therefore, the molar ratio of the dialkyl carbonate used relative to 1 mole of the repeating unit of the polycarbonate resin used is preferably less than 100, more preferably less than 70, and further preferably less than 50.

[0102] For example, the molar ratio of the dialkyl carbonate used in the decomposition reaction is preferably 1.8 to 100, more preferably 1.9 to 70, and even more preferably 2.0 to 50, relative to 1 mol of the repeating unit of the polycarbonate resin used in the decomposition reaction. Alternatively, the molar ratio may be 2.5 to 45, 3.0 to 40, or the like.

[0103] It should be noted that, in the present application, the amount (mole, mass) of the polycarbonate resin used in the decomposition reaction refers to the input amount of the polycarbonate resin (the amount supplied to the reaction tank). In addition, sometimes the "polycarbonate resin used in the decomposition reaction" is abbreviated as "the polycarbonate resin used". The same is true for other materials such as dialkyl carbonates, aliphatic alcohols, and catalysts.

[0104] The number of moles of the repeating unit of the polycarbonate resin used is the value obtained by dividing the mass of the polycarbonate resin used (the mass input) by the molecular weight of the repeating unit derived from bisphenol. In the case of the polycarbonate resin represented by the above general formula (1), the repeating unit derived from bisphenol has a structure of n=1 in the above general formula (1). The number of moles of the dialkyl carbonate used is the value obtained by dividing the mass of the dialkyl carbonate used (the mass input) by the molecular weight of the dialkyl carbonate. Therefore, the molar ratio of the dialkyl carbonate used to 1 mole of the repeating unit of the polycarbonate resin used is "(mass of the dialkyl carbonate used [g] / molecular weight of the dialkyl carbonate [g / mol]) / (mass of the polycarbonate resin used [g] / molecular weight of the repeating unit of the polycarbonate resin [g / mol])".

[0105] It should be noted that, since dialkyl carbonate is generated as the polycarbonate resin decomposes, the dialkyl carbonate contained in the reaction solution at the end of the reaction includes dialkyl carbonate not derived from the polycarbonate resin (dialkyl carbonate supplied to the reaction tank) and dialkyl carbonate derived from the polycarbonate resin (dialkyl carbonate generated by alcoholysis of the polycarbonate resin). A portion of the dialkyl carbonate contained in the reaction solution at the end of the reaction is dialkyl carbonate not derived from the polycarbonate resin. The molar ratio of dialkyl carbonate (the total of the dialkyl carbonate used and the generated dialkyl carbonate) relative to 1 mol of the repeating unit of the polycarbonate resin used at the end of the reaction is greater than the molar ratio of dialkyl carbonate used relative to 1 mol of the repeating unit of the polycarbonate resin used. The molar ratio of dialkyl carbonate (the total of the dialkyl carbonate used and the generated dialkyl carbonate) relative to 1 mol of the repeating unit of the polycarbonate resin used at the end of the reaction is preferably 2.8 or more, more preferably 2.81 or more, more preferably 3.3 or more, and further preferably 3.8 or more.

[0106] (Aliphatic monohydric alcohol)

[0107] One of the characteristics of the bisphenol production method of the present invention is the use of aliphatic monohydric alcohols. Examples of the aliphatic monohydric alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, n-pentanol, isopentanol, n-hexanol, n-heptanol, n-octanol, n-nonanol, n-decanol, n-undecanol, and n-dodecanol.

[0108] Among them, the aliphatic monohydric alcohol is preferably an alcohol having 1 to 5 carbon atoms, and more preferably any one selected from the group consisting of methanol, ethanol, and butanol.

[0109] In addition, the aliphatic monohydric alcohol preferably uses an aliphatic monohydric alcohol having the same alkyl group as the dialkyl carbonate used. For example, when dimethyl carbonate is used as the dialkyl carbonate, methanol is preferably used, when diethyl carbonate is used as the dialkyl carbonate, ethanol is preferably used, and when dibutyl carbonate is used as the dialkyl carbonate, butanol is preferably used.

[0110] When the amount of aliphatic monohydric alcohol used is small relative to the amount of polycarbonate resin used, the polycarbonate resin becomes difficult to decompose, the decomposition rate decreases, and the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of aliphatic monohydric alcohol to 1 mol of repeating unit of polycarbonate resin ((mass of aliphatic monohydric alcohol used [g] / molecular weight of aliphatic monohydric alcohol [g / mol]) / (mass of polycarbonate resin used [g] / molecular weight of repeating unit of polycarbonate resin [g / mol])) is preferably 0.1 or more, more preferably 0.5 or more, and further preferably 1.0 or more. In addition, when the amount of aliphatic monohydric alcohol used is large relative to the amount of polycarbonate resin used, there is a tendency for the manufacturing efficiency to deteriorate. Therefore, the molar ratio of aliphatic monohydric alcohol to 1 mol of repeating unit of polycarbonate resin is preferably 20.0 or less, more preferably 15.0 or less, and further preferably 10.0 or less.

[0111] The decomposition of polycarbonate resin can be controlled by adjusting the amount of aliphatic monohydric alcohol and the reaction time. When the structure of the decomposition product to be obtained is controlled by the amount of aliphatic monohydric alcohol, in order to efficiently manufacture dialkyl carbonate, the molar ratio of aliphatic monohydric alcohol to 1 mole of repeating unit of polycarbonate resin is preferably more than 2.0, more preferably more than 2.1, and further preferably more than 2.2. In addition, in order to efficiently manufacture bisphenol-alkyl carbonate condensation products (sometimes abbreviated as "condensation products"), the molar ratio of aliphatic monohydric alcohol to 1 mole of repeating unit of polycarbonate resin is preferably less than 2.0, and can be less than 1.95, less than 1.9, less than 1.85, less than 1.8, etc.

[0112] For example, in order to efficiently manufacture dialkyl carbonate, it is preferred that the molar ratio of the aliphatic monohydric alcohol relative to 1 mole of the repeating unit of the polycarbonate resin is 2.0 or more and 20.0 or less, 2.1 or more and 15.0 or less, or 2.2 or more and 10.0 or less. In addition, in order to efficiently manufacture bisphenol-alkyl carbonate condensates, it is preferred that the molar ratio of the aliphatic monohydric alcohol relative to 1 mole of the repeating unit of the polycarbonate resin is 0.1 or more and less than 2.0, 0.5 or more and 1.95 or less, or 1.0 or more and 1.9 or less.

[0113] In addition, the molar ratio of the aliphatic monohydric alcohol used relative to the dialkyl carbonate used (the molar number of the aliphatic monohydric alcohol used / the molar number of the dialkyl carbonate used) is preferably more than 0.01, more preferably more than 0.05. In addition, this molar ratio is preferably below 15.0, more preferably below 10.0, more preferably below 8.0, more preferably below 5.0. If the molar ratio of the aliphatic monohydric alcohol used relative to the dialkyl carbonate used is small, then the polycarbonate resin is difficult to decompose, and the decomposition rate reduces, and the decomposition time is long-termized. In addition, if this molar ratio is large, then when reclaiming dialkyl carbonate, the separation of the aliphatic monohydric alcohol and dialkyl carbonate becomes numerous and complicated.

[0114] For example, the molar ratio of the aliphatic monohydric alcohol used to the dialkyl carbonate used (input molar ratio) is preferably 0.01 to 10.0, 0.05 to 8.0, 0.1 to 6.0, 0.15 to 5.0 or 0.2 to 3.0. In addition, the molar ratio can be 0.25 to 2.5, 0.3 to 1.8, etc.

[0115] (catalyst)

[0116] One of the characteristics of the method for producing bisphenol of the present invention is that a catalyst selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal alkoxides, alkali metal oxides, chain alkylamines and pyridine is further used.

[0117] Wherein, the catalyst is preferably any one selected from the group consisting of alkali metal hydroxide, alkali metal carbonate, alkali metal alkoxide and alkali metal oxide, more preferably alkali metal hydroxide or alkali metal carbonate. It is believed that when using inorganic metal catalysts such as alkali metal hydroxide and alkali metal carbonate, dialkyl carbonate will decompose, so it is not preferred. However, the inventors have found that in the presence of dialkyl carbonate and aliphatic monohydric alcohol, when alkali metal hydroxide, alkali metal carbonate etc. are used as catalysts to decompose polycarbonate resin, polycarbonate resin decomposes with high reaction rate, and bisphenol with good color tone can be obtained. In addition, by using any one selected from the group consisting of alkali metal hydroxide, alkali metal carbonate, alkali metal alkoxide and alkali metal oxide, it is also not easy to produce odor, so it is preferred to use these catalysts.

[0118] [Alkali metal hydroxide]

[0119] In the present invention, alkali metal hydroxide is an alkali metal ion (M + ) and hydroxide ion (OH - ) is a salt thereof, which is a compound represented by MOH (M represents an alkali metal atom). As the alkali metal hydroxide, sodium hydroxide or potassium hydroxide is preferred.

[0120] If the amount of the alkali metal hydroxide used is small relative to the polycarbonate resin used, the decomposition rate slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the alkali metal hydroxide used relative to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the alkali metal hydroxide used [g] / molecular weight of the alkali metal hydroxide [g / mol]) / (the mass of the polycarbonate resin used [g] / molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0001 or more, more preferably 0.0005 or more, and further preferably 0.0007 or more. For example, it can be set to 0.001 or more, 0.01 or more, etc. Relative to the polycarbonate resin used, when the amount of the alkali metal hydroxide used is large, the amount of acid required for neutralization after decomposition increases, and there is a tendency for the manufacturing efficiency to decrease. Therefore, the molar ratio of the alkali metal hydroxide used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably less than 1, more preferably less than 0.9, and further preferably less than 0.8.

[0121] [Alkali metal carbonate]

[0122] In the present invention, alkali metal carbonate is an alkali metal ion (M + ) and carbonate ions (CO3 2- ) is a salt of M2CO3 or MHCO3 (M represents an alkali metal atom). As the alkali metal carbonate, sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate is preferred, and sodium carbonate or potassium carbonate is more preferred.

[0123] If the amount of the alkali metal carbonate used is small relative to the polycarbonate resin used, the decomposition rate slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the alkali metal carbonate used relative to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the alkali metal carbonate used [g] / the molecular weight of the alkali metal carbonate [g / mol]) / (the mass of the polycarbonate resin used [g] / the molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0001 or more, more preferably 0.0005 or more, and further preferably 0.001 or more. For example, it can be set to 0.001 or more, 0.01 or more, etc. If the amount of the alkali metal carbonate used is large relative to the polycarbonate resin used, the amount of acid required for neutralization after decomposition increases, and there is a tendency for the manufacturing efficiency to decrease. Therefore, the molar ratio of the alkali metal carbonate used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably 1 or less, more preferably 0.9 or less, and further preferably 0.8 or less.

[0124] [Alkali metal alkoxide]

[0125] In the present invention, the alkali metal alkoxide is an alkali metal ion (M + ) and aliphatic or aromatic alcohol salts, which is a compound represented by the following formula (2).

[0126] MOR H …Formula (2)

[0127] In formula (2), M represents an alkali metal atom, preferably sodium or potassium. H represents an alkyl group or an aryl group, and is preferably an alkyl group having 1 to 5 carbon atoms or a phenyl group.

[0128] As the alkali metal alkoxide, sodium phenoxide, sodium methoxide, sodium ethoxide, potassium phenoxide, potassium methoxide, potassium ethoxide and potassium tert-butoxide are preferred.

[0129] When the amount of the alkali metal alkoxide used is small relative to the polycarbonate resin used, the decomposition speed slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the alkali metal alkoxide used relative to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the alkali metal alkoxide used [g] / the molecular weight of the alkali metal alkoxide [g / mol]) / (the mass of the polycarbonate resin used [g] / the molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0001 or more, more preferably 0.0005 or more, and further preferably 0.001 or more. For example, it can be set to 0.001 or more, 0.01 or more, etc. When the amount of the alkali metal alkoxide used is large relative to the polycarbonate resin used, the amount of acid required for neutralization after decomposition increases, and there is a tendency for the manufacturing efficiency to decrease. Therefore, the molar ratio of the alkali metal alkoxide used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably 1 or less, more preferably 0.9 or less, and further preferably 0.8 or less.

[0130] [Alkali metal oxides]

[0131] Examples of the alkali metal oxide include sodium oxide and potassium oxide.

[0132] If the amount of the alkali metal oxide used is small relative to the polycarbonate resin used, the decomposition speed slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the alkali metal oxide used relative to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the alkali metal oxide used [g] / the molecular weight of the alkali metal oxide [g / mol]) / (the mass of the polycarbonate resin used [g] / the molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0001 or more, more preferably 0.0005 or more, and further preferably 0.001 or more. For example, it can be set to 0.001 or more, 0.01 or more, etc. If the amount of the alkali metal oxide used is large relative to the polycarbonate resin used, the amount of acid required for neutralization after decomposition increases, and there is a tendency for the manufacturing efficiency to decrease. Therefore, the molar ratio of the alkali metal oxide used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably 1 or less, more preferably 0.9 or less, and further preferably 0.8 or less.

[0133] [Chain alkylamine]

[0134] In the present invention, the chain alkylamine is a compound having an amine structure in which at least one hydrogen atom of ammonia is substituted by an alkyl group. The chain alkylamine preferably has a boiling point of 200°C or less, and more preferably has a boiling point of 160°C or less. If it is such a boiling point, it can be removed together with the dialkyl carbonate by reducing pressure and / or heating. In addition, if the boiling point is too low, the chain alkylamine may volatilize during the decomposition reaction and reduce the decomposition rate, so the boiling point of the chain alkylamine is preferably above 10°C, and more preferably above 30°C.

[0135] The chain alkylamine is preferably a chain alkylmonoamine or a chain alkyldiamine.

[0136] Among the chain alkyl monoamines, monoalkyl monoamines as primary amines react with the carbonate bond portion of the polycarbonate resin to form isocyanates, so dialkyl monoamines as secondary amines or trialkyl monoamines as tertiary amines are more preferred. Dialkyl monoamines as secondary amines react with the carbonate bond portion of the polycarbonate resin to form tetraalkyl ureas, so trialkyl monoamines as tertiary amines are more preferred.

[0137] The chain alkylamine is preferably an alkyl monoamine represented by the general formula (I).

[0138] [Chemistry 6]

[0139]

[0140] In the general formula (I), R A represents an alkyl group having 1 to 3 carbon atoms, R B ~R CEach independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0141] R A Preferably methyl, ethyl, n-propyl or isopropyl, R B ~R C A hydrogen atom, a methyl group, an ethyl group, an n-propyl group or an isopropyl group is respectively preferred independently.

[0142] Specific examples of the chain alkylamine represented by the general formula (I) include methylamine, ethylamine, propylamine, dimethylamine, diethylamine, trimethylamine, triethylamine and the like.

[0143] The chain alkylamine is preferably an alkyldiamine represented by the general formula (II).

[0144] [Chemistry 7]

[0145]

[0146] In the general formula (II), R D ~R G Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and m represents an integer of 1 to 6.

[0147] R D ~R G Each independently preferred is methyl, ethyl, n-propyl or isopropyl.

[0148] Specific examples of the chain alkylamine represented by the general formula (II) include ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, N-methylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethyltrimethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N'-diethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, 1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diaminopropane, and the like.

[0149] If the amount of the chain alkylamine used is small relative to the polycarbonate resin used, the decomposition speed slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the amino group N of the chain alkylamine used to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the alkylamine used [g] × the number of amino group N / the molecular weight of the chain alkylamine [g / mol]) / (the mass of the polycarbonate resin used [g] / the molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0005 or more, more preferably 0.0007 or more, and further preferably 0.001 or more. For example, it can be set to 0.01 or more, 0.1 or more, etc. If the amount of the chain alkylamine used is large relative to the polycarbonate resin used, it is easier to generate amine odor, or it is difficult to generate dialkyl carbonate and condensate. Therefore, the molar ratio of N of the amino group of the chain alkylamine used to 1 mol of the repeating unit of the polycarbonate resin used is preferably 4.5 or less, and the smaller the ratio, the more preferably it is in the order of 4.0 or less, 3.0 or less, 2.0 or less, 1.0 or less, 0.9 or less, and 0.8 or less.

[0150] [Pyridine]

[0151] In the present invention, pyridine may be unsubstituted or may have a substituent such as a methyl group or a hydroxyl group. Unsubstituted pyridine is preferred.

