Nucleated bimodal polypropylene
By developing α-nucleated bimodal polypropylene compositions and utilizing metallocene catalysts and cocatalyst systems for sequential polymerization, the problems of insufficient polypropylene stiffness and optical properties are solved, improving the competitiveness of the material and reducing environmental and health risks. .
Patent Information
- Application Number
- CN202380023540.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-08
AI Technical Summary
The stiffness and optical properties of existing polypropylene are not sufficient to compete with polystyrene, and its recycling requires high-purity raw materials, which poses environmental, health and safety issues.
Develop an alpha-nucleated bimodal polypropylene composition, which contains two different polypropylenes (PP1 and PP2) and an alpha-nucleating agent, and performs sequential polymerization through a specific metallocene catalyst and cocatalyst system to control the melt Flow rate, molecular weight distribution and comonomer content, resulting in materials with high stiffness and excellent optical properties.
The high stiffness and improved optical properties of polypropylene are achieved, reducing the environmental, health and safety risks of the material, and improving its competitiveness in injection molded products.
Smart Images

Figure BDA0005008420500000041 
Figure BDA0005008420500000051 
Figure BDA0005008420500000061
Abstract
Description
Technical Field
[0001] The invention relates to an alpha-nucleated bimodal polypropylene and a thin-wall injection-molded product made thereof. Background Art
[0002] Polystyrene is one of the polymers widely used in daily life (including packaging) due to its excellent combination of high stiffness, high transparency and low cost. However, the disadvantages of polystyrene are that its monomers have problems in terms of environment, health and safety, and recycling requires high purity raw materials, so other polymers that do not have these disadvantages are preferred. One of such polymers is polypropylene.
[0003] Polypropylene is one of the best choices because it is relatively cheap, has good stiffness, and can be widely used without environmental, health and safety issues. However, although its stiffness is already quite good, it is still not comparable to the stiffness of polystyrene. In addition, the optical properties of typical polypropylene need to be further improved to compete with polystyrene. It is well known that propylene homopolymers produced using metallocene catalysts have improved behavior in terms of the properties required for injection molded articles compared to known propylene homopolymers produced using Ziegler-Natta catalysts. However, such metallocene propylene homopolymers are still not sufficiently competitive with respect to polystyrene.
[0004] Therefore, it is an object of the present invention to provide a polypropylene having enhanced stiffness and optical properties compared to prior art polypropylenes. Summary of the invention
[0005] The present invention has been found to provide a polypropylene having a bimodal molecular weight distribution and a low comonomer content, ie not more than 0.75 mol %, wherein the bimodal polypropylene is α-nucleated.
[0006] Therefore, the present invention relates to an α-nucleated polypropylene composition (n-PP) comprising
[0007] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0008] (b) a second polypropylene (PP2), and
[0009] (c) an α-nucleating agent,
[0010] in
[0011] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0012] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0013] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0014] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg);
[0015] (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 3.5 to 6.5;
[0016] (iii) in the range of >0.35 to 0.85 mol% 13 2,1 erythro regiodefects measured by C NMR; and
[0017] (iv) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene.
[0018] Preferably, the α-nucleated polypropylene composition (n-PP) contains at least one α-nucleating agent selected from the group consisting of polymeric nucleating agents, sorbitol-based nucleating agents, nonitol-based nucleating agents and benzenetriamide-based nucleating agents. Still more preferably, the α-nucleating agent is selected from the group consisting of 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol, bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS) and polyvinylcyclohexane (p-VCH). Still more preferably, the one or more α-nucleating agents present in the α-nucleated polypropylene composition (n-PP) are selected from the group consisting of 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol, bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS) and polyvinylcyclohexane (p-VCH).
[0019] Preferably, the total amount of α-nucleating agents in the α-nucleated polypropylene composition (n-PP) is in the range of 0.001 to 2.0 wt%. Therefore, it is particularly preferred that the one or more α-nucleating agents present in the α-nucleated polypropylene composition (n-PP) are selected from the group consisting of polyvinylcyclohexane (p-VCH), 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol and bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS), wherein further, based on the total amount of the α-nucleated polypropylene composition (n-PP), the total amount of the one or more α-nucleating agents is in the range of 0.1 to 0.8 wt%.
[0020] Further preferred embodiments of the alpha-nucleated polypropylene composition (n-PP) according to this invention are defined in the claims.