[0152] When the amount of pyridine used is small relative to the polycarbonate resin used, the decomposition rate slows down, the decomposition time is prolonged, and there is a tendency for the efficiency to deteriorate. Therefore, the molar ratio of the pyridine used relative to 1 mol of the repeating unit of the polycarbonate resin used ((the mass of the pyridine used [g] / the molecular weight of the pyridine [g / mol]) / (the mass of the polycarbonate resin used [g] / the molecular weight of the repeating unit of the polycarbonate resin [g / mol])) is preferably 0.0005 or more, more preferably 0.0007 or more, and further preferably 0.001 or more. For example, it can be set to 0.01 or more, 0.1 or more, etc. If the amount of pyridine used is large relative to the polycarbonate resin used, it is easier to generate odor, or it is difficult to generate dialkyl carbonate and condensation products. Therefore, the molar ratio of the pyridine used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably 4.5 or less, and the smaller the order of 4.0 or less, 3.0 or less, 2.0 or less, 1.0 or less, 0.9 or less, and 0.8 or less is more preferred.

[0153] (Preparation of reaction solution)

[0154] The bisphenol production method of the present invention is to prepare a reaction solution by mixing a polycarbonate resin, a dialkyl carbonate (a dialkyl carbonate not derived from the polycarbonate resin), an aliphatic monohydric alcohol and a catalyst. That is, in the bisphenol production method of the present invention, a dialkyl carbonate not derived from the polycarbonate resin is supplied to a reaction tank for decomposing the polycarbonate resin to prepare the reaction solution.

[0155] The mixing order of the polycarbonate resin, dialkyl carbonate (dialkyl carbonate not derived from the polycarbonate resin), aliphatic monohydric alcohol and catalyst is not particularly limited. For example, dialkyl carbonate, aliphatic monohydric alcohol and catalyst may be sequentially supplied to the polycarbonate resin, or polycarbonate resin, aliphatic monohydric alcohol and catalyst may be sequentially supplied to the dialkyl carbonate. In order to be able to mix more uniformly, the polycarbonate resin is preferably supplied to the reaction tank after the dialkyl carbonate and / or aliphatic monohydric alcohol.

[0156] (Reaction solution)

[0157] The prepared reaction solution (reaction solution at the start of the reaction) contains a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst. At least the reaction after the reaction just starts is preferably carried out in a slurry solution in which the polycarbonate resin is dispersed in a liquid component containing a dialkyl carbonate and an aliphatic monohydric alcohol. The theoretical slurry concentration (mass of the solid component used in the preparation of the reaction solution / mass of all materials used in the preparation of the reaction solution) in the prepared reaction solution is preferably 0.05 or more, more preferably 0.1 or more. In addition, it is preferably 0.5 or less, more preferably 0.4 or less. When the theoretical slurry concentration (concentration of the solid component) is too low, the decomposition efficiency is reduced, and when the theoretical slurry concentration is too high, mixing is poor.

[0158] The liquid component in the prepared reaction solution contains dialkyl carbonate and aliphatic monohydric alcohol as main components, and the total mass of dialkyl carbonate and aliphatic monohydric alcohol relative to the mass of all liquid components is 0.8 or more, 0.9 or more, 0.95 or more, etc.

[0159] The total mass of the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst relative to the mass of the prepared reaction solution may be 0.9 or more, 0.95 or more, 0.98 or more, 0.99 or more, etc. Alternatively, the reaction solution may be composed of a polycarbonate resin, a dialkyl carbonate, aliphatic monohydric alcohol and a catalyst.

[0160] When it is desired to obtain dialkyl carbonate and condensation products together with bisphenol, if water is contained in the reaction solution prepared, the dialkyl carbonate and condensation products generated are easily decomposed. Therefore, the content of water in the prepared reaction solution (the mass of water / reaction solution) is usually below 0.005. The content of water in the reaction solution is preferably below 0.001, more preferably below 0.0005.

[0161] The preparation of the reaction solution is preferably carried out at 10°C or more, more preferably at 20°C or more. In addition, the preparation of the reaction solution is preferably carried out at 40°C or less, more preferably at 35°C or less. When the temperature during the preparation of the reaction solution is too low, the dissolution rate of the polycarbonate resin decreases. In addition, sometimes the viscosity of the reaction solution increases, which is prone to poor mixing or difficult to mix uniformly. In addition, when the temperature during the preparation of the reaction solution is too high, depending on the type of catalyst, it is easy to volatilize, and it may be difficult to prepare to a specified concentration and difficult to control the decomposition reaction.

[0162] (Decomposition reaction)

[0163] In the bisphenol production method of the present invention, the carbonate bond of the polycarbonate resin is partially cut due to the presence of dialkyl carbonate, aliphatic monohydric alcohol and catalyst, and decomposition occurs. That is, the polycarbonate resin reacts with the aliphatic monohydric alcohol and decomposes by alcoholysis. Thus, decomposition products such as bisphenol, dialkyl carbonate, and condensation product of bisphenol and dialkyl carbonate are generated. By controlling the amount of dialkyl carbonate and aliphatic monohydric alcohol and the reaction time, the decomposition reaction can be controlled, for example, bisphenol and dialkyl carbonate are preferentially generated.

[0164] For example, by setting the molar ratio of the aliphatic monohydric alcohol to 1 mol of the repeating unit of the polycarbonate resin to 2.0 or more, the polycarbonate resin is preferentially decomposed into bisphenol and dialkyl carbonate, thereby efficiently obtaining bisphenol and dialkyl carbonate.

[0165] Alternatively, the molar ratio of the aliphatic monohydric alcohol to 1 mol of the repeating unit of the polycarbonate resin may be set to less than 2.0, or the reaction time may be shortened to produce a condensate of bisphenol and dialkyl carbonate.

[0166] It should be noted that in order to prevent the decomposition reaction from occurring during the preparation of the reaction solution (mixing of the polycarbonate resin, dialkyl carbonate (dialkyl carbonate not derived from the polycarbonate resin), aliphatic monohydric alcohol and catalyst), the concentration of the polycarbonate resin, the temperature during the preparation of the reaction solution, etc. can be controlled to clearly separate the preparation process of the reaction solution and the decomposition reaction process, but the preparation process of the reaction solution and the decomposition process do not necessarily need to be clearly separated. The decomposition reaction of the polycarbonate resin can be performed during the preparation of the reaction solution, and a portion of the polycarbonate resin is decomposed. By decomposing a portion of the polycarbonate resin during the preparation of the reaction solution, the decomposition reaction can be performed more efficiently.

[0167] The decomposition reaction may be carried out under normal pressure or under increased pressure. However, since the reaction proceeds sufficiently even under normal pressure, it is preferably carried out under normal pressure.

[0168] (Reaction temperature)

[0169] From the preparation of the reaction solution to the cessation of the decomposition reaction, it can be carried out at the same temperature as the temperature when the reaction solution is prepared, but it is preferably heated to a specified reaction temperature after the reaction solution is prepared (after the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst are mixed). When the temperature during the preparation of the reaction solution is too high, it is likely to be difficult to control the decomposition reaction. By heating the reaction solution after preparation, the decomposition reaction can be stably carried out, so it is preferred.

[0170] The reaction temperature is appropriately selected according to the type of dialkyl carbonate, reaction time, etc. At high temperatures, the aliphatic monohydric alcohol in the reaction solution evaporates and alcoholysis stops. In addition, at low temperatures, solvent decomposition is difficult to proceed, the reaction rate is reduced, and the time required for decomposition is prolonged. Therefore, the reaction temperature is preferably 20°C or more, and the higher the order of 30°C or more and 40°C or more, the more preferred. In addition, it is preferably 120°C or less, and the smaller the value in the order of 110°C or less, 100°C or less, and 95°C or less, the more preferred.

[0171] In particular, the decomposition of the polycarbonate resin is preferably carried out at a reaction temperature of 20 to 120° C. and normal pressure, more preferably at a reaction temperature of 30 to 110° C. and normal pressure, and further preferably at a reaction temperature of 40 to 100° C. and normal pressure.

[0172] It should be noted that, when the reaction is carried out at the same temperature as when the reaction solution is prepared, the reaction temperature is the average temperature from the time when the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst are mixed to the time when the neutralization and distillation operations for stopping the decomposition reaction are started. In addition, when the temperature is raised after the reaction solution is prepared and the reaction is carried out, it is the average temperature from the time when the specified temperature is reached to the time when the neutralization and distillation operations for stopping the decomposition reaction are started.

[0173] In addition, as described later, when the first decomposition step and the second decomposition step are performed, the reaction temperature of each step is also preferably set to the above reaction temperature. In addition, in the first decomposition step and the second decomposition step, the reaction temperature may be the same or different.

[0174] (Reaction time)

[0175] The reaction time is appropriately selected based on the theoretical slurry concentration, reaction temperature, etc. When the reaction time is long, the generated bisphenol tends to decompose, so it is preferably 30 hours or less, and the shorter the reaction time is, the more preferably it is in the order of 25 hours or less, 20 hours or less, 15 hours or less, 10 hours or less, and 5 hours or less. In addition, when the reaction time is short, the decomposition reaction may not proceed sufficiently, so it is preferably 0.1 hours or more, more preferably 0.5 hours or more, and even more preferably 1 hour or more.

[0176] It should be noted that the reaction time is the time from the moment when the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst are mixed to the moment when the neutralization and distillation operations for stopping the decomposition reaction are started. The end point of the reaction time can be determined by tracking the decomposition reaction by liquid chromatography or the like.

[0177] In addition, when the polycarbonate resin is decomposed by performing the first decomposition step and the second decomposition step, the above reaction time is the total time of the first decomposition step and the second decomposition step.

[0178] (Decomposition method)

[0179] The bisphenol production method of the present invention only needs to decompose the polycarbonate resin by alcoholysis. Therefore, after preparing the reaction solution, the decomposition reaction may be carried out without additional supply until the reaction is completed, or water may be supplied during the reaction to control the balance of the decomposition reaction.

[0180] In order to increase the yield of bisphenol or facilitate the recycling of dialkyl carbonate and aliphatic monohydric alcohol, it is preferred to add water to the reaction solution after the decomposition reaction has proceeded to a certain extent.

[0181] [Method for decomposing polycarbonate resin (1)]

[0182] For example, as a method (1) for decomposing a polycarbonate resin, there can be mentioned a method comprising a first decomposition step and a second decomposition step, wherein the first decomposition step and the second decomposition step are performed continuously, wherein the first decomposition step comprises decomposing the polycarbonate resin in a reaction liquid containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst to obtain a first decomposition liquid containing bisphenol, and wherein the second decomposition step comprises mixing the first decomposition liquid with water to hydrolyze the dialkyl carbonate, regenerate the aliphatic monohydric alcohol, and decompose the polycarbonate resin to produce bisphenol.

[0183] By this method, the polycarbonate resin can be decomposed by alcoholysis, and the dialkyl carbonate and condensate produced together with bisphenol can be hydrolyzed to regenerate (produce) aliphatic monohydric alcohol. As a result, the equilibrium of the decomposition reaction of the polycarbonate resin is shifted, and the decomposition reaction of the polycarbonate resin becomes easier to proceed.

[0184] [First decomposition step]

[0185] The first decomposition step is a step of decomposing the polycarbonate resin in a reaction solution containing the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and a catalyst to obtain a first decomposition solution containing bisphenol. In the first decomposition step, the polycarbonate resin reacts with the aliphatic monohydric alcohol to decompose by alcoholysis, and the aliphatic monohydric alcohol is consumed to generate decomposition products such as bisphenol, dialkyl carbonate, and a condensate of bisphenol and dialkyl carbonate.

[0186] In the first decomposition step, the prepared reaction liquid is preferably in a slurry state. The theoretical slurry concentration (mass of solid components used in the preparation of the reaction liquid / mass of all materials used in the preparation of the reaction liquid) in the prepared reaction liquid is preferably above 0.05, and more preferably above 0.1. In addition, it is preferably below 0.5, and more preferably below 0.4. When the theoretical slurry concentration (concentration of solid components) is too low, the decomposition efficiency decreases, and when the theoretical slurry concentration is too high, the mixing is poor. Therefore, it is preferred that at the end of the first decomposition step, the slurry state in which the polycarbonate resin is dispersed has disappeared. In addition, it is more preferred that at the end of the first decomposition step, the polycarbonate resin is completely dissolved, and the first decomposition liquid becomes a non-slurry liquid.

[0187] The method for preparing the reaction solution and the reaction temperature are as described above. The molar ratio of the aliphatic monohydric alcohol used relative to 1 mol of the repeating unit of the polycarbonate resin used is preferably 2.0 or more, more preferably 2.1 or more, and even more preferably 2.2 or more.

[0188] In order to prevent the decomposition product from being hydrolyzed in the first decomposition step, the first decomposition step is preferably carried out under conditions where the amount of water relative to 1 mol of the repeating unit of the polycarbonate resin used (i.e., the amount of the polycarbonate resin charged) is 0.1 mol or less, 0.05 mol or less, 0.01 mol or less, etc. In addition, the water content of the prepared reaction solution can be managed, and the first decomposition step can be carried out with the water content of the prepared reaction solution being 0.5 mass % or less, 0.1 mass % or less, 0.05 mass % or less, etc.

[0189] The reaction time of the first decomposition step is not particularly limited. In the case of a slurry-like reaction solution at the start of the reaction, it is preferably set to a time longer than the time until the slurry-like state in which the polycarbonate resin is dispersed disappears and becomes a non-slurry-like liquid. In addition, it is more preferably set to a time longer than the time until the reaction solution becomes a liquid in which at least all the polycarbonate resin has been dissolved. If the second decomposition step is transferred to the second decomposition step in the state of the slurry-like reaction solution, the dissolution rate of the undissolved polycarbonate resin decreases, and there is a tendency that the decomposition takes time. For example, the first decomposition step can be set to more than 0.1 hours, more than 0.25 hours, more than 0.5 hours, more than 1 hour, etc.

[0190] [Second decomposition step]

[0191] The second decomposition step is a step of hydrolyzing the dialkyl carbonate by mixing the first decomposition liquid with water, regenerating the aliphatic monohydric alcohol, and decomposing the polycarbonate resin to generate bisphenol. In the second decomposition step, the alcoholysis of the polycarbonate resin is also carried out together with the hydrolysis of the dialkyl carbonate. At this time, in addition to the unreacted aliphatic monohydric alcohol, the aliphatic monohydric alcohol generated by the hydrolysis of the dialkyl carbonate can also react with the polycarbonate resin, so the reaction rate of the decomposition of the polycarbonate resin is increased. The reaction liquid (decomposition liquid) at the end of the second decomposition step dissolves the bisphenol and becomes a non-slurry liquid. Even if the polycarbonate resin remains at the end of the second decomposition step, the slurry in which the polycarbonate resin is dispersed will disappear and become a non-slurry liquid. It is preferred that the polycarbonate resin is completely dissolved at the end of the second decomposition step, and the decomposition liquid is a non-slurry liquid.

[0192] In addition, it is preferred that the aliphatic monohydric alcohol regenerated in the second decomposition step is separated from bisphenol in the form of a mixture with dialkyl carbonate, and the mixture of the aliphatic monohydric alcohol and dialkyl carbonate is reused in the first decomposition step. This further reduces the environmental load.

[0193] For example, the decomposition liquid obtained in the second decomposition step contains bisphenol, aliphatic monohydric alcohol and dialkyl carbonate. By distilling the decomposition liquid or the liquid obtained by neutralizing it, the aliphatic monohydric alcohol and dialkyl carbonate can be recovered. In particular, dimethyl carbonate and methanol are azeotropic, so when using dimethyl carbonate and methanol, the mixture of dimethyl carbonate and methanol can be recovered by distillation. The recovered distillation removal liquid can be reused in the preparation of the reaction liquid of the first decomposition step.

[0194] In the second decomposition process, when the amount of water mixed with the first decomposition liquid is too small, the amount of the regenerated aliphatic monohydric alcohol is small, and the decomposition promotion effect of the undecomposed polycarbonate resin is low. On the other hand, when it is too much, the amount of the regenerated aliphatic monohydric alcohol becomes more, so the undecomposed polycarbonate resin can be efficiently decomposed. However, in the case of recycling the mixture of aliphatic monohydric alcohol and dialkyl carbonate and reusing it in the first decomposition process, since the aliphatic monohydric alcohol becomes excessive, it is difficult to directly use the entire amount recovered. In particular, since methanol and dimethyl carbonate form an azeotropic composition, it is difficult to obtain them separately by distillation. Therefore, the amount of water mixed with the first decomposition liquid is preferably 0.5 mol or more and 1.5 mol or less, more preferably 0.6 mol or more and 1.4 mol or less, and most preferably 0.7 mol or more and 1.3 mol or less, relative to 1 mol of the repeating unit of the polycarbonate resin used.

[0195] The amount of the aliphatic monohydric alcohol and dialkyl carbonate contained in the decomposition liquid after the second decomposition process is preferably in the range of 80 mass % to 120 mass %, and more preferably in the range of 90 mass % to 110 mass % relative to the amount (input amount) used in the first decomposition process. If it is a composition within this range, even if the reaction liquid of the first decomposition process is prepared in the state of a mixed liquid of aliphatic monohydric alcohol and dialkyl carbonate, it is easy to adjust the reaction liquid to a desired composition. Therefore, as a mixed liquid of aliphatic monohydric alcohol and dialkyl carbonate, it is easy to reuse in the first decomposition process.

[0196] [Method for decomposing polycarbonate resin (2)]

[0197] In the case where it is desired to obtain a condensate together with bisphenol, it is preferred to carry out the decomposition reaction in a manner that does not hydrolyze the condensate. In such a case, it is preferred that after the reaction solution is prepared, no additional water is supplied, and the decomposition reaction is carried out until the reaction is completed. In order to suppress the hydrolysis of the decomposition product, the decomposition reaction is preferably carried out under conditions such as a water content of 0.5% by mass or less, 0.1% by mass or less, or 0.05% by mass or less. The amount of water relative to 1 mol of the repeating unit of the polycarbonate resin used can be managed, and the conditions such as 0.1 mol or less, 0.05 mol or less, or 0.01 mol or less of water relative to 1 mol of the repeating unit of the polycarbonate resin used can be set.

[0198] (Method for stopping decomposition reaction of polycarbonate resin)

[0199] The method for stopping the decomposition reaction of the polycarbonate resin is appropriately selected according to the type of catalyst used. When a chain alkylamine or pyridine is used as a catalyst, the decomposition reaction can be stopped by removing and neutralizing the chain alkylamine or pyridine by distillation. In the method of supplying an acid and removing the chain alkylamine or pyridine by neutralization, ammonium salts or pyridinium salts are produced, which also need to be removed, so the removal of the chain alkylamine or pyridine is preferably a method of removing by distillation. In addition, when an alkali metal hydroxide or an alkali metal carbonate is used as a catalyst, the decomposition reaction can be stopped by neutralization.

[0200] (Bisphenol Recovery)

[0201] The recovery of bisphenol from the reaction liquid after the decomposition reaction can be carried out by stopping the decomposition reaction of the polycarbonate resin and then performing a method such as crystallization or column chromatography.

[0202] Bisphenol is preferably recovered by crystallization, and the method for producing bisphenol of the present invention preferably includes a crystallization step for recovering bisphenol by crystallization. Specifically, after the decomposition reaction of the polycarbonate resin, the organic phase obtained by removing the catalyst and the solvent from the reaction solution or adding a mixed organic solvent is washed with water or saline, and then neutralized and washed with ammonium chloride water, etc. as needed. Then, the washed organic phase is cooled to crystallize.

[0203] As the organic solvent that can be used during neutralization and crystallization, aromatic hydrocarbons such as toluene, xylene, ethylbenzene, diethylbenzene, isopropylbenzene and mesitylene, aliphatic hydrocarbons such as hexane, heptane, octane, nonane, decane, undecane and dodecane, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, n-pentanol, isopentanol, n-hexanol, n-heptanol, n-octanol, n-nonanol, n-decanol, n-undecanol, n-dodecanol, aliphatic alcohols such as ethylene glycol, diethylene glycol and triethylene glycol, etc. can be used.

[0204] In addition, before the crystallization, the remaining dialkyl carbonate and the organic solvent may be removed by distillation and then the crystallization may be performed.

[0205] (Recovery of Bisphenol-Alkyl Carbonate Condensate)

[0206] The method for producing bisphenol of the present invention can further recover the bisphenol-alkyl carbonate condensate represented by the following formula (III) produced as a by-product during the decomposition of the polycarbonate resin.

[0207] [Chemistry 8]

[0208]

[0209] In formula (III), R is methyl, ethyl or butyl, preferably methyl.

[0210] The recovery (isolation and purification) of the bisphenol-alkyl carbonate condensate can be carried out by a conventional method, for example, crystallization, purification by column chromatography, etc.

[0211] [Bisphenol production method (1)]

[0212] The method for producing bisphenol of the present invention may be a method for producing bisphenol (1) comprising the following step A, step B1, and step C1.

[0213] Step A: a step of decomposing the polycarbonate resin in a reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a polycarbonate decomposition solution containing bisphenol,

[0214] Step B1: a step of concentrating the polycarbonate decomposition liquid obtained in step A to obtain a concentrated liquid,

[0215] Step C1: Aromatic hydrocarbons are supplied to the concentrated liquid obtained in step B1 to perform crystallization, thereby precipitating bisphenol to obtain a slurry containing bisphenol, and the obtained slurry is subjected to solid-liquid separation to obtain bisphenol.

[0216] [Process A]

[0217] In step A, for example, a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol, and a catalyst selected from the group consisting of an alkali metal hydroxide, an alkali metal carbonate, an alkali metal alkoxide, a chain alkylamine, and pyridine is stirred for a predetermined time. As a result, the polycarbonate resin is decomposed to generate bisphenol, thereby obtaining a polycarbonate decomposition solution containing bisphenol. The types of the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol, the catalyst, the mixing ratio thereof, the reaction temperature, etc. are as described above.

[0218] In addition, in step A, it is preferred to decompose the polycarbonate resin in a slurry-like reaction liquid and carry out the reaction. In step A, after preparing a slurry-like reaction liquid, no additional supply is performed, and the decomposition reaction is performed until the reaction is completed, or water can be mixed during the reaction to control the balance of the decomposition reaction. The theoretical slurry concentration (the mass of the solid components used in the preparation of the reaction liquid / the mass of all materials used in the preparation of the reaction liquid) in the prepared reaction liquid is preferably 0.05 or more, and more preferably 0.1 or more. In addition, it is preferably 0.5 or less, and more preferably 0.4 or less. When the theoretical slurry concentration (concentration of the solid components) is too low, the decomposition efficiency is reduced, and when the theoretical slurry concentration is too high, the mixing is poor. Moreover, as the decomposition reaction proceeds, the polycarbonate resin will dissolve, and the slurry state in which the polycarbonate resin is dispersed will disappear. At the end of step A, a non-slurry liquid in which bisphenol is dissolved can be obtained. Even if polycarbonate resin remains at the end of step A, it becomes a non-slurry liquid, preferably a liquid in which the polycarbonate resin is completely dissolved.

[0219] [Process B1]

[0220] In step B1, the concentration of the polycarbonate decomposition liquid can be carried out by distilling off the solvent. The distillation is preferably carried out in a manner that the concentrated liquid becomes less than 70% by mass of the polycarbonate decomposition liquid, preferably less than 60% by mass, and more preferably less than 50% by mass. In addition, the distillation is preferably carried out in a manner that the concentrated liquid becomes more than 20% by mass of the polycarbonate decomposition liquid, preferably more than 30% by mass. If over-concentrated, there are problems of bisphenol precipitation and solidification of the concentrated liquid. For example, the distillation can be carried out at a temperature of 50 to 200° C. and a pressure of 0.1 kPa to 150 kPa.

[0221] In addition, the polycarbonate decomposition liquid can be concentrated after neutralization and washing. Neutralization is performed by mixing the polycarbonate decomposition liquid with an acid such as hydrochloric acid, sulfuric acid, phosphoric acid, etc. Neutralization is preferably performed in a manner that adjusts the amount of the mixed acid so that the pH becomes 5.5 to 9.0 (preferably pH 6.0 to 8.0). After the polycarbonate decomposition liquid is mixed with the acid, the aqueous phase is removed, or the neutralization salt is removed when the neutralization salt precipitates, thereby obtaining a neutralized liquid containing bisphenol. The neutralized liquid can also be concentrated.

[0222] [Process C1]

[0223] In step C1, first, the concentrate is mixed with an aromatic hydrocarbon, and bisphenol is precipitated from the mixed solution containing the concentrate and the aromatic hydrocarbon by crystallization. Examples of the aromatic hydrocarbon mixed with the concentrate include toluene, xylene, ethylbenzene, diethylbenzene, isopropylbenzene, mesitylene, etc., and toluene is preferred.

[0224] Crystallization can be generally performed by cooling a mixed solution containing a concentrate and aromatic hydrocarbons. For example, the temperature before crystallization is 60 to 100°C (preferably 70 to 90°C) and then cooled to 40 to 70°C (preferably 40 to 65°C). Thus, bisphenol is precipitated in the mixed solution to obtain a slurry containing bisphenol.

[0225] Next, the bisphenol-containing slurry is subjected to solid-liquid separation, so that the bisphenol can be recovered as a solid component. The solid-liquid separation can be performed by known means such as filtration and centrifugation. For example, a horizontal belt filter, a rotary vacuum filter, a rotary pressure filter, an intermittent filter, a centrifugal filter separator, a centrifugal sedimentation separator, or a hybrid centrifugal separator thereof (a screen sedimentation centrifuge) can be used for solid-liquid separation.

[0226] The obtained bisphenol can be further purified by washing with water, washing by suspension, etc. In addition, crystallization can be performed multiple times. By dissolving the bisphenol obtained in step C1 in an aromatic hydrocarbon and crystallizing the obtained solution, bisphenol with higher purity can be precipitated.

[0227] [Bisphenol production method (2)]

[0228] The method for producing bisphenol of the present invention may be a method for producing bisphenol (2) comprising the following step A, step B2, and step C2.

[0229] Step A: a step of decomposing the polycarbonate resin in a reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a polycarbonate decomposition solution containing bisphenol,

[0230] Step B2: a step of removing the dialkyl carbonate and the aliphatic monohydric alcohol from the solution containing the polycarbonate decomposition liquid obtained in step A and the aromatic monohydric alcohol to obtain a solution containing bisphenol and the aromatic monohydric alcohol,

[0231] Step C2: a step of recovering bisphenol from the solution containing bisphenol and aromatic monohydric alcohol obtained in step B2.

[0232] The step A of the method for producing bisphenol (2) is the same as the step A of the method for producing bisphenol (1).

[0233] [Process B2]

[0234] In step B2, the dialkyl carbonate and the aliphatic monohydric alcohol can be removed by distillation of the solution containing the polycarbonate decomposition liquid and the aromatic monohydric alcohol. For example, the distillation can be performed at a temperature of 50 to 200° C. and a pressure of 0.1 kPa to 150 kPa. In addition, it is preferred that at least a portion of the aromatic monohydric alcohol is also removed by distillation.

[0235] In addition, the polycarbonate decomposition liquid can be subjected to step B2 after neutralization and washing in the same manner as step B1 of the bisphenol production method (1). Step B2 is carried out, for example, using a mixed solution of the polycarbonate decomposition liquid obtained in step A and an aromatic monohydric alcohol. The polycarbonate decomposition liquid can be subjected to step B2 after neutralization and washing and mixed with an aromatic monohydric alcohol.

[0236] [Process C2]

[0237] The bisphenol can be recovered from the solution containing bisphenol and aromatic monohydric alcohol obtained in step B2 by crystallization, etc. For example, when a polycarbonate resin derived from bisphenol A is used and phenol is used as the aromatic monohydric alcohol in step B2, a polycarbonate decomposition liquid containing bisphenol A can be obtained in step A, and a solution containing bisphenol A and phenol can be obtained in step B2.

[0238] In step C2, the solution containing bisphenol A and phenol may be crystallized to obtain crystals of an adduct of bisphenol A and phenol, and then phenol may be removed from the melt of the adduct crystals to obtain bisphenol A. Alternatively, the solution containing bisphenol A and phenol may be added to a reaction step, a purification step, a mother liquor circulation step (a step of subjecting bisphenol A in the mother liquor to alkaline decomposition), etc., of a production facility for producing bisphenol A from acetone and phenol, and crystallized together with bisphenol A produced by the production facility to obtain crystals of an adduct of bisphenol A and phenol, and then phenol may be removed from the melt of the adduct crystals to obtain bisphenol A.

[0239] <Uses of bisphenol>

[0240] The bisphenol obtained by the bisphenol production method of the present invention (hereinafter sometimes referred to as "regenerated bisphenol") can be used as a constituent component, curing agent, additive or precursor thereof of various thermoplastic resins such as polyether resins, polyester resins, polyarylate resins, polycarbonate resins, polyurethane resins, acrylic resins, epoxy resins, unsaturated polyester resins, phenolic resins, polybenzoxazine resins, cyanate resins, etc., which are used in various applications such as optical materials, recording materials, insulating materials, transparent materials, electronic materials, adhesive materials, heat-resistant materials, etc. In addition, it is also useful as a color developer, anti-fading agent, bactericide, antibacterial and antifungal agent, etc., for heat-sensitive recording materials, etc.

[0241] Among them, since it can impart good mechanical properties, it is preferably used as a raw material (monomer) for thermoplastic resins and thermosetting resins, and more preferably as a raw material for polycarbonate resins and epoxy resins. In addition, it is also preferably used as a developer, and is particularly preferably used in combination with a leuco dye or a color-changing temperature regulator.

[0242] <Bisphenol-alkyl carbonate condensate production method>

[0243] The present invention relates to a method for producing a bisphenol-alkyl carbonate condensate represented by the following formula (III), wherein a polycarbonate resin is decomposed in the presence of a dialkyl carbonate, an aliphatic monohydric alcohol, and a catalyst selected from the group consisting of an alkali metal hydroxide, an alkali metal carbonate, an alkali metal alkoxide, an alkali metal oxide, a chain alkylamine, and pyridine (hereinafter sometimes described as "the method for producing the condensate of the present invention").

[0244] [Chemistry 9]

[0245]

[0246] In formula (III), R is methyl, ethyl or butyl.

[0247] In the method for producing a condensate of the present invention, a polycarbonate resin is decomposed in the presence of a dialkyl carbonate, an aliphatic monohydric alcohol, and any one catalyst selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal alkoxides, alkali metal oxides, chain alkylamines, and pyridine.

[0248] The types and amounts of the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst, reaction temperature, reaction time, etc. used in the method for producing the condensate of the present invention are the same as those of the method for producing bisphenol of the present invention, and the preferred embodiment is also the same. In addition, similar to the method for producing bisphenol of the present invention, the method for producing the condensate of the present invention preferably decomposes the polycarbonate resin in a slurry-like reaction solution containing the polycarbonate resin, dialkyl carbonate, aliphatic monohydric alcohol and catalyst.

[0249] As described above, in the bisphenol production method of the present invention, the amount of aliphatic monohydric alcohol and the reaction time can be adjusted to produce a bisphenol-alkyl carbonate condensate as a byproduct. By recovering the bisphenol-alkyl carbonate condensate, a bisphenol-alkyl carbonate condensate can be obtained. The recovery of the bisphenol-alkyl carbonate condensate is as described above.

[0250] In order to more efficiently produce the bisphenol-alkyl carbonate condensate, the molar ratio of the aliphatic monohydric alcohol used to 1 mol of the repeating unit of the polycarbonate resin used is preferably less than 2.0, and can be 1.95 or less, 1.9 or less, 1.85 or less, 1.8 or less, etc.

[0251] In addition, a bisphenol-alkyl carbonate condensate can be obtained by shortening the reaction time.

[0252] Bisphenol-alkyl carbonate condensates can use alkyl carbonate as a protective group, so different functional groups can be selectively introduced into the two hydroxyl groups of bisphenol to derive new products.

[0253] <Method for producing recycled polycarbonate resin of the present invention>

[0254] The present invention relates to a method for producing a recycled polycarbonate resin using a bisphenol raw material containing bisphenol (recycled bisphenol) obtained by the bisphenol production method of the present invention to produce a recycled polycarbonate resin (hereinafter, sometimes described as "the recycled polycarbonate resin production method of the present invention"). The recycled polycarbonate resin production method of the present invention is a method using a chemical recycling method, and the chemical recycling method uses recycled bisphenol obtained by decomposing a polycarbonate resin contained in waste plastics etc. into bisphenol as a monomer as a raw material to produce a polycarbonate resin.

[0255] The polycarbonate resin production method of the present invention can be carried out by appropriately selecting a known polycarbonate resin polymerization method, except that a bisphenol raw material containing recycled bisphenol is used as bisphenol. Polycarbonate resin is generally produced by polymerizing bisphenol and a carbonic acid diester in the presence of a catalyst.

[0256] In the method for producing a recycled polycarbonate resin of the present invention, the recycled polycarbonate resin can be obtained, for example, by polymerizing a bisphenol raw material containing recycled bisphenol (bisphenol obtained by the method for producing bisphenol of the present invention) and a carbonic acid diester raw material.

[0257] For example, the recycled polycarbonate resin can be produced by a method in which a bisphenol raw material containing recycled bisphenol and a carbonic acid diester raw material such as diphenyl carbonate are subjected to an ester exchange reaction in the presence of an alkali metal compound and / or an alkaline earth metal compound.

[0258] Regenerated bisphenol can be used as the whole bisphenol raw material, or it can be mixed with general bisphenol other than recycled bisphenol and used as a part of the bisphenol raw material. The amount of recycled bisphenol is not particularly limited, and can be any amount such as 0.1% by mass or more, 1% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more. The higher the proportion of recycled bisphenol, the more environmentally friendly it is, so from the perspective of environmental considerations, the amount of recycled bisphenol relative to the bisphenol raw material is preferably large.

[0259] The above-mentioned transesterification reaction can be carried out by appropriately selecting a known method, and an example of a method using diphenyl carbonate as a carbonic acid diester raw material is described below.