[0021] Additionally, the present invention also relates to an injection molded article, more preferably a thin-walled injection molded article, consisting of the α-nucleated polypropylene composition (n-PP) according to the present invention, wherein preferably the thin-walled injection molded article has a wall thickness of at most 1.0 mm.
[0022] Hereinafter, the present invention is described in more detail. DETAILED DESCRIPTION
[0023] The α-nucleated polypropylene composition (n-PP) according to the present invention comprises two different polypropylenes (PP1) and (PP2) and an additional α-nucleating agent. The main components of the α-nucleated polypropylene composition (n-PP) are the two different polypropylenes (PP1) and (PP2). In other words, the total amount of the two different polypropylenes (PP1) and (PP2) is at least 94 wt.-%, more preferably at least 95 wt.-%, based on the α-nucleated polypropylene composition (n-PP).
[0024] The remainder of the α-nucleated polypropylene composition (n-PP) is the α-nucleating agent, one or more other optional polypropylenes as further defined below and optionally typical additives like antioxidants, antistatic agents and antifogging agents.
[0025] The amount of the α-nucleating agent is preferably in the range of 0.001 to 2.0 wt.-%, more preferably in the range of 0.01 to 1.0 wt.-%, still more preferably in the range of 0.05 to 0.5 wt.-%, yet more preferably in the range of 0.1 to 0.8 wt.-%, based on the total α-nucleated polypropylene composition (n-PP).
[0026] Typically the total amount of additives except the α-nucleating agent should not exceed 1.0 wt.-%, preferably in the range of 0.05 to 1.0 wt.-%, based on the total α-nucleated polypropylene composition (n-PP).
[0027] The α-nucleating agent and the additive may be added to the polypropylene comprising the polypropylene (PP1) and (PP2) and a small amount of a polyolefin different from the polypropylene (PP1) and (PP2). The term "different from" in this context means that the polyolefin differs from the polypropylene (PP1) and (PP2) in at least one typical characterizing feature in the polymer field, such as molecular weight, for example in terms of melt flow rate MFR. 2 (230° C.; 2.16 kg), melting point and / or misintercalation, e.g. in terms of 2,1 erythro regio defects. Preferably, the polyolefin used for this purpose is a polypropylene, especially a propylene homopolymer. Thus, this polypropylene, more preferably this propylene homopolymer, has a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg). Even more preferably, the polypropylene, still more preferably the propylene homopolymer, has been produced with a Ziegler-Natta catalyst of the 4th or 5th generation (see Nello Pasquini "Polypropylene Handbook", 2nd edition, pages 17 / 18), and therefore has a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C. p,m A typical further feature of such a polypropylene, more preferably such a propylene homopolymer, produced with a Ziegler-Natta catalyst of generation 4 or 5 is that it does not show 2,1 erythro regio-defects, i.e. there are no detectable 2,1 erythro regio-defects when analyzed according to the present invention. Accordingly, it is preferred that the α-nucleated polypropylene composition (n-PP) comprises one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg). More preferably, the one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2) have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230° C.; 2.16 kg) and a maximum melting peak temperature T measured by DSC (scanning rate of 10° C. / min; second heating step) in the range of 162 to 169° C. p,mEven more preferably, the one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2) have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 2,1 erythro regio defects measured by C NMR.The total amount of the one or more propylene homopolymers defined in this paragraph is in the range of 0.5 to 4.0 wt.-%, based on the total amount of the α-nucleated polypropylene composition (n-PP).
[0028] Accordingly, the present invention in particular relates to an α-nucleated polypropylene composition (n-PP) comprising, preferably consisting of, the following components,
[0029] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0030] (b) a second polypropylene (PP2),
[0031] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0032] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0033] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m, more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0034] in
[0035] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0036] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0037] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0038] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg);
[0039] (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 3.5 to 6.5;
[0040] (iii) in the range of >0.35 to 0.85 mol% 13 2,1 erythro regiodefects measured by C NMR; and
[0041] (iv) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0042] wherein optionally, still further, the α-nucleated polypropylene composition (n-PP) complies with
[0043] (v) Equation 2, preferably Equation 2a,
[0044]
[0045] in
[0046] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0047] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0048] "[(PP1) / (n-PP)]" is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP).
[0049] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%, more preferably the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer.