[0260] In the method for producing a regenerated polycarbonate resin of the present invention, diphenyl carbonate is preferably used in excess relative to the bisphenol raw material. From the perspective of fewer terminal hydroxyl groups in the produced regenerated polycarbonate resin and excellent thermal stability of the polymer, the amount of diphenyl carbonate used relative to the bisphenol raw material is preferably large, and from the perspective of fast transesterification reaction speed and easy production of a regenerated polycarbonate resin of a desired molecular weight, it is preferably small. Thus, relative to 1 mole of the used bisphenol raw material, the amount of diphenyl carbonate used is usually 1.001 moles or more, preferably 1.002 moles or more, and is usually 1.3 moles or less, preferably 1.2 moles or less.

[0261] As a method for supplying the raw materials, the bisphenol raw material and diphenyl carbonate may be supplied in solid form, but it is preferred that one or both of them be melted and supplied in a liquid state.

[0262] When the regenerated polycarbonate resin is produced by the transesterification reaction of diphenyl carbonate and bisphenol raw materials, a transesterification catalyst is usually used. As the transesterification catalyst, an alkali metal compound and / or an alkaline earth metal compound is preferably used. They can be used alone or in any combination and ratio. In practical applications, an alkali metal compound is preferably used.

[0263] The amount of the catalyst used is usually 0.05 μmol or more, preferably 0.08 μmol or more, more preferably 0.10 μmol or more, and usually 100 μmol or less, preferably 50 μmol or less, more preferably 20 μmol or less, per 1 mol of the bisphenol raw material or diphenyl carbonate.

[0264] By setting the amount of the catalyst used within the above range, the polymerization activity required for producing a regenerated polycarbonate resin having a desired molecular weight can be easily obtained, and the polymer hue is excellent. In addition, the polymer branching does not excessively proceed, and a polycarbonate resin having excellent fluidity during molding can be easily obtained.

[0265] In order to produce the regenerated polycarbonate resin by the above method, it is preferred that the above two raw materials are continuously supplied to a raw material mixing tank, and the obtained mixture and the transesterification catalyst are continuously supplied to a polymerization tank.

[0266] When a regenerated polycarbonate resin is produced by the transesterification method, generally, two raw materials supplied to a raw material mixing tank are uniformly stirred and then supplied to a polymerization tank to which a catalyst is added to produce a polymer.

[0267] (Recycled polycarbonate resin and composition thereof)

[0268] The regenerated polycarbonate resin obtained by the regenerated polycarbonate resin manufacturing method of the present invention can be used directly, and can also be used as a regenerated polycarbonate resin composition containing unused polycarbonate resin and regenerated polycarbonate resin. The regenerated polycarbonate resin composition can be obtained by appropriately selecting a known mixing method, etc., and mixing unused polycarbonate resin and regenerated polycarbonate resin. In the case of making a regenerated polycarbonate resin composition containing unused polycarbonate resin and regenerated polycarbonate resin, the amount of the regenerated polycarbonate resin is not particularly limited, and the more the proportion of the regenerated polycarbonate resin, the more environmentally friendly. Therefore, from the viewpoint of considering the environment, the amount of the regenerated polycarbonate resin relative to the regenerated polycarbonate resin composition is preferably 50% by mass or more, and the larger the order of 70% by mass or more, 80% by mass or more, and 90% by mass or more is more preferred.

[0269] The obtained recycled polycarbonate resin and composition can be molded into various molded products such as optical members and optical recording media in the same manner as unused polycarbonate resin.

[0270] <Epoxy resin production method>

[0271] The present invention relates to a method for producing an epoxy resin, wherein bisphenol is obtained by the bisphenol production method of the present invention, and then an epoxy resin is produced using a polyhydroxy compound raw material containing the bisphenol. In addition, the present invention also relates to a method for producing an epoxy resin, wherein an epoxy resin raw material containing the epoxy resin obtained by the epoxy resin production method is further reacted with a polyhydroxy compound raw material to produce an epoxy resin.

[0272] In the method for producing an epoxy resin of the present invention, an epoxy resin (hereinafter sometimes referred to as "regenerated epoxy resin") is produced using recycled bisphenol and / or an epoxy resin produced using recycled bisphenol as at least a part of the raw materials.

[0273] The epoxy resin production method of the present invention is not particularly limited except that the regenerated bisphenol (the bisphenol obtained by the bisphenol production method of the present invention) and / or the epoxy resin produced by using the regenerated bisphenol is used as a raw material, and a known production method can be used. For example, as described later, the regenerated bisphenol can be used as at least a part of the polyol raw material when the one-step method, oxidation method, or two-step method is used for production. The obtained epoxy resin can also be used as at least a part of the epoxy resin raw material when the two-step method is used for production.

[0274] It should be noted that "epoxy resin raw material" refers to the epoxy resin used as a raw material for the epoxy resin production method of the present invention. "Polyhydroxy compound" is a general term for phenolic compounds with a valence of 2 or more and alcohol compounds with a valence of 2 or more, and "polyhydroxy compound raw material" refers to a polyhydroxy compound used as a raw material for the epoxy resin production method of the present invention.

[0275] As the method for producing the epoxy resin of the present invention, a one-step method, an oxidation method, a two-step method, etc. can be utilized.

[0276] The method for producing an epoxy resin by a one-step process is a method for producing an epoxy resin by reacting a regenerated bisphenol (the bisphenol obtained by the method for producing a bisphenol of the present invention) with an epihalohydrin.

[0277] The method for producing epoxy resin by oxidation is a method in which regenerated bisphenol is allylated using an allyl halide (allyl chloride, allyl bromide, etc.) and then subjected to an oxidation reaction to obtain an epoxy resin.

[0278] The method for producing an epoxy resin by a two-step process is a method of reacting an epoxy resin raw material with a polyol raw material, and as the raw material, recycled bisphenol and / or an epoxy resin produced using recycled bisphenol is used.

[0279] Hereinafter, methods for producing epoxy resins by a one-step method, an oxidation method, and a two-step method will be described.

[0280] (Method for producing epoxy resin using a one-step process)

[0281] In the present invention, the method for producing the epoxy resin by the one-step method is not particularly limited as long as it is a known production method, and is described in detail below.

[0282] The epoxy resin production method using the one-step method can also be produced by using a polyol other than the regenerated bisphenol (hereinafter sometimes referred to as "other polyols") in combination with the regenerated bisphenol. That is, the epoxy resin production method using the one-step method is a method for obtaining an epoxy resin by reacting a polyol raw material with an epihalohydrin, and at least a part of the polyol raw material can be a method of regenerated bisphenol.

[0283] The content of the recycled bisphenol in the polyol raw material is not particularly limited, but a higher content of the recycled bisphenol is environmentally friendly, so it is preferably 1 to 100% by mass, more preferably 10 to 100% by mass.

[0284] Here, "other polyols" is a general term for divalent or higher phenolic compounds and divalent or higher alcohol compounds other than recycled bisphenol. In the one-step method for producing epoxy resin, "polyol raw materials" are all polyols obtained by combining recycled bisphenol and other polyols used as needed.

[0285] Examples of other polyhydroxy compounds include bisphenol A, tetramethylbisphenol A, bisphenol F, tetramethylbisphenol F, bisphenol S, bisphenol C, bisphenol AD, bisphenol AF, hydroquinone, resorcinol, methylresorcinol, biphenol, tetramethylbiphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resins, cresol novolac resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A novolac resins, naphthol novolac resins, brominated bisphenol A, brominated phenol novolac resins, and various polyphenols such as benzaldehyde and hydroxyl groups. Various phenolic resins such as polyphenol resins obtained by condensation reaction of various aldehydes such as benzaldehyde, crotonaldehyde, and glyoxal, polyphenol resins obtained by condensation reaction of xylene resin and phenols, co-condensation resins of heavy oil or asphalt with phenols and formaldehyde, chain aliphatic diols such as ethylene glycol, trimethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol, cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol, polyalkylene ether glycols such as polyethylene ether glycol, polyoxytrimethylene ether glycol, and polypropylene ether glycol, etc.

[0286] During the reaction, the polyhydroxy compound raw material is dissolved in epihalohydrin to prepare a uniform solution. As the epihalohydrin, epichlorohydrin or epibromohydrin is generally used, and epichlorohydrin is preferred in the present invention.

[0287] Relative to 1 equivalent of hydroxyl group of polyol raw material (all polyols), the usage amount of epihalohydrin is preferably equivalent to 1.0~14.0 equivalents, particularly 2.0~10.0 equivalents. When the amount of epihalohydrin is above the above lower limit, it is easy to control the high molecular weight reaction, and the epoxy resin obtained can be made to be a suitable epoxy equivalent, so it is preferred. On the other hand, when the amount of epihalohydrin is below the above upper limit, there is a tendency to improve production efficiency, so it is preferred.

[0288] Next, while stirring the above solution, an alkali metal hydroxide in an amount equivalent to usually 0.1 to 3.0 equivalents, preferably 0.8 to 2.0 equivalents, of hydroxyl groups of the polyol raw material is added in the form of a solid or aqueous solution and reacted. When the amount of the alkali metal hydroxide added is above the above lower limit, the unreacted hydroxyl groups are not easy to react with the generated epoxy resin, and the high molecular weight reaction is easy to control, so it is preferred. In addition, when the amount of the alkali metal hydroxide added is below the above upper limit, impurities caused by side reactions are not easy to be generated, so it is preferred. As the alkali metal hydroxide used here, sodium hydroxide or potassium hydroxide can be generally mentioned.

[0289] The reaction can be carried out under normal pressure or reduced pressure, and the reaction temperature is preferably 20 to 200° C., more preferably 40 to 150° C. When the reaction temperature is above the lower limit, the reaction is easy to proceed and the reaction is easy to control, so it is preferred. In addition, when the reaction temperature is below the upper limit, side reactions are not easy to proceed, and it is particularly easy to reduce the amount of polymer, so it is preferred.

[0290] In addition, the reaction is carried out while dehydrating by the following method: the reaction solution is azeotroped while maintaining a specified temperature as needed, the condensate obtained by cooling the volatilized steam is subjected to oil / water separation, and the oil from which the water is removed is returned to the reaction system. In order to suppress the rapid reaction, the alkali metal hydroxide is preferably added intermittently or continuously in small amounts for 0.1 to 24 hours, more preferably for 0.5 to 10 hours. When the addition time of the alkali metal hydroxide is above the above lower limit, it is possible to prevent the reaction from proceeding rapidly, and the control of the reaction temperature becomes easy, so it is preferred. When the addition time is below the above upper limit, it is easy to reduce the amount of polymer, so it is preferred.

[0291] After the reaction is completed, the insoluble by-product salts can be removed by filtering or washing with water, and then the unreacted epihalohydrin can be removed by distilling off by heating and / or distilling under reduced pressure.

[0292] In this reaction, catalysts such as quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide, tertiary amines such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol, imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole, phosphonium salts such as ethyltriphenylphosphonium iodide, and phosphines such as triphenylphosphine can also be used.

[0293] Furthermore, in the reaction, an inert organic solvent may be used, such as alcohols such as ethanol and isopropanol, ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone, ethers such as dioxane and ethylene glycol dimethyl ether, glycol ethers such as methoxypropanol, and aprotic polar solvents such as dimethyl sulfoxide and dimethylformamide.

[0294] [Manufacture of epoxy resin with reduced total chlorine content]

[0295] When it is necessary to reduce the total chlorine content of the epoxy resin obtained as described above, the epoxy resin having a reduced total chlorine content can be produced by reacting with a base.

[0296] In the reaction with the base, an organic solvent for dissolving the epoxy resin can be used. The organic solvent used in the reaction is not particularly limited, and from the perspectives of manufacturing efficiency, operability, and workability, a ketone-based organic solvent is preferably used. In addition, from the perspective of further reducing the amount of hydrolyzable chlorine, an aprotic polar solvent can be used.

[0297] Examples of ketone organic solvents include methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone and the like. Methyl isobutyl ketone is particularly preferred in terms of effect and ease of post-treatment. These may be used alone or in combination of two or more.

[0298] As aprotic polar solvent, for example, dimethyl sulfoxide, diethyl sulfoxide, dimethyl sulfone, cyclopentane, dimethylformamide, dimethylacetamide, hexamethylphosphoramide etc. can be listed. They can be used alone or in combination of two or more. Among these aprotic polar solvents, dimethyl sulfoxide is preferred from the aspect of being easy to obtain and having excellent effect.

[0299] The amount of the solvent used is such that the concentration of the epoxy resin in the liquid subjected to the treatment with the alkali is generally 1 to 95% by mass, preferably 5 to 80% by mass.

[0300] As the base, a solid or solution of an alkali metal hydroxide can be used. As the alkali metal hydroxide, potassium hydroxide, sodium hydroxide, etc. can be mentioned, preferably sodium hydroxide. In addition, the alkali metal hydroxide can also be used as an alkali metal hydroxide dissolved in an organic solvent or water. It is preferably used in the form of a solution formed by dissolving the alkali metal hydroxide in an aqueous solvent or an organic solvent.

[0301] The amount of the alkali metal hydroxide used is preferably 0.01 to 20.0 parts by mass relative to 100 parts by mass of the epoxy resin, calculated as the solid content of the alkali metal hydroxide. More preferably, it is 0.10 to 10.0 parts by mass. When the amount of the alkali metal hydroxide is below the above lower limit, the effect of reducing the total chlorine content is low. In addition, when it is above the above upper limit, a large amount of polymer is generated, so the yield is reduced.

[0302] The reaction temperature is preferably 20 to 200° C., more preferably 40 to 150° C., and the reaction time is preferably 0.1 to 24 hours, more preferably 0.5 to 10 hours.

[0303] After the reaction, the excess alkali metal hydroxide and by-product salts can be removed by washing with water or the like, and the organic solvent can be removed by heating and / or distillation under reduced pressure and / or steam distillation.

[0304] (Method for producing epoxy resin by oxidation method)

[0305] The method for producing the epoxy resin by oxidation is not particularly limited as long as it is a known production method, and can be carried out according to the methods described in, for example, JP-A-2011-225711, JP-A-2012-092247, JP-A-2012-111858, and the like.

[0306] In the method for producing epoxy resin by oxidation, other polyols other than recycled bisphenol may be used in combination with recycled bisphenol, as in the one-step method. That is, the method for producing epoxy resin by oxidation is a method of obtaining epoxy resin by allylating a polyol raw material with an allyl halide and then subjecting it to oxidation reaction, and at least a part of the polyol raw material may be recycled bisphenol.

[0307] In the method for producing epoxy resin by oxidation, the "polyhydroxy compound raw material" refers to all polyhydroxy compounds after the regenerated bisphenol and other polyhydroxy compounds used as needed are combined. As other polyhydroxy compounds, the same compounds as those in the one-step method can be cited. The content of the regenerated bisphenol in the polyhydroxy compound raw material is not particularly limited, and since a high content of the regenerated bisphenol is environmentally friendly, it is preferably 1 to 100% by mass, and more preferably 10 to 100% by mass.

[0308] (Method for producing epoxy resin using two-step method)

[0309] The method for producing the epoxy resin by the two-step method is not particularly limited as long as it is a known production method, and will be described in detail below.

[0310] The method for producing an epoxy resin using a two-step process may be a method comprising a step of reacting an epoxy resin raw material with a polyol raw material, wherein at least a portion of the epoxy resin raw material is an epoxy resin produced using recycled bisphenol, and / or at least a portion of the polyol raw material is recycled bisphenol. The method for producing an epoxy resin using a two-step process may be any one of the following methods (i) to (iii).

[0311] Method (i): A method of reacting an epoxy resin other than the epoxy resin produced using recycled bisphenol with a polyol raw material containing recycled bisphenol.

[0312] In the method (i), the epoxy resin raw material is an epoxy resin other than the epoxy resin produced using recycled bisphenol. In addition, the polyol raw material is all polyols obtained by combining recycled bisphenol and other polyols used as necessary.

[0313] Method (ii): A method in which an epoxy resin raw material containing an epoxy resin produced using recycled bisphenol is reacted with a polyol raw material containing recycled bisphenol.

[0314] In method (ii), the epoxy resin raw material is the total epoxy resin obtained by combining the epoxy resin produced using recycled bisphenol and other epoxy resins used as needed. Also, the polyol raw material is the total polyol obtained by combining the recycled bisphenol and other polyols used as needed.

[0315] Method (iii): A method of reacting an epoxy resin raw material containing an epoxy resin produced using recycled bisphenol with a polyol other than recycled bisphenol.

[0316] In the method (iii), the epoxy resin raw material is the total epoxy resin obtained by combining the epoxy resin produced using recycled bisphenol and other epoxy resins used as required. In addition, the polyol raw material is a polyol other than recycled bisphenol.

[0317] The epoxy resin produced using the regenerated bisphenol used in method (ii) and method (iii) can be obtained by a one-step method for producing an epoxy resin or an oxidation method for producing an epoxy resin. In addition, the epoxy resin obtained by method (i) can be used. It should be noted that other epoxy resins other than the epoxy resin produced using the regenerated bisphenol are the same as other epoxy resins described later in the method for producing epoxy resin cured products, and other polyhydroxy compounds are the same as the one-step method.

[0318] In the methods (i) and (ii), the content of recycled bisphenol in the recycled bisphenol-containing polyol is not particularly limited, but a higher content of recycled bisphenol is more environmentally friendly, and therefore, it is preferably 1 to 100% by mass, more preferably 10 to 100% by mass.

[0319] In the method (ii) and the method (iii), the content of the epoxy resin produced using recycled bisphenol in the epoxy resin raw material containing the epoxy resin produced using recycled bisphenol is not particularly limited. A higher content of the epoxy resin produced using recycled bisphenol is more environmentally friendly, and therefore, it is preferably 1 to 100% by mass, and more preferably 10 to 100% by mass.

[0320] In the two-step reaction, the amount of the epoxy resin raw material and the polyol raw material used is preferably (epoxy equivalent) : (hydroxyl equivalent) = 1: 0.1 to 2.0 in terms of the equivalent ratio. More preferably, it is 1: 0.2 to 1.2. When the equivalent ratio is within the above range, it is easy to increase the molecular weight and more epoxy terminal groups can remain, so it is preferred.

[0321] In addition, a catalyst can be used in the reaction utilizing the two-step method. As the catalyst, any catalyst can be used as long as it is a compound having a catalytic ability to promote the reaction of an epoxy group with a phenolic hydroxyl group or an alcoholic hydroxyl group. For example, alkali metal compounds, organophosphorus compounds, tertiary amines, quaternary ammonium salts, cyclic amines, imidazoles, etc. can be cited. Among them, quaternary ammonium salts are preferred. In addition, the catalyst can be used in one species only, or in combination of two or more species. The amount of the catalyst used is usually 0.001 to 10% by mass relative to the epoxy resin raw material.

[0322] In addition, in the reaction utilizing the two-step method, a solvent can be used. As the solvent, any solvent can be used as long as it is a solvent that dissolves the epoxy resin raw material. For example, aromatic solvents, ketone solvents, amide solvents, glycol ether solvents, etc. can be cited. Only one solvent can be used, or two or more solvents can be used in combination. In addition, the resin concentration in the solvent is preferably 10 to 95% by mass. More preferably, it is 20 to 80% by mass. In addition, when a high-viscosity product is produced midway in the reaction, a solvent can also be added to continue the reaction. After the reaction is completed, the solvent can be removed as needed, or it can be further added.

[0323] In the reaction using the two-step method, the reaction temperature is preferably 20 to 250° C., more preferably 50 to 200° C. When the reaction temperature is above the upper limit, the generated epoxy resin may be degraded. In addition, when it is below the lower limit, the reaction may not proceed sufficiently. In addition, the reaction time is usually 0.1 to 24 hours, preferably 0.5 to 12 hours.

[0324] <Method for producing cured epoxy resin>

[0325] The method for producing a cured epoxy resin of the present invention is to obtain an epoxy resin by the above-mentioned epoxy resin production method, obtain a composition containing the epoxy resin and a curing agent (hereinafter sometimes referred to as an "epoxy resin composition"), and then cure the epoxy resin composition to obtain a cured epoxy resin.

[0326] Furthermore, other epoxy resins other than the epoxy resin obtained by the epoxy resin production method of the present invention (hereinafter sometimes simply referred to as "other epoxy resins"), curing agents, curing accelerators, inorganic fillers, coupling agents, etc. may be appropriately blended into the epoxy resin composition as necessary.

[0327] The content of the regenerated epoxy resin in the epoxy resin composition is not particularly limited. A high content of the regenerated epoxy resin is environmentally friendly, so the regenerated epoxy resin is preferably 40 parts by mass or more, more preferably 60 parts by mass or more, relative to 100 parts by mass of all epoxy resin components in the epoxy resin composition. In the case of containing other epoxy resins, the regenerated epoxy resin can be 40 to 99 parts by mass, 60 to 99 parts by mass, etc., relative to 100 parts by mass of all epoxy resin components in the epoxy resin composition. It should be noted that "all epoxy resin components" are equivalent to the amount of all epoxy resins contained in the epoxy resin composition, which is the total of the regenerated epoxy resin and other epoxy resins used as needed.

[0328] (Curing agent)

[0329] In the present invention, the curing agent refers to a substance that contributes to the cross-linking reaction and / or chain extension reaction between epoxy groups of the epoxy resin. It should be noted that in the present invention, even a substance generally referred to as a "curing accelerator" is regarded as a curing agent as long as it contributes to the cross-linking reaction and / or chain extension reaction between epoxy groups of the epoxy resin.

[0330] In the epoxy resin composition, the content of the curing agent is preferably 0.1 to 1000 parts by mass based on 100 parts by mass of the total epoxy resin component, and more preferably 500 parts by mass or less.

[0331] As a curing agent, there is no particular limitation, and all curing agents known as epoxy resin curing agents can be used. For example, amine curing agents such as phenolic curing agents, aliphatic amines, polyetheramines, alicyclic amines, aromatic amines, acid anhydride curing agents, amide curing agents, tertiary amines, imidazoles, etc. can be listed. One curing agent can be used alone, or two or more can be used in combination. When two or more curing agents are used in combination, they can be pre-mixed and used after preparing a mixed curing agent, or when the regenerated epoxy resin obtained by the epoxy resin manufacturing method of the present invention and the components of other epoxy resins are mixed, the components of the curing agent can be added separately and mixed simultaneously.

[0332] [Phenolic curing agent]

[0333] Specific examples of phenolic curing agents include recycled bisphenol, bisphenol A, tetramethyl bisphenol A, bisphenol F, tetramethyl bisphenol F, bisphenol C, bisphenol S, bisphenol AD, bisphenol AF, hydroquinone, resorcinol, methyl resorcinol, biphenol, tetramethyl biphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resin, cresol novolac resin, phenol aralkyl resin, biphenyl aralkyl resin, naphthol aralkyl resin, terpene phenol resin, dicyclopentadiene phenol resin, bisphenol A novolac resin, trisphenol methane type resin, naphthol novolac resin, brominated bisphenol A , various polyphenols such as brominated phenol novolac resins, polyphenol resins obtained by condensation reaction of various phenols with various aldehydes such as benzaldehyde, hydroxybenzaldehyde, crotonaldehyde, and glyoxal, polyphenol resins obtained by condensation reaction of xylene resins and phenols, co-condensation resins of heavy oil or asphalt with phenols and formaldehydes, phenol·benzaldehyde·xylene dimethanol condensation products, phenol·benzaldehyde·xylylene dihalide condensation products, phenol·benzaldehyde·4,4'-dimethanol biphenyl condensation products, phenol·benzaldehyde·4,4'-dihalide biphenyl condensation products and other phenol resins.

[0334] These phenolic curing agents may be used alone or in combination of two or more in any combination and in any blending ratio.

[0335] The amount of the phenolic curing agent added is preferably 0.1 to 1000 parts by mass, more preferably 500 parts by mass or less, based on 100 parts by mass of the total epoxy resin components in the epoxy resin composition.

[0336] [Amine curing agent]

[0337] Examples of the amine-based curing agent (excluding tertiary amines) include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines.

[0338] Examples of the aliphatic amines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminopropane, hexamethylenediamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-hydroxyethylethylenediamine, and tetrakis(hydroxyethyl)ethylenediamine.

[0339] Examples of the polyetheramines include triethylene glycol diamine, tetraethylene glycol diamine, diethylene glycol bis(propylamine), polyoxypropylene diamine, and polyoxypropylene triamine.

[0340] Examples of the alicyclic amines include isophoronediamine, menthanediamine, N-aminoethylpiperazine, bis(4-amino-3-methyldicyclohexyl)methane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, and norbornenediamine.

[0341] Examples of the aromatic amines include tetrachloro-p-xylylenediamine, m-xylylenediamine, p-xylylenediamine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, 2,4-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, m-aminophenol, m-aminobenzylamine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethanolamine, methylbenzylamine, α-(m-aminophenyl)ethylamine, α-(p-aminophenyl)ethylamine, diaminodiethyldimethyldiphenylmethane, and α,α'-bis(4-aminophenyl)-p-diisopropylbenzene.

[0342] The amine curing agents listed above may be used alone or in combination of two or more in any combination and in any mixing ratio.

[0343] The above-mentioned amine curing agent is preferably used in a manner that the equivalent ratio of the functional group in the curing agent to the epoxy group in all epoxy resin components contained in the epoxy resin composition is in the range of 0.1 to 2.0. More preferably, the equivalent ratio is in the range of 0.8 to 1.2. When it is within this range, unreacted epoxy groups and functional groups of the curing agent are unlikely to remain, so it is preferred.

[0344] [Tertiary amine]

[0345] Examples of the tertiary amine include 1,8-diazabicyclo(5,4,0)undecene-7, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol.

[0346] The tertiary amines listed above may be used alone or in combination of two or more in any combination and in any mixing ratio.

[0347] The tertiary amine is preferably used in a manner such that the equivalent ratio of the functional group in the curing agent to the epoxy group in all epoxy resin components contained in the epoxy resin composition is in the range of 0.1 to 2.0. More preferably, the equivalent ratio is in the range of 0.8 to 1.2. Within this range, unreacted epoxy groups and functional groups of the curing agent are unlikely to remain, so it is preferred.

[0348] [Anhydride curing agent]

[0349] Examples of the acid anhydride-based curing agent include acid anhydrides and modified products of acid anhydrides.

[0350] Examples of the acid anhydride include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic anhydride, dodecenylsuccinic anhydride, polyadipic anhydride, polyazelaic anhydride, polysebacic anhydride, poly(ethyloctadecane dioic acid) anhydride, poly(phenylhexadecane dioic acid) anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, methylnadic anhydride, and trialkyltetrahydrophthalic anhydride. , methylcyclohexene dicarboxylic anhydride, methylcyclohexene tetracarboxylic anhydride, ethylene glycol ditrimellitate dianhydride, chlorobridged anhydride, nadic anhydride, methyl nadic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexane-1,2-dicarboxylic anhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, 1-methyl-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic anhydride, etc.

[0351] As modified products of acid anhydrides, for example, substances obtained by modifying the above acid anhydrides with diols can be cited. Here, as examples of diols that can be used for modification, alkylene glycols such as ethylene glycol, propylene glycol, and neopentyl glycol, polyether diols such as polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol can be cited. Furthermore, copolymerized polyether diols of two or more diols and / or polyether diols among them can also be used.

[0352] The acid anhydride curing agents listed above may be used alone or in combination of two or more in any combination and in any amount.

[0353] When an anhydride curing agent is used, it is preferably used in a manner that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components in the epoxy resin composition is in the range of 0.1 to 2.0. More preferably, the equivalent ratio is in the range of 0.8 to 1.2. When it is within this range, unreacted epoxy groups and functional groups of the curing agent are unlikely to remain, so it is preferred.

[0354] [Amide curing agent]

[0355] As the amide curing agent, dicyandiamide and its derivatives, polyamide resins, etc. can be mentioned. Only one amide curing agent can be used, or two or more amide curing agents can be mixed and used in any combination and ratio. When using an amide curing agent, it is preferably used in a manner that the total amount of the amide curing agent relative to the total epoxy resin component and the amide curing agent in the epoxy resin composition is 0.1 to 20 mass %.

[0356] [Imidazoles]

[0357] Examples of the imidazoles include 2-phenylimidazole, 2-ethyl-4(5)-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-( 1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and the above imidazoles. It should be noted that imidazoles have catalytic ability and are therefore generally classified as curing accelerators, but are classified as curing agents in the present invention.

[0358] The above-mentioned imidazoles may be used alone or in combination of two or more in any ratio.

[0359] When using imidazoles, it is preferable to use imidazoles so that the total amount of imidazoles is 0.1 to 20% by mass based on the total amount of all epoxy resin components and imidazoles in the epoxy resin composition.

[0360] [Other curing agents]

[0361] In the epoxy resin composition, in addition to the above-mentioned curing agent, other curing agents may be used. There are no particular limitations on other curing agents that can be used in the epoxy resin composition, and all curing agents generally known as curing agents for epoxy resins may be used.

[0362] These other curing agents may be used alone or in combination of two or more.

[0363] [Other epoxy resins]

[0364] The epoxy resin composition may contain other epoxy resins other than the epoxy resin obtained by the epoxy resin production method of the present invention. By containing other epoxy resins, various physical properties can be improved.

[0365] Other epoxy resins that can be used in the epoxy resin composition correspond to all epoxy resins other than the epoxy resin obtained by the epoxy resin production method of the present invention. Specific examples include bisphenol A type epoxy resin, bisphenol C type epoxy resin, trisphenol methane type epoxy resin, anthracene type epoxy resin, phenol modified xylene resin type epoxy resin, bisphenol cyclododecyl type epoxy resin, bisphenol diisopropylidene resorcinol type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, bisphenol AF type epoxy resin, hydroquinone type epoxy resin, methyl hydroquinone type epoxy resin, dibutyl hydroquinone type epoxy resin, resorcinol type epoxy resin, methyl resorcinol type epoxy resin, biphenol type epoxy resin, tetramethyl biphenol type epoxy resin, tetramethyl bisphenol F type epoxy resin, dihydroxy diphenyl ether type epoxy resin, epoxy resin derived from thiodiphenol, dihydroxy naphthalene type epoxy resin, dihydroxy anthracene type epoxy resin, dihydroxy dihydroanthracene type epoxy resin, dicyclopentadiene type epoxy resin, epoxy resin derived from dihydroxy Epoxy resins derived from stilbene, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, terpene phenol type epoxy resins, dicyclopentadiene phenol type epoxy resins, epoxy resins derived from condensates of phenol-hydroxybenzaldehyde, epoxy resins derived from condensates of phenol-crotonaldehyde, epoxy resins derived from condensates of phenol-glyoxal, epoxy resins derived from co-condensation resins of heavy oil or asphalt with phenols and formaldehyde, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenol, epoxy resins derived from xylene dimethylamine, epoxy resins derived from methylhexahydrophthalic acid, epoxy resins derived from dimer acid, etc. These may be used alone or in any combination and in any blending ratio.

[0366] When the epoxy resin composition contains the above-mentioned other epoxy resin, the content thereof is preferably 1 to 60 parts by mass, more preferably 40 parts by mass or less, based on 100 parts by mass of all epoxy resin components in the composition.

[0367] (Curing accelerator)

[0368] The epoxy resin composition preferably contains a curing accelerator. By containing a curing accelerator, the curing time can be shortened and the curing temperature can be lowered, and a desired cured product can be easily obtained.

[0369] The curing accelerator is not particularly limited, and specific examples thereof include organic phosphines, phosphorus compounds such as phosphonium salts, tetraphenylborate salts, organic acid dihydrazides, and boron halide amine complexes.

[0370] Examples of phosphorus compounds that can be used as a curing accelerator include organic phosphines such as triphenylphosphine, diphenyl (p-tolyl) phosphine, tri(alkylphenyl)phosphine, tri(alkoxyphenyl)phosphine, tri(alkyl-alkoxyphenyl)phosphine, tri(dialkylphenyl)phosphine, tri(trialkylphenyl)phosphine, tri(tetraalkylphenyl)phosphine, tri(dialkoxyphenyl)phosphine, tri(trialkoxyphenyl)phosphine, tri(tetraalkoxyphenyl)phosphine, trialkylphosphine, dialkylarylphosphine, and alkyldiarylphosphine, or complexes of these organic phosphines with organic boron, compounds obtained by adding these organic phosphines to quinone compounds such as maleic anhydride, 1,4-benzoquinone, 2,5-methylbenzoquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone, and compounds such as diazonophenylmethane.

[0371] Among the curing accelerators listed above, organic phosphines and phosphonium salts are preferred, and organic phosphines are most preferred. In addition, the curing accelerator may be one of the curing accelerators listed above, or two or more of them may be mixed in any combination and ratio.

[0372] The curing accelerator is preferably used in an amount of 0.1 to 20 parts by mass relative to 100 parts by mass of all epoxy resin components in the epoxy resin composition. When the content of the curing accelerator is above the above lower limit, a good curing acceleration effect can be obtained. On the other hand, when it is below the above upper limit, it is easy to obtain desired cured properties, so it is preferred.

[0373] (Inorganic filler)

[0374] Inorganic fillers can be added to the epoxy resin composition. Examples of inorganic fillers include fused silica, crystalline silica, glass powder, aluminum oxide, calcium carbonate, calcium sulfate, talc, boron nitride, and the like. Only one of these can be used, or two or more can be used in any combination and mixing ratio. The amount of the inorganic filler is preferably 10 to 95% by mass of the entire epoxy resin composition.