[0050] The α-nucleated polypropylene composition (n-PP) is dominated by the first polypropylene (PP1) and the second polypropylene (PP2), since these two polymers constitute at least 94 wt% of the α-nucleated polypropylene composition (n-PP). As described below, the first polypropylene (PP1) and the second polypropylene (PP2) are produced together in a sequential polymerization process using a specific metallocene catalyst. The first polypropylene (PP1) is produced in a first reactor, and then the second polypropylene (PP2) is produced in a second reactor and in the presence of the first polypropylene (PP1). Therefore, since the α-nucleated polypropylene composition (n-PP) has the polymerization product of the first polypropylene (PP1) and the second polypropylene (PP2) as the main components (at least 94 wt%), at least some of the final properties are also driven by the two polypropylenes (PP1) and (PP2).
[0051] Accordingly, since both the polypropylenes (PP1) and (PP2) are produced in the presence of the specific metallocene catalyst the final α-nucleated polypropylene composition (n-PP) has a certain amount of 2,1 erythro regio defects, preferably also a rather low xylene solubles content and a rather high crystallinity in terms of pentad isotacticity [mmmm].
[0052] Thus, the α-nucleated polypropylene composition (n-PP) has a carbonyl group-containing polyol in the range of >0.35 to 0.85 mol%, preferably in the range of 0.50 to 0.85 mol%. 132,1-erythro regiodefect measured by C NMR.
[0053] Further it is preferred that the alpha-nucleated polypropylene composition (n-PP) has a pentad isotacticity [mmmm] of at least 98.0 %, more preferably at least 99.0 %, still more preferably at least 99.2 %.
[0054] Additionally or alternatively with respect to the previous paragraph, it is preferred that the α-nucleated polypropylene composition (n-PP) has a xylene cold soluble fraction (XCS) measured according to ISO 16152 at 25 °C of not more than 1.0 wt.-%, more preferably in the range of 0.1 to 1.0 wt.-%, still more preferably in the range of 0.4 to 0.9 wt.-%.
[0055] Accordingly, the present invention in particular relates to an α-nucleated polypropylene composition (n-PP) comprising, preferably consisting of, the following components,
[0056] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0057] (b) a second polypropylene (PP2),
[0058] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0059] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0060] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m, more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0061] in
[0062] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0063] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0064] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0065] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0066] (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 3.5 to 6.5,
[0067] (iii) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR;
[0068] (iv) a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0069] (v) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0070] wherein optionally, still further, the α-nucleated polypropylene composition (n-PP) complies with
[0071] (vi) Equation 2, preferably Equation 2a,
[0072]
[0073] in
[0074] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0075] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0076] "[(PP1) / (n-PP)]" is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP).
[0077] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%, more preferably the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer.
[0078] The melt flow rates of the polypropylenes (PP1) and (PP2) are substantially different, otherwise a rather broad molecular weight distribution (MWD) of the α-nucleated polypropylene composition (n-PP) in the range of 3.5 to 6.5 is not possible. Even more preferably the molecular weight distribution (MWD) of the α-nucleated polypropylene composition (n-PP) is in the range of 4.0 to 5.5. Another consequence of the substantially different melt flow rates of the polypropylenes (PP1) and (PP2) is a melt flow rate MFR of the α-nucleated polypropylene composition (n-PP). 2 Also substantially higher than the melt flow rate MFR of the first polypropylene (PP1) 2 Therefore, it is preferred that the α-nucleated polypropylene composition (n-PP) complies with
[0079] (a) Equation 2, preferably Equation 2a,
[0080]
[0081] in
[0082] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0083] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0084] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0085] and optionally, in accordance with
[0086] (b) Equation 3, preferably Equation 3a,
[0087] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0088] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0089] in
[0090] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0091] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0092] Therefore, the present invention particularly relates to an α-nucleated polypropylene composition (n-PP) comprising
[0093] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0094] (b) a second polypropylene (PP2),
[0095] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0096] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0097] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0098] in
[0099] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0100] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0101] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0102] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0103] (ii) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0104] (iii) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 132,1 red zone defects measured by CNMR,
[0105] (iv) a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0106] (v) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0107] Wherein still further, the α-nucleated polypropylene composition (n-PP) complies with
[0108] (i) Equation 2, preferably Equation 2a,
[0109]
[0110] in
[0111] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0112] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0113] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0114] and optionally, in accordance with
[0115] (ii) Equation 3, preferably Equation 3a,
[0116] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0117] 75 g / 10min>MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0118] in
[0119] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0120] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0121] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%, more preferably the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer.