[0375] (Release Agent)

[0376] A release agent may be added to the epoxy resin composition. As the release agent, for example, natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid and zinc stearate and their metal salts, hydrocarbon-based release agents such as paraffin wax may be used. These may be used alone or in combination of two or more in any combination and mixing ratio.

[0377] The amount of the release agent is preferably 0.001 to 10.0 parts by mass based on 100 parts by mass of the total epoxy resin component in the epoxy resin composition. When the amount of the release agent is within the above range, good release properties can be exhibited while maintaining curing characteristics, which is preferred.

[0378] (Coupling agent)

[0379] The epoxy resin composition may be mixed with a coupling agent. The coupling agent is preferably used together with an inorganic filler. By mixing with the coupling agent, the adhesion between the epoxy resin as a matrix and the inorganic filler can be improved. Examples of the coupling agent include silane coupling agents, titanate coupling agents, and the like.

[0380] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino silanes such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane, mercaptosilanes such as 3-mercaptopropyltrimethoxysilane, p-phenylvinyltrimethoxysilane, vinyltrichlorosilane, vinyltri(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyl silanes such as γ-methacryloxypropyltrimethoxysilane, and epoxy-based, amino-based, and vinyl-based polymer silanes.

[0381] Examples of the titanate coupling agent include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetrakis(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, and bis(dioctyl pyrophosphate)ethylene titanate.

[0382] These coupling agents may be used alone or in combination of two or more in any ratio.

[0383] When a coupling agent is used in the epoxy resin composition, the amount thereof is preferably 0.001 to 10.0 parts by mass relative to 100 parts by mass of the total epoxy resin component. When the amount of the coupling agent is greater than the lower limit, there is a tendency to improve the adhesion between the epoxy resin as the matrix and the inorganic filler by adding the coupling agent. On the other hand, when the amount of the coupling agent is less than the upper limit, the coupling agent is less likely to ooze out from the obtained cured product, so it is preferred.

[0384] (Other ingredients)

[0385] The epoxy resin composition may be mixed with components other than the above. Other components include, for example, flame retardants, plasticizers, reactive diluents, pigments, etc., which may be mixed as needed. However, it does not prevent mixing with components other than the above-mentioned components.

[0386] Examples of the flame retardant include halogen flame retardants such as brominated epoxy resins and brominated phenolic resins, antimony compounds such as antimony trioxide, phosphorus flame retardants such as red phosphorus, phosphates, and phosphines, nitrogen flame retardants such as melamine derivatives, and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0387] (Curing method)

[0388] By curing the epoxy resin composition, an epoxy resin cured product can be obtained. There is no particular limitation on the curing method, and a cured product can usually be obtained by a thermal curing reaction using heating. During the thermal curing reaction, it is preferred to appropriately select the curing temperature according to the type of curing agent used. For example, when a phenolic curing agent is used, the curing temperature is usually 80 to 250°C. In addition, by adding a curing accelerator to these curing agents, the curing temperature can also be lowered. The reaction time is preferably 0.01 to 20 hours. When the reaction time is above the lower limit, there is a tendency for the curing reaction to proceed sufficiently, so it is preferred. On the other hand, when the reaction time is below the upper limit, it is easy to reduce the deterioration caused by heating and the energy loss during heating, so it is preferred.

[0389] (use)

[0390] The epoxy resin cured product obtained by curing the epoxy resin composition has a high elastic modulus at 250° C., and can obtain a cured product having excellent heat deformation resistance.

[0391] Therefore, epoxy resin cured products can be effectively used for any purpose as long as these physical properties are required. For example, they can be suitably used in coating fields such as electrodeposition coatings for automobiles, heavy-duty anti-corrosion coatings for ships and bridges, and coatings for the inner surface coating of beverage cans; in electrical and electronic fields such as laminated boards, semiconductor sealing materials, insulating powder coatings, and coil impregnation; in any of the uses in the fields of earthquake-resistant reinforcement of bridges, concrete reinforcement, floor materials for buildings, linings for water pipe facilities, drainage and permeable pavement, and adhesives for vehicles and aircraft, such as civil engineering, construction, and adhesives.

[0392] The epoxy resin composition may be used after being cured for the above-mentioned applications, or may be cured during the production process for the above-mentioned applications.

[0393] Example

[0394] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. However, the present invention is not limited to the following Examples unless it exceeds the gist of the present invention.

[0395] [Raw materials and reagents]

[0396] As the polycarbonate resin (PC), "NOVAREX (registered trademark) M7027BF" manufactured by Mitsubishi Chemical Engineering-Plastics Corporation was used.

[0397] Reagents obtained from Fujifilm Wako Pure Chemical Industries, Ltd. were used as methanol, dimethyl carbonate, ethanol, diethyl carbonate, butanol, triethylamine, sodium phenolate, sodium hydroxide, potassium hydroxide, acetonitrile, and cesium carbonate.

[0398] As 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), a reagent produced by Tokyo Chemical Industry Co., Ltd. was used.

[0399] Dibutyl carbonate used was a reagent produced by Merck.

[0400] As diphenyl carbonate, a product of Mitsubishi Chemical Corporation was used.

[0401] [analyze]

[0402] The formation confirmation, purity and quantification of bisphenol A were carried out by high performance liquid chromatography under the following steps and conditions.

[0403] Quantitative method: internal standard method with biphenyl as internal standard

[0404] · Equipment: LC-2010A manufactured by Shimadzu Corporation, 5μm 150mm×4.6mmID manufactured by Waters Corporation

[0405] Method: Low-pressure gradient method

[0406] Analysis temperature: 40℃

[0407] ·Eluent composition:

[0408] Liquid A Acetonitrile

[0409] Solution B 85% phosphoric acid: water = 1mL: 999mL solution

[0410] When the analysis time is 0 minutes, the volume ratio of liquid A: liquid B is 35:65 (the same applies below). When the analysis time is 0 to 5 minutes, the eluent composition is made into liquid A: liquid B = 35:65. Then, when the analysis time is 5 to 40 minutes, the liquid A: liquid B is slowly made into 90:10.

[0411] Flow rate: 0.85mL / min

[0412] Detection wavelength: 280nm

[0413] [Viscosity average molecular weight (Mv)]

[0414] The viscosity average molecular weight (Mv) was calculated by dissolving a polycarbonate resin in dichloromethane (concentration: 6.0 g / L) and measuring the specific viscosity (ηsp) at 20° C. using an Ubbelohde viscometer.

[0415] ηsp / C=[η](1+0.28ηsp)

[0416] [η] = 1.23 × 10 -4 Mv 0.83

[0417] [Particle YI]

[0418] The pellet YI (transparency of polycarbonate resin) was evaluated by measuring the YI value (yellowness index value) of polycarbonate resin pellets in reflected light according to ASTM D1925. The apparatus used was a spectrophotometer "CM-5" manufactured by Konica Minolta, Inc., and the measurement conditions were 30 mm measuring diameter and SCE.

[0419] The calibration glass "CM-A212" for petri dish measurement was inserted into the measurement part, and the zero point calibration box "CM-A124" was placed on top of it to perform zero point calibration, and then the built-in white calibration plate was used to perform white calibration. Next, the white calibration plate "CM-A210" was used for measurement, and it was confirmed that L* was 99.40±0.05, a* was 0.03±0.01, b* was -0.43±0.01, and YI was -0.58±0.01.

[0420] YI was measured by filling the pellets to a depth of about 40 mm in a cylindrical glass container having an inner diameter of 30 mm and a height of 50 mm. The pellets were taken out of the glass container and then measured again twice, and the average value of the three measured values ​​was used.

[0421] [Measurement of pH]

[0422] The pH was measured using a pH meter "pH METER ES-73" manufactured by Horiba, Ltd., on a 25°C water phase taken out from the flask.

[0423] [Melted color of bisphenol A]

[0424] The melting color of bisphenol A is in the test tube "P-24" manufactured by Nippon Rika Glass Co., Ltd. 20 g of bisphenol C was added to the mixture, and the mixture was melted at 175° C. for 30 minutes. The Hazen color number was measured using “SE6000” manufactured by Nippon Denshoku Industries Co., Ltd.

[0425] [Example 1]

[0426] In a nitrogen atmosphere, a jacketed separable flask equipped with a Dimrot cooling tube, a stirring blade, and a thermometer was added with 52 g of methanol (52 g ÷ 32 g / mol = 1.6 mol, repeating unit (molar ratio) of methanol / PC = 1.6 mol ÷ 0.31 mol = 5.2), 120 g of dimethyl carbonate (120 g ÷ 90 g / mol = 1.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 1.3 mol ÷ 0.31 mol = 4.2) and 100 g of dimethyl carbonate (100 g ÷ 90 g / mol = 1.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 1.3 mol ÷ 0.31 mol = 4.2). ) and 1.1g of sodium hydroxide (0.03 mol, the repeating unit (molar ratio) of sodium hydroxide / PC = 0.03 mol ÷ 0.31 mol = 0.10), then 80g of polycarbonate resin (the molecular weight of the repeating unit of the polycarbonate resin is 254g / mol, so the molar number of the repeating unit = 80g ÷ 254g / mol = 0.31 mol) was added at room temperature (the amount of liquid is 52g + 120g + 1.1g + 80g = 253.1g).

[0427] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0428] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 18.5 mass % (18.5÷100×253.1 g÷228 g / mol÷0.31 mol×100=66 mol %).

[0429] [Example 2]

[0430] Under a nitrogen atmosphere, 52 g of methanol (1.6 mol, repeating unit (molar ratio) of methanol / PC = 5.2), 120 g of dimethyl carbonate (1.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 4.2) and 1.1 g of potassium hydroxide (0.02 mol, repeating unit (molar ratio) of potassium hydroxide / PC = 0.02 mol / 0.31 mol = 0.06) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 0.31 mol) was added at room temperature (the amount of liquid was 52 g + 120 g + 1.1 g + 80 g = 253.1 g).

[0431] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution at 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 65° C. to obtain a uniform reaction solution.

[0432] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 23.2 mass % (23.2÷100×253.1 g÷228 g / mol÷0.31 mol×100=83 mol %).

[0433] [Example 3]

[0434] Under a nitrogen atmosphere, 80 g of methanol (80 g ÷ 32 g / mole = 2.5 moles, repeating unit (molar ratio) of methanol / PC = 2.5 moles ÷ 0.31 moles = 8.1), 120 g of dimethyl carbonate (1.3 moles, repeating unit (molar ratio) of dimethyl carbonate / PC = 4.2) and 20 g of triethylamine (0.20 mole, repeating unit (molar ratio) of triethylamine / PC = 0.20 mole ÷ 0.31 mole = 0.65) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 80 g ÷ 254 g / mole = 0.31 mole) was added at room temperature (the amount of liquid was 80 g + 120 g + 20 g + 80 g = 300 g).

[0435] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution at 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 65° C. to obtain a uniform reaction solution.

[0436] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 19.5 mass % (19.5÷100×300 g÷228 g / mol÷0.31 mol×100=83 mol %).

[0437] [Example 4]

[0438] Under a nitrogen atmosphere, 52 g of methanol (1.6 mol, repeating unit (molar ratio) of methanol / PC = 5.2), 120 g of dimethyl carbonate (1.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 4.2) and 1.1 g of potassium carbonate (0.01 mol, repeating unit (molar ratio) of potassium carbonate / PC = 0.01 mol ÷ 0.31 mol = 0.03) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 0.31 mol) was added at room temperature (the amount of liquid was 52 g + 120 g + 1.1 g + 80 g = 253.1 g).

[0439] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0440] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 24.1 mass % (24.1÷100×253.1 g÷228 g / mol÷0.31 mol×100=86 mol %).

[0441] [Comparative Example 1]

[0442] In a nitrogen atmosphere, at room temperature, 80 g of polycarbonate resin (number of moles of repeating units = 0.31 mol), 201 g of methanol (201 g ÷ 32 g / mol = 6.28 mol, repeating unit (molar ratio) of methanol / PC = 6.28 mol ÷ 0.31 mol = 20.25), and 15 g of triethylamine were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade, and a thermometer.

[0443] Next, the internal temperature was tried to be raised to 85° C., but since methanol refluxed at around 64° C., the reaction was allowed to proceed while maintaining reflux. It was confirmed that the polycarbonate resin was visible as a solid component in the reaction solution and was not decomposed despite the 4-hour reaction.

[0444] Table 1 summarizes the reaction yields of the catalysts, solvents, and bisphenols in Examples 1 to 4 and Comparative Example 1.

[0445] [Table 1]

[0446] catalyst Solvents Bisphenol A generation rate Example 1 Sodium hydroxide Dimethyl carbonate / methanol 66 mol% Example 2 Potassium hydroxide Dimethyl carbonate / methanol 83 mol% Example 3 Triethylamine Dimethyl carbonate / methanol 83 mol% Example 4 Potassium carbonate Dimethyl carbonate / methanol 86 mol% Comparative Example 1 Triethylamine Methanol No decomposition reaction

[0447] [Example 5]

[0448] (i) Production of bisphenol A

[0449] Under a nitrogen atmosphere, 125 g of methanol (125 g ÷ 32 g / mol = 3.9 mol, repeating unit (molar ratio) of methanol / PC = 3.9 mol ÷ 0.79 mol = 4.9), 300 g of dimethyl carbonate (300 g ÷ 90 g / mol = 3.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 3.3 mol ÷ 0.79 mol = 4.2) and 3 g of potassium hydroxide were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 200 g of a polycarbonate resin (number of moles of repeating units = 200 g ÷ 254 g / mol = 0.79 mol) was added at room temperature (the amount of liquid was 125 g + 300 g + 3 g + 200 g = 628 g).

[0450] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0451] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 24.3 mass % (24.3÷100×628 g÷228 g / mol÷0.79 mol×100=85 mol %).

[0452] Dilute sulfuric acid was added to the obtained reaction solution until the pH of the aqueous phase reached 6. The precipitated potassium sulfate salt was filtered out by vacuum filtration to obtain a uniform extract.

[0453] The obtained extract was transferred to a distillation apparatus equipped with a thermometer, stirring blades, a distillation tube, and a pressure regulator. The pressure was increased from normal pressure (760 Torr) to 120 Torr, and while observing the distillate amount, the internal temperature was raised from room temperature to 80°C, and 392 g was extracted as a fraction to obtain a still residue.

[0454] 280 g of toluene was added to the obtained still residue to prepare a uniform solution at 80° C. Then, the temperature was slowly lowered to 5° C. to obtain a slurry liquid. The obtained slurry liquid was filtered and separated using a centrifugal separator to obtain a coarse cake.

[0455] Under a nitrogen atmosphere, the total amount of the obtained filter cake is supplied to a jacketed separable flask equipped with a Dimrot cooling tube, a stirring blade, and a thermometer. Then, 10 g of dimethyl carbonate and 280 g of toluene are supplied. The obtained slurry liquid is heated to 80°C to prepare a uniform solution. The obtained uniform solution is washed 3 times with 100 g of desalted water. Then, the temperature is lowered to 5°C to obtain a slurry liquid. The obtained slurry liquid is filtered and separated with a centrifuge to obtain a refined filter cake. Using an evaporator equipped with an oil bath, all the refined filter cakes are dried at an oil bath temperature of 85°C and 15 Torr for 3 hours to obtain 121 g of solid.

[0456] The obtained solid was confirmed by high performance liquid chromatography to be bisphenol A with a purity of 99.9%. The melt color of the obtained bisphenol A was APHA11.

[0457] (ii) Production of recycled polycarbonate resin

[0458] In a glass reaction tank with a content of 150 mL equipped with a stirrer and a distillation tube, 100.00 g (0.44 mole) of bisphenol A obtained in (i) above, 96.30 g (0.45 mole) of diphenyl carbonate and 160 μL of a 400 mass ppm cesium carbonate aqueous solution were added. The glass reaction tank was depressurized to about 100 Pa, and then the operation of returning to atmospheric pressure using nitrogen was repeated 3 times to replace the interior of the reaction tank with nitrogen. Then, the reaction tank was immersed in an oil bath at 200° C. to dissolve the contents.

[0459] The rotation speed of the stirrer was set to 100 times per minute, and the phenol produced as a byproduct of the oligomerization reaction between bisphenol A and diphenyl carbonate in the reaction tank was distilled off, and the pressure in the reaction tank was reduced from 101.3 kPa to 13.3 kPa in 40 minutes by an absolute pressure gauge. Next, the pressure in the reaction tank was maintained at 13.3 kPa, and the phenol was further distilled off while the transesterification reaction was carried out for 80 minutes. Then, the external temperature of the reaction tank was raised to 250° C., and the pressure in the reaction tank was reduced from 13.3 kPa to 399 Pa in 40 minutes by an absolute pressure gauge, and the distilled phenol was removed to the outside of the system.