[0122] As mentioned above, the α-nucleated polypropylene composition (n-PP) consists essentially of a first polypropylene (PP1) and a second polypropylene (PP2). Further, the comonomer content of the α-nucleated polypropylene composition (n-PP) does not exceed 0.75 mol%. Therefore, the maximum amount of comonomer in one of the two polypropylenes (PP1) and (PP2) can be 3 mol%, assuming that the other polypropylene is a propylene homopolymer. In fact, only the second polypropylene (PP2) can have such a high amount. However, the content of comonomer is 3 mol% means that the polypropylene is still crystalline. In other words, the α-nucleated polypropylene composition (n-PP) mainly contains two crystalline polypropylenes. Therefore, the α-nucleated polypropylene composition (n-PP) contains two miscible polypropylenes. Therefore, it is preferred that the α-nucleated polypropylene composition (n-PP) is single-phase. In other words, the α-nucleated polypropylene composition (n-PP) does not include polymer components that are immiscible with each other, because this is the case of a multiphase propylene copolymer. In contrast to a single-phase system, a multiphase system comprises a continuous polymer phase, such as polypropylene, wherein other immiscible polymers (such as elastomeric polymers) are dispersed as inclusions. On the contrary, the polypropylene system containing a polypropylene matrix and inclusions as a second polymer phase would be referred to as multiphase and is not a part of the present invention. For example, the presence of a second polymer phase or so-called inclusions can be seen by a high-resolution microscope (such as an electron microscope or an atomic force microscope) or by dynamic mechanical thermal analysis (DMTA). In particular, in DMTA, the presence of a multiphase structure can be identified by the presence of at least two different glass transition temperatures.
[0123] Accordingly, the present invention particularly relates to an α-nucleated single-phase polypropylene composition (n-PP) comprising
[0124] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2(230°C; 2.16 kg),
[0125] (b) a second polypropylene (PP2),
[0126] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0127] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0128] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0129] in
[0130] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0131] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0132] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0133] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg);
[0134] (ii) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5;
[0135] (iii) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR;
[0136] (iv) a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0137] (v) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0138] Wherein still further, the α-nucleated polypropylene composition (n-PP) complies with
[0139] (vi) Equation 2, preferably Equation 2a,
[0140]
[0141] in
[0142] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0143] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0144] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0145] and optionally, in accordance with
[0146] (vii) Equation 3, preferably Equation 3a,
[0147] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0148] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0149] in
[0150] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0151] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0152] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%, more preferably the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is an α-nucleated propylene homopolymer.
[0153] The α-nucleated polypropylene composition (n-PP) according to the present invention can be further defined by its melting and crystallization behavior. The α-nucleated polypropylene composition (n-PP) according to the present invention is characterized in particular by a relatively small gap between the melting temperature and the crystallization temperature. For defining the melting and crystallization temperatures, the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) is always used. p,m and the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c Therefore, it is especially preferred that the α-nucleated polypropylene composition (n-PP) has a maximum melting peak temperature T p,m , which is quite high for metallocene produced polypropylene. Therefore, it is preferred that the α-nucleated polypropylene composition (n-PP) according to the present invention has
[0154] (a) Highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,as well as
[0155] (b) The highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0156] wherein further, the nucleated polypropylene composition (n-PP) complies with equation 1, preferably equation 1a,
[0157] 22 ℃ <Tp,m- Tp,c <33 ℃ (1)
[0158] 23℃ <Tp,m-Tp,c<30℃(1a)
[0159] in
[0160] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step) p,m [℃], and
[0161] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [℃].
[0162] Therefore, the present invention particularly relates to an α-nucleated polypropylene composition (n-PP), the α-nucleated polypropylene composition (n-PP) comprising
[0163] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0164] (b) a second polypropylene (PP2), and
[0165] (c) an α-nucleating agent,
[0166] in
[0167] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0168] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0169] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0170] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0171] (ii) the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,
[0172] (iii) the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0173] (iv) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0174] (v) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR,
[0175] (vi) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0176] Wherein further, the nucleated polypropylene composition (n-PP) complies with
[0177] (vii) Equation 1, preferably Equation 1a,
[0178] 22 ℃ <Tp,m- Tp,c <33 ℃ (1)
[0179] 23℃ <Tp,m-Tp,c<30℃(1a)
[0180] in
[0181] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step) p,m [℃], and
[0182] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [°C], wherein optionally, still further, the α-nucleated polypropylene composition (n-PP) complies with
[0183] (viii) Equation 2, preferably Equation 2a,
[0184]
[0185] in
[0186] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0187] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0188] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0189] (ix) and optionally, conforming to Equation 3, preferably Equation 3a,
[0190] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0191] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0192] in
[0193] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0194] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0195] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase, even more preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol-%, most preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer.
[0196] Therefore, the present invention particularly relates to an α-nucleated polypropylene composition (n-PP) comprising
[0197] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0198] (b) a second polypropylene (PP2),
[0199] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0200] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0201] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0202] in
[0203] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0204] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0205] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0206] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0207] (ii) the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,
[0208] (iii) the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0209] (iv) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0210] (v) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR,
[0211] (vi) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0212] Wherein further, the nucleated polypropylene composition (n-PP) complies with
[0213] (vii) Equation 1, preferably Equation 1a,
[0214] 22 ℃ <Tp,m- Tp,c <33 ℃ (1)
[0215] 23℃ <Tp,m-Tp,c<30℃(1a)
[0216] in
[0217] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step) p,m [℃], and
[0218] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c[°C], wherein optionally, still further, the α-nucleated polypropylene composition (n-PP) complies with
[0219] (viii) Equation 2, preferably Equation 2a,
[0220]
[0221] in
[0222] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0223] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0224] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0225] (ix) and further, optionally, conforming to Equation 3, preferably Equation 3a,
[0226] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0227] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0228] in
[0229] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0230] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0231] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase, even more preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol-%, most preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer.
[0232] The alpha-nucleated polypropylene composition (n-PP) according to this invention can be further defined by its high stiffness and low haze.
[0233] Accordingly, it is preferred that the α-nucleated polypropylene composition (n-PP) has a flexural modulus measured according to ISO 178 on injection molded specimens in the range of 1950 to 2250 MPa and / or a haze measured according to ASTM D1003-00 on injection molded plaques of 1 mm thickness below 10%, more preferably in the range of 5.0 to below 10.0%. Accordingly, all previously defined embodiments additionally have a flexural modulus measured according to ISO 178 on injection molded specimens in the range of 1950 to 2250 MPa and optionally a haze measured according to ASTM D1003-00 on injection molded plaques of 1 mm thickness below 10%, more preferably in the range of 5.0 to below 10.0%.
[0234] As mentioned above, the first polypropylene (PP1) and the second polypropylene (PP2) of the α-nucleated polypropylene composition (n-PP) are produced in a sequential polymerization process using a specific metallocene catalyst. Therefore, the first polypropylene (PP1) and the second polypropylene (PP2) of the α-nucleated polypropylene composition (n-PP) must be produced using a metallocene catalyst as disclosed in WO 2019 / 179959, which is incorporated herein by reference.
[0235] The metallocene catalyst complex for the production of the first polypropylene (PP1) and the second polypropylene (PP2) of the α-nucleated polypropylene composition (n-PP) is in particular defined by formula (I):
[0236]
[0237] In the complex of formula (I), it is preferred that if Mt is Zr or Hf, preferably Zr; each X is a sigma ligand. Most preferably, each X is independently a hydrogen atom, a halogen atom, a C 1 -C 6 Alkoxy or R' group, wherein R' is C 1 -C 6alkyl, phenyl or benzyl group. Most preferably, X is a chlorine, benzyl or methyl group. Preferably, the two X groups are identical. The most preferred options are two chlorides, two methyl groups or two benzyl groups, especially two chlorides. For further preferred definitions of residues, reference is made to WO 2019 / 179959.
[0238] In particular, preferred metallocene catalyst complexes are:
[0239] Racemic-trans-dimethylsilylene[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacene-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride (MC-1);
[0240] Racemic-trans-dimethylsilylene[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacene-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylindene-1-yl]zirconium dichloride (MC-2);
[0241] Racemic-trans-dimethylsilylene[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacene-1-yl][2-methyl-4-(3',5'-di-tert-butylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride (MC-3).