[0460] Then, the external temperature of the reaction tank was raised to 290°C, and the absolute pressure of the reaction tank was reduced to 30 Pa to carry out the polycondensation reaction. When the stirrer of the reaction tank reached a predetermined stirring power, the polycondensation reaction was terminated. The time from the temperature rise to 290°C to the end of the polymerization (late polymerization time) was 140 minutes.

[0461] Next, the pressure of the reaction vessel was restored to 101.3 kPa in absolute pressure by nitrogen gas, and then increased to a gauge pressure of 0.2 MPa, and the polycarbonate resin was extracted in the form of strands from the bottom of the reaction vessel to obtain polycarbonate resin in the form of strands.

[0462] Then, the strands were pelletized using a rotary cutter to obtain pelletized polycarbonate resin.

[0463] The viscosity average molecular weight (Mv) of the obtained polycarbonate resin was 20,900, and the particle YI was 8.4, and a polycarbonate resin having a good color tone was obtained.

[0464] [Comparative Example 2]

[0465] In Example 5, the same procedures as in Example 5 were carried out except that 3 g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) was added instead of 3 g of potassium hydroxide.

[0466] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 24.1 mass % (24.1÷100×628 g÷228 g / mol÷0.79 mol×100=84 mol %).

[0467] 120 g of a solid was obtained, and the obtained solid was confirmed to be bisphenol A with a purity of 99.9% by high performance liquid chromatography. The melt color of the obtained bisphenol A was APHA89.

[0468] The obtained polycarbonate resin pellets had a YI of 15.

[0469] In Example 5 and Comparative Example 2, the type of catalyst, the production rate of bisphenol A (BPA), the melt color of the obtained bisphenol A (BPA), and the obtained polycarbonate (PC) resin pellet YI are summarized in Table 2. As can be seen from Table 2, by using potassium hydroxide, the melt color of the obtained bisphenol A is good, and the obtained polycarbonate resin pellet YI is also good.

[0470] [Table 2]

[0471]

[0472] It should be noted that the method for producing bisphenol of the present invention can use a general-purpose catalyst, and the catalyst cost is also low. For example, 500 g of sodium hydroxide costs 1,250 yen, 500 g of potassium hydroxide costs 1,400 yen, 500 mL of triethylamine costs 1,450 yen, and 100 g of potassium carbonate costs 2,200 yen. On the other hand, 5 g of TBD costs 16,300 yen. When TBD is used, the catalyst cost becomes high in order to obtain the same production rate of bisphenol A.

[0473] [Example 6]

[0474] In a nitrogen atmosphere, 52 g of ethanol (52 g ÷ 46 g / mol = 1.1 mol, ethanol / PC repeating unit (molar ratio) = 1.1 mol ÷ 0.31 mol = 3.5), 120 g of diethyl carbonate (120 g ÷ 118 g / mol = 1.0 mol, diethyl carbonate / PC repeating unit (molar ratio) = 1.0 mol ÷ 0.31 mol = 3.2) and 1.1 g of potassium hydroxide (0.02 mol, potassium hydroxide / PC repeating unit (molar ratio) = 0.02 mol ÷ 0.31 mol = 0.06) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 0.31 mol) was added at room temperature (liquid amount: 52 g + 120 g + 1.1 g + 80 g = 253.1 g).

[0475] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0476] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 22.5 mass % (22.5÷100×253.1 g÷228 g / mol÷0.31 mol×100=81 mol %).

[0477] [Example 7]

[0478] In a nitrogen atmosphere, 10 g of butanol (10 g ÷ 74 g / mol = 135 mmol, butanol / PC repeating unit (molar ratio) = 135 mmol ÷ 39.4 mmol = 3.4), 30 g of dibutyl carbonate (30 g ÷ 174 g / mol = 172 mmol, dibutyl carbonate / PC repeating unit (molar ratio) = 172 mmol ÷ 39.4 mmol = 4.4) and 0.1 g of potassium hydroxide (1.8 mmol, potassium hydroxide / PC repeating unit (molar ratio) = 1.8 mmol ÷ 39.4 mmol = 0.05) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade, and a thermometer. Then, 10 g of a polycarbonate resin (number of moles of repeating units = 10 g ÷ 254 g / mol = 39.4 mol) was added at room temperature (liquid amount: 10 g + 30 g + 0.1 g + 10 g = 50.1 g).

[0479] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0480] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 7.1 mass % (7.1÷100×50.1 g÷228 g / mol÷0.04 mol×100=39 mol %).

[0481] [Example 8]

[0482] Under a nitrogen atmosphere, 16 g of methanol (16 g ÷ 32 g / mol = 0.5 mol, repeating unit (molar ratio) of methanol / PC = 0.5 mol ÷ 0.31 mol = 1.6), 160 g of dimethyl carbonate (160 g ÷ 90 g / mol = 1.8 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 1.8 mol ÷ 0.31 mol = 5.8) and 1.6 g of potassium hydroxide were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 0.31 mol) was added at room temperature (the amount of liquid is 16 g + 160 g + 1.6 g + 80 g = 257.6 g).

[0483] Then, the jacket temperature was raised to 65° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution when the temperature reached 65° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 65° C. to obtain a uniform reaction solution.

[0484] The obtained reaction solution was neutralized with dilute sulfuric acid, and potassium sulfate was filtered to obtain a filtrate. The filtrate was placed in an eggplant-shaped flask and dried and solidified under full vacuum using an evaporator equipped with an oil bath to obtain 57 g of a solid. A portion of the obtained solid was analyzed by high performance liquid chromatography, and the results showed that bisphenol A was 87.3% by mass and bisphenol-methyl carbonate condensate was 12.7% by mass.

[0485] [Example 9A]

[0486] In a 1L four-necked flask equipped with a thermometer, a stirring device, and a cooling tube, 46g of bisphenol A obtained in Example 5 (BPA purity 99%), 259g of epichlorohydrin, 100g of isopropyl alcohol, and 36g of water were placed, and the temperature was raised to 40°C to make it uniformly dissolved, and then 38g of a 48.5% by weight sodium hydroxide aqueous solution was added dropwise over 90 minutes. While dropping, the temperature was raised from 40°C to 65°C over 90 minutes. Then, the temperature was maintained at 65°C for 30 minutes to complete the reaction, and the reaction solution was transferred to a 1L separatory funnel, 69g of 65°C water was added, and the mixture was allowed to stand at 65°C for 1 hour. After standing, the water layer was extracted from the separated oil layer and water layer, and the by-product salt and excess sodium hydroxide were removed. Then, epichlorohydrin was completely removed under reduced pressure at 150°C.

[0487] Then, 102 g of methyl isobutyl ketone was added, the temperature was raised to 65° C. to make it uniformly dissolved, and then 1.4 g of a 48.5 wt % sodium hydroxide aqueous solution was added. After reacting for 60 minutes, 57 g of methyl isobutyl ketone was added, and the mixture was washed four times with 200 g of water. Then, the methyl isobutyl ketone was completely removed under reduced pressure at 150° C. to obtain the regenerated epoxy resin of Example 9A.

[0488] The epoxy equivalent of the obtained epoxy resin was measured in accordance with JIS K7236 (2009) and found to be 179 g / equivalent.

[0489] [Reference Example 1A]

[0490] In a 1L four-necked flask equipped with a thermometer, a stirring device, and a cooling tube, 46g of bisphenol A (manufactured by Mitsubishi Chemical Corporation), 259g of epichlorohydrin, 100g of isopropyl alcohol, and 36g of water were added. After heating to 40°C to dissolve evenly, 38g of a 48.5% by weight sodium hydroxide aqueous solution was added dropwise over 90 minutes. While dropping, the temperature was raised from 40°C to 65°C over 90 minutes. Then, the reaction was terminated by maintaining it at 65°C for 30 minutes, and the reaction solution was transferred to a 1L separatory funnel, 69g of 65°C water was added, and it was allowed to stand at 65°C for 1 hour. After standing, the water layer was extracted from the separated oil layer and water layer, and the by-product salt and excess sodium hydroxide were removed. Then, epichlorohydrin was completely removed under reduced pressure at 150°C.

[0491] Then, 102 g of methyl isobutyl ketone was added, the temperature was raised to 65° C. to make it uniformly dissolved, and then 1.4 g of a 48.5 wt % sodium hydroxide aqueous solution was added. After reacting for 60 minutes, 57 g of methyl isobutyl ketone was added, and the mixture was washed four times with 200 g of water. Then, the methyl isobutyl ketone was completely removed under reduced pressure at 150° C. to obtain the epoxy resin of Reference Example 1A.

[0492] The epoxy equivalent of the obtained epoxy resin was measured in accordance with JIS K 7236 (2009) and found to be 179 g / equivalent.

[0493] [Example 9B and Reference Example 1B]

[0494] (Epoxy resin composition)

[0495] The epoxy resin of Example 9A or Reference Example 1A, a curing agent (manufactured by Shin Nippon Chemical Co., Ltd., trade name: RIKACID MH-700) and a curing catalyst (manufactured by Shikoku Chemical Industry Co., Ltd., trade name: Curezol 2E4MZ) were weighed in the ratio shown in Table 2, and stirred and mixed at room temperature until uniform, to obtain an epoxy resin composition.

[0496] (Epoxy resin cured product)

[0497] Two glass plates with release PET films attached were prepared, with both release PET films facing inward, and the distance between the glass plates was adjusted to 3 mm to prepare a mold. The epoxy resin composition was cast in the mold, heated at 100°C for 3 hours, and then heated at 140°C for 3 hours to obtain an epoxy resin cured product. The obtained cured product was cut into a length of 5 cm, a width of 1 cm, and a thickness of 3 mm to obtain a test piece.

[0498] (Evaluation of physical properties of cured product)

[0499] The test piece was heated from 30°C to 280°C at 5°C / min using a thermomechanical analyzer (DMA: EXSTAR6100 manufactured by Seiko Instruments) in a three-point bending mode, and E' at 250°C was measured as the 250°C elastic modulus.

[0500] [Table 3]

[0501] Example 9B Reference Example 1B Epoxy Resin of Example 9A share 100 - Epoxy resin of Reference Example 1A share - 100 Curing agent share 92 92 Curing catalyst share 1 1 250℃ elastic modulus MPa 14 11

[0502] [Evaluation of results]

[0503] As can be seen from Table 3, the epoxy resin cured product of Example 9B has a higher elastic modulus at 250° C. and is superior in heat deformation resistance than the epoxy resin cured product of Reference Example 1B.

[0504] [Example 10]

[0505] (First Decomposition Step)

[0506] Under a nitrogen atmosphere, 52 g of methanol (1.6 mol, repeating unit (molar ratio) of methanol / PC = 5.2), 120 g of dimethyl carbonate (1.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 4.2) and 1.1 g of sodium hydroxide (0.03 mol, repeating unit (molar ratio) of sodium hydroxide / PC = 0.10) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of polycarbonate resin (number of moles of repeating unit = 0.31 mol) was added at room temperature (liquid amount: 52 g + 120 g + 1.1 g + 80 g = 253.1 g).

[0507] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction solution at 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a first decomposition solution (uniform reaction solution).

[0508] The composition of a portion of the obtained first decomposition liquid was confirmed by high performance liquid chromatography, and the result showed that bisphenol A was 18.5 mass % (18.5÷100×253.1 g÷228 g / mol÷0.31 mol×100=66 mol %). The composition was also confirmed by gas chromatography, and the result showed that methanol was 14.7 mass % and dimethyl carbonate was 55.2 mass %.

[0509] (Second Decomposition Step)

[0510] 5.6 g (0.31 mol) of water was added to the first decomposition liquid, and the mixture was stirred for 1 hour while maintaining the temperature at 70° C. After 1 hour, the stirring was stopped and the mixture was allowed to stand, whereupon white solid was confirmed to have precipitated on the wall of the separable flask.

[0511] The reaction liquid was extracted and the weight was measured to be 243.8 g. The composition was confirmed by high performance liquid chromatography and found to contain 25.7 mass % bisphenol A (25.7÷100×243.8g÷228g / mol÷0.31 mol×100=88.6 mol %).

[0512] In addition, utilizing gas chromatography to confirm composition, result methanol is 21.1 mass %, and the recovery rate with respect to the methanol supplied to reaction is 98.9 mass % (21.1÷100×243.8÷52g×100=98.9 mass %). In addition, dimethyl carbonate is 49.0 mass %, and the recovery rate with respect to the dimethyl carbonate supplied to reaction is 99.5 mass % (49.0÷100×243.8÷120g×100=99.5 mass %).

[0513] [Example 11]

[0514] (First Decomposition Step)

[0515] The first decomposition step was carried out in the same manner as in Example 10 to obtain a first decomposition liquid (uniform reaction liquid). The composition of a portion of the obtained first decomposition liquid was confirmed by high performance liquid chromatography, and the result showed that bisphenol A was 18.4 mass % (18.4÷100×253.1g÷228g / mol÷0.31mol×100=66mol%). In addition, the composition was confirmed by gas chromatography, and the result showed that methanol was 14.6 mass % and dimethyl carbonate was 55.3 mass %.

[0516] (Second Decomposition Step)

[0517] 4.5 g (0.25 mol) of water was added to the first decomposition liquid, and the mixture was stirred for 1 hour while maintaining the temperature at 70° C. After 1 hour, the stirring was stopped and the mixture was allowed to stand, whereupon white solid was confirmed to have precipitated on the wall of the separable flask.

[0518] The reaction liquid was extracted and the weight was measured to be 245.8 g. The composition was confirmed by high performance liquid chromatography and found to contain 24.5 mass % bisphenol A (24.5÷100×245.8g÷228g / mol÷0.31 mol×100=85.2 mol %).

[0519] In addition, utilizing gas chromatography to confirm composition, result methanol is 19.1 mass %, and the recovery rate with respect to the methanol supplied to reaction is 90.3 mass % (19.1÷100×245.8÷52g×100=90.3 mass %). In addition, dimethyl carbonate is 51.3 mass %, and the recovery rate with respect to the dimethyl carbonate supplied to reaction is 105.1 mass % (51.3÷100×245.8÷120g×100=105.1 mass %).

[0520] Dilute sulfuric acid was added to the obtained reaction solution until the pH of the aqueous phase reached 6. The precipitated potassium sulfate salt was filtered and separated by vacuum filtration to obtain a uniform extract.

[0521] The obtained extract was dried and solidified using an evaporator equipped with an oil bath to obtain bisphenol. In addition, the distillate was 165 g, and the composition was confirmed by gas chromatography. As a result, methanol was 28.4 mass% (28.4÷100×165g=46.9g) and dimethyl carbonate was 70.4 mass% (70.4÷100×165g=116.2g).

[0522] [Example 12]

[0523] (First Decomposition Step)

[0524] In a nitrogen atmosphere, a jacketed separable flask equipped with a Dimrot cooling tube, a stirring blade, and a thermometer was added 165 g of the distillate obtained in Example 11 (containing 46.9 g of methanol and 116.2 g of dimethyl carbonate), 5.1 g of methanol (totaling 52 g (1.6 mol) with the methanol in the distillate, the repeating unit (molar ratio) of methanol / PC = 1.6 mol ÷ 0.31 mol = 5.2), 3.8 g of dimethyl carbonate (totaling 120 g with the dimethyl carbonate in the distillate) and 1.6 mol ÷ 0.31 mol = 5.2. (1.3 mol, repeating unit of dimethyl carbonate / PC (molar ratio) = 1.3 mol ÷ 0.31 mol = 4.2) and 1.1g of sodium hydroxide (0.03 mol, repeating unit of sodium hydroxide / PC (molar ratio) = 0.10), then 80g of polycarbonate resin (number of moles of repeating unit = 80g ÷ 254g / mole = 0.31 mol) was added at room temperature (the amount of liquid was 165g + 5.1g + 3.8g + 1.1g + 80g = 255.0g).

[0525] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in a slurry state) was observed in the reaction liquid at 70° C. The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a first decomposition liquid (uniform reaction liquid).

[0526] The composition of a portion of the obtained first decomposition liquid was confirmed by high performance liquid chromatography, and the result showed that bisphenol A was 18.4 mass % (18.4÷100×255.0g÷228g / mol÷0.31mol×100=66mol%). The composition was also confirmed by gas chromatography, and the result showed that methanol was 14.6 mass % and dimethyl carbonate was 54.8 mass %.

[0527] (Second Decomposition Step)

[0528] 6.7 g (0.37 mol) of water was added to the first decomposition liquid, and the mixture was stirred for 1 hour while maintaining the temperature at 70° C. After 1 hour, the stirring was stopped and the mixture was allowed to stand, whereupon white solid was confirmed to have precipitated on the wall of the separable flask.

[0529] The reaction liquid was extracted and the weight was measured to be 243.6 g. The composition was confirmed by high performance liquid chromatography and found to contain 26.2 mass % bisphenol A (26.2÷100×243.6 g÷228 g / mol÷0.31 mol×100=90.3 mol %).

[0530] In addition, utilizing gas chromatography to confirm composition, result methanol is 23.1 mass %, and the recovery rate with respect to the methanol supplied to reaction is 109.9 mass % (23.1÷100×243.6÷52g×100=108.2 mass %). In addition, dimethyl carbonate is 46.3 mass %, and the recovery rate with respect to the dimethyl carbonate supplied to reaction is 94.1 mass % (46.3÷100×243.6÷120g×100=94.0 mass %).

[0531] [Example 13]

[0532] (First decomposition step)

[0533] The first decomposition step was carried out in the same manner as in Example 10 to obtain a first decomposition liquid (uniform reaction liquid). The composition of a portion of the obtained first decomposition liquid was confirmed by high performance liquid chromatography, and the result showed that bisphenol A was 18.5 mass % (18.5÷100×253.1g÷228g / mol÷0.31mol×100=66mol%). In addition, the composition was confirmed by gas chromatography, and the result showed that methanol was 14.7 mass % and dimethyl carbonate was 55.2 mass %.

[0534] (Second Decomposition Step)

[0535] 2.2 g (0.12 mol) of water was added to the first decomposition liquid, and the mixture was stirred for 1 hour while maintaining the temperature at 70° C. After 1 hour, the stirring was stopped and the mixture was allowed to stand, whereupon white solid was confirmed to have precipitated on the wall of the separable flask.

[0536] The reaction liquid was extracted and the weight was measured to be 248.8 g. The composition was confirmed by high performance liquid chromatography and found to contain 22.6 mass % bisphenol A (22.6÷100×248.8g÷228g / mol÷0.31 mol×100=79.6 mol %).

[0537] In addition, utilizing gas chromatography to confirm composition, result methanol is 15.9 mass %, and the recovery rate with respect to the methanol supplied to reaction is 77.0 mass % (15.9÷100×248.8÷52g×100=76.1 mass %). In addition, dimethyl carbonate is 54.8 mass %, and the recovery rate with respect to the dimethyl carbonate supplied to reaction is 113.6 mass % (54.8÷100×248.8÷120g×100=113.6 mass %).

[0538] [Example 14]

[0539] (First decomposition step)

[0540] The first decomposition step was carried out in the same manner as in Example 10 to obtain a first decomposition liquid (uniform reaction liquid). The composition of a portion of the obtained first decomposition liquid was confirmed by high performance liquid chromatography, and the result showed that bisphenol A was 18.5 mass % (18.5÷100×253.1g÷228g / mol÷0.31mol×100=66mol%). In addition, the composition was confirmed by gas chromatography, and the result showed that methanol was 14.7 mass % and dimethyl carbonate was 55.2 mass %.

[0541] (Second Decomposition Step)

[0542] 11.2 g (0.62 mol) of water was added to the first decomposition liquid, and the mixture was stirred for 1 hour while maintaining the temperature at 70° C. After 1 hour, the stirring was stopped and the mixture was allowed to stand, whereupon white solid was confirmed to have precipitated on the wall of the separable flask.

[0543] The reaction liquid was extracted and the weight was measured to be 235.4 g. The composition was confirmed by high performance liquid chromatography and found to contain 27.6 mass % bisphenol A (27.6÷100×235.4 g÷228 g / mol÷0.31 mol×100=91.9 mol %).

[0544] In addition, utilize gas chromatography to confirm composition, result methanol is 30.6 mass %, and the recovery rate with respect to the methanol supplied to reaction is 138.5 mass % (30.6÷100×235.4÷52g×100=138.5 mass %). In addition, dimethyl carbonate is 38.6 mass %, and the recovery rate with respect to the dimethyl carbonate supplied to reaction is 75.7 mass % (38.6÷100×235.4÷120g×100=75.7 mass %).

[0545] The results of Examples 10 to 14 are summarized in Table 4. As can be seen from Table 4, by adding water during the reaction to hydrolyze the dialkyl carbonate, the decomposition reaction of bisphenol A can be promoted, and the yield of bisphenol A can be further improved. In addition, by adjusting the amount of water added to a certain range, the aliphatic monohydric alcohol can be regenerated from the dialkyl carbonate generated by the alcoholysis of the polycarbonate resin, and the ratio of the dialkyl carbonate and the aliphatic monohydric alcohol in the recovered mixture can be maintained at a ratio (80% by mass to 120% by mass) that is easy to reuse in the first decomposition step.

[0546] [Table 4]

[0547]

[0548] [Example 15]

[0549] Under a nitrogen atmosphere, 50 g of methanol (50 g ÷ 32 g / mole = 1.6 moles, repeating unit (molar ratio) of methanol / PC = 1.6 moles ÷ 0.31 moles = 5.2), 120 g of dimethyl carbonate (1.3 moles, repeating unit (molar ratio) of dimethyl carbonate / PC = 4.2) and 1.2 g of potassium hydroxide (0.02 mole, repeating unit (molar ratio) of potassium hydroxide / PC = 0.02 mole ÷ 0.31 mole = 0.1) were added to a jacketed separable flask equipped with a Dimrot cooler, a stirring blade and a thermometer, and then 80 g of a polycarbonate resin (number of moles of repeating units = 0.31 moles) was added at room temperature (liquid amount: 50 g + 120 g + 1.2 g + 80 g = 251.2 g).

[0550] Then, the jacket temperature was raised to 70° C. Undissolved polycarbonate resin (in slurry form) was observed in the reaction solution at 70° C. The theoretical slurry concentration at the start of decomposition was 0.32 (mass of polycarbonate resin 80 g÷mass of decomposition solution 251.2 g=0.32).

[0551] The reaction was continued for 3 hours while maintaining the jacket temperature at 70° C. to obtain a uniform reaction solution.

[0552] The composition of a part of the obtained reaction liquid was confirmed by high performance liquid chromatography, and as a result, bisphenol A was 24.5 mass% (24.5÷100×251.2 g÷228 g / mol÷0.31 mol×100=87 mol%).

[0553] [Example 16]

[0554] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 105 g (1.2 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 3.9). The theoretical slurry concentration at the start of decomposition was 0.34 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 236.2 g = 0.34).

[0555] The reaction liquid was uniform 3 hours after the start of decomposition. The composition of a portion of the reaction liquid was confirmed by high performance liquid chromatography, and the content of bisphenol A was 26.7% by mass (26.7÷100×236.2g÷228g / mol÷0.31mol×100=89mol%).

[0556] [Example 17]

[0557] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 94 g (1.0 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 3.2). The theoretical slurry concentration at the start of decomposition was 0.36 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 225.2 g = 0.36).

[0558] The reaction liquid was uniform 3 hours after the start of decomposition. The composition of a portion of the reaction liquid was confirmed by high performance liquid chromatography, and the content of bisphenol A was 28.0 mass % (28.0÷100×225.2g÷228g / mol÷0.31mol×100=89mol%).

[0559] [Example 18]

[0560] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 74 g (0.8 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 2.6). The theoretical slurry concentration at the start of decomposition was 0.39 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 205.2 g = 0.39).

[0561] The reaction liquid was uniform 3 hours after the start of decomposition. The composition of a portion of the reaction liquid was confirmed by high performance liquid chromatography, and the content of bisphenol A was 28.4 mass % (28.4÷100×205.2g÷228g / mol÷0.31mol×100=82mol%).

[0562] [Example 19]

[0563] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 52 g (0.6 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 1.9). The theoretical slurry concentration at the start of decomposition was 0.44 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 183.2 g = 0.44).

[0564] The reaction liquid was uniform 3 hours after the start of decomposition. The composition of a portion of the reaction liquid was confirmed by high performance liquid chromatography, and the content of bisphenol A was 25.2 mass % (25.2÷100×183.2g÷228g / mol÷0.31mol×100=65mol%).

[0565] The reaction was further continued for 1 hour while maintaining the temperature at 70°C. A portion of the reaction solution taken 4 hours after the start of decomposition was analyzed by high performance liquid chromatography to determine the composition of bisphenol A at 30.8 mass % (30.8÷100×183.2g÷228g / mol÷0.31mol×100=80mol%).

[0566] [Comparative Example 3]

[0567] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 45 g (0.5 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 1.6).

[0568] After the decomposition started, part of the polycarbonate resin accumulated between the thermometer and the separable flask. The accumulated polycarbonate resin lumps were not completely dissolved even 3 hours after the decomposition started. The theoretical slurry concentration at the start of decomposition was 0.45 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 176.2 g = 0.45).

[0569] [Comparative Example 4]

[0570] The polycarbonate resin was decomposed under the same conditions as in Example 15 except that the supply amount of dimethyl carbonate was changed from 120 g to 30 g (0.3 mol, dimethyl carbonate / PC repeating unit (molar ratio) = 1.0).

[0571] After the decomposition started, the polycarbonate resin was not dispersed but agglomerated, and an excessive load was applied to the stirring blade, causing it to run idle and unable to stir, thus stopping the decomposition reaction. The theoretical slurry concentration at the start of decomposition was 0.50 (mass of polycarbonate resin 80g ÷ mass of decomposition liquid 161.2g = 0.50).

[0572] [Comparative Example 5]

[0573] The polycarbonate resin was decomposed under the same conditions as in Example 15, except that the supply amount of dimethyl carbonate was changed from 120 g to 30 g (0.3 mol, repeating unit (molar ratio) of dimethyl carbonate / PC = 1.0), and the supply amount of methanol was changed from 50 g to 80 g (2.5 mol, repeating unit (molar ratio) of methanol / PC = 8.1).

[0574] The polycarbonate resin had good miscibility, but even 3 hours after the start of decomposition, a large amount of polycarbonate resin was not dissolved. The reaction was continued at 70°C for 1 hour, but the polycarbonate resin was not completely dissolved. The theoretical slurry concentration at the start of decomposition was 0.42 (mass of polycarbonate resin 80 g ÷ mass of decomposition liquid 191.2 g = 0.42).

[0575] The results of Examples 15 to 19 and Comparative Examples 3 to 5 are summarized in Table 5. As can be seen from Table 5, the dissolution rate and decomposition rate of the polycarbonate resin can be maintained by supplying an appropriate amount of dialkyl carbonate solvent relative to the repeating units of the polycarbonate resin to be decomposed. If the supply amount of dialkyl carbonate relative to the repeating units of the polycarbonate resin is small, the dissolution rate of the polycarbonate resin decreases, the time required for the decomposition of the polycarbonate resin becomes longer, and the efficiency is not high.

[0576] [Table 5]

[0577]

[0578] * Theoretical slurry concentration = mass of solid content in reaction solution / mass of reaction solution

[0579] Possibility of Industrial Application

[0580] According to the present invention, useful compounds such as bisphenol can be obtained from waste plastics etc. by chemical recycling. Furthermore, these compounds can be used to produce polycarbonate resins and epoxy resins again, which is industrially useful.

Claims

1. A method for producing bisphenol, which comprises performing a decomposition reaction of a polycarbonate resin in a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst, wherein: The molar ratio of the dialkyl carbonate used in the decomposition reaction to 1 mol of the repeating unit derived from bisphenol in the polycarbonate resin used in the decomposition reaction is 1.8 or more, The catalyst is any one selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal alkoxides, alkali metal oxides, chain alkylamines and pyridine.

2. The method for producing bisphenol according to claim 1, wherein The reaction solution is in the form of slurry.

3. The method for producing bisphenol according to claim 1 or 2, wherein: The dialkyl carbonate includes a dialkyl carbonate not derived from the polycarbonate resin.

4. The method for producing bisphenol according to claim 1 or 2, wherein: The reaction liquid is prepared by mixing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst.

5. The method for producing bisphenol according to claim 1 or 2, wherein: The alkali metal hydroxide is sodium hydroxide or potassium hydroxide, The alkali metal carbonate is sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate, The alkali metal alkoxide is sodium phenolate or sodium methoxide, The alkali metal oxide is sodium oxide or potassium oxide.

6. The method for producing bisphenol according to claim 1 or 2, wherein: The chain alkylamine is represented by the following formula (I) or the following formula (II), [Chemistry 1] In formula (I), R A represents an alkyl group having 1 to 3 carbon atoms, R B ~R C Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, [Chemistry 2] In formula (II), R D ~R G Each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and m represents an integer of 1 to 6.

7. The method for producing bisphenol according to claim 1 or 2, wherein: The dialkyl carbonate is dimethyl carbonate, diethyl carbonate or dibutyl carbonate.

8. The method for producing bisphenol according to claim 1 or 2, wherein: The bisphenol is 2,2-bis(4-hydroxyphenyl)propane.

9. The method for producing bisphenol according to claim 1 or 2, wherein: The aliphatic monohydric alcohol is methanol, ethanol or butanol.

10. The method for producing bisphenol according to claim 1 or 2, comprising the following steps A, B1 and C1: Step A: a step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a non-slurry polycarbonate decomposition solution containing bisphenol, Step B1: a step of concentrating the polycarbonate decomposition liquid obtained in the step A to obtain a concentrated liquid, Step C1: A step of supplying an aromatic hydrocarbon to the concentrated liquid obtained in the step B1 to precipitate bisphenol by crystallization to obtain a slurry containing bisphenol, and subjecting the obtained slurry to solid-liquid separation to obtain bisphenol.

11. The method for producing bisphenol according to claim 1 or 2, comprising the following steps A, B2 and C2: Step A: a step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a non-slurry polycarbonate decomposition solution containing bisphenol, Step B2: a step of removing the dialkyl carbonate and the aliphatic monohydric alcohol from the solution containing the polycarbonate decomposition liquid obtained in the step A and the aromatic monohydric alcohol to obtain a solution containing bisphenol and the aromatic monohydric alcohol, Step C2: a step of recovering bisphenol from the solution containing bisphenol and aromatic monohydric alcohol obtained in the step B2.

12. The method for producing bisphenol according to claim 1, comprising a first decomposition step and a second decomposition step. A first decomposition step of decomposing the polycarbonate resin in the reaction solution containing the polycarbonate resin, the dialkyl carbonate, the aliphatic monohydric alcohol and the catalyst to obtain a first decomposition solution containing bisphenol; a second decomposition step of mixing the first decomposition liquid with water to hydrolyze the dialkyl carbonate, regenerate the aliphatic monohydric alcohol, and decompose the polycarbonate resin to generate bisphenol; The first decomposition step and the second decomposition step are performed continuously.

13. The method for producing bisphenol according to claim 12, wherein: The amount of water mixed with the first decomposition liquid is 0.5 mol or more and 1.5 mol or less per 1 mol of the repeating unit derived from bisphenol of the polycarbonate resin used in the decomposition reaction.

14. The method for producing bisphenol according to claim 12 or 13, wherein: The aliphatic monohydric alcohol regenerated in the second decomposition step is separated from bisphenol in the form of a mixture with the dialkyl carbonate, and the mixture of the aliphatic monohydric alcohol and the dialkyl carbonate is reused in the first decomposition step.

15. The method for producing bisphenol according to claim 12 or 13, wherein: The reaction liquid is in a slurry state, and the first decomposition liquid is not in a slurry state.

16. The method for producing bisphenol according to claim 1 or 2, wherein: Further, recovering a bisphenol-alkyl carbonate condensate represented by the following formula (III) produced as a by-product during the decomposition of the polycarbonate resin, [Chemistry 3] In formula (III), R is methyl, ethyl or butyl.

17. The method for producing bisphenol according to claim 16, wherein: In the formula (III), R is a methyl group.

18. A method for producing a recycled polycarbonate resin, comprising producing a recycled polycarbonate resin using a bisphenol raw material containing bisphenol obtained by the bisphenol production method according to claim 1 or 2.

19. A method for producing an epoxy resin, comprising producing an epoxy resin using a polyhydroxy compound raw material containing bisphenol after obtaining bisphenol by the bisphenol production method according to claim 1 or 2.

20. A method for producing an epoxy resin, comprising: obtaining an epoxy resin by the method for producing an epoxy resin according to claim 19, and then further reacting an epoxy resin raw material containing the epoxy resin with a polyhydroxy compound raw material to produce the epoxy resin.

21. A method for producing a cured epoxy resin, comprising obtaining an epoxy resin by the method for producing an epoxy resin according to claim 19, obtaining an epoxy resin composition containing the epoxy resin and a curing agent, and curing the epoxy resin composition to obtain a cured epoxy resin.

22. A method for producing a bisphenol-alkyl carbonate condensate, which comprises decomposing a polycarbonate resin in a reaction solution containing a polycarbonate resin, a dialkyl carbonate, an aliphatic monohydric alcohol and a catalyst, and producing a bisphenol-alkyl carbonate condensate represented by the following formula (III). in, The catalyst is any one selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal alkoxides, alkali metal oxides, chain alkylamines and pyridine. [Chemistry 4] In formula (III), R is methyl, ethyl or butyl.

Citation Information

Patent Citations

  • Ring opening of polycarbonate

    JP1994340591A

  • Method for recovering useful product from waste plastic

    JP2004051620A

  • Method for producing epoxy resin, epoxy resin, and curable resin composition

    JP2011225711A

  • Curable composition for sealing semiconductor