[0242] The corresponding dimethyl zirconium analogs of the three catalysts defined above are also possible, but not preferred. The most preferred catalyst is the one used in the examples of the present invention, namely MC-2.
[0243] Catalyst
[0244] In order to form an active catalytic species, it is usually necessary to employ a cocatalyst which is well known in the art. Here, a cocatalyst system comprising a boron-containing cocatalyst and an aluminoxane cocatalyst is used in combination with the metallocene catalyst complex defined above.
[0245] Typical aluminoxane cocatalysts are prior art. A preferred aluminoxane is methylaluminoxane (MAO). Since the aluminoxanes used as cocatalysts according to the invention are not pure compounds due to the way they are prepared, the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.
[0246] As mentioned above, the aluminoxane cocatalyst is used in combination with a boron-containing cocatalyst.
[0247] Boron-based cocatalysts of interest include those of formula (Z)
[0248] BY 3 (Z),
[0249] Wherein Y is the same or different and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkaryl group, an aralkyl group, a halogenated alkyl group or a halogenated aryl group, each group having 1 to 10 carbon atoms in the alkyl group and 6 to 20 carbon atoms in the aryl group or each group having fluorine, chlorine, bromine or iodine. Preferred examples of Y are methyl, propyl, isopropyl, isobutyl or trifluoromethyl, unsaturated groups such as aryl or halogenated aryl groups (e.g., phenyl, tolyl, benzyl group, p-fluorophenyl, 3,5-difluorophenyl, pentachlorophenyl, pentafluorophenyl, 3,4,5-trifluorophenyl and 3,5-bis(trifluoromethyl)phenyl)). Preferred options are trifluoroborane, triphenylborane, tri(4-fluorophenyl)borane, tri(3,5-difluorophenyl)borane, tri(4-fluoromethylphenyl)borane, tri(2,4,6-trifluorophenyl)borane, tri(pentafluorophenyl)borane, tri(tolyl)borane, tri(3,5-dimethyl-phenyl)borane, tri(3,5-difluorophenyl)borane and / or tri(3,4,5-trifluorophenyl)borane. Particular preference is given to tri(pentafluorophenyl)borane.
[0250] Preferred ionic compounds that can be used include triethylammonium tetra(phenyl)borate, tributylammonium tetra(phenyl)borate, trimethylammonium tetra(tolyl)borate, tributylammonium tetra(tolyl)borate, tributylammonium tetra(pentafluorophenyl)borate, tripropylammonium tetra(dimethylphenyl)borate, tributylammonium tetra(trifluoromethylphenyl)borate, tributylammonium tetra(4-fluorophenyl)borate, N,N-dimethylcyclohexylammonium tetra(pentafluorophenyl)borate, N,N-dimethylbenzylammonium tetra(pentafluorophenyl)borate, N,N-dimethylanilinium tetra(phenyl)borate, N,N-diethylanilinium tetra(pentafluorophenyl)borate, N,N-dimethylanilinium tetra(pentafluorophenyl)borate, N,N-di(propyl)ammonium tetrakis(pentafluorophenyl)borate, di(cyclohexyl)ammonium tetrakis(pentafluorophenyl)borate, triphenylphosphonium tetrakis(phenyl)borate, triethylphosphonium tetrakis(phenyl)borate, diphenylphosphonium tetrakis(phenyl)borate, tri(methylphenyl)phosphonium tetrakis(phenyl)borate, tri(dimethylphenyl)phosphonium tetrakis(phenyl)borate, triphenylcarbeniumtetrakis(pentafluorophenyl)borate or ferroceniumtetrakis(pentafluorophenyl)borate.
[0251] Preferred are triphenylcarbonium tetrakis(pentafluorophenyl)borate, N,N-dimethylcyclohexyl ammonium tetrakis(pentafluorophenyl)borate or N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate. Certain boron cocatalysts are particularly preferred. Preferred borates include trityl ions. Therefore, it is particularly preferred to use N,N-dimethylammonium-tetrakispentafluorophenylborate and Ph 3 CB(PhF 5 ) 4 and their analogs.
[0252] Especially preferred is the combination of a borate cocatalyst such as trityl tetrakis(pentafluorophenyl)borate and methylaluminoxane (MAO).
[0253] Suitable amounts of promoters are well known to the skilled person.
[0254] The molar ratio of boron to the metal ion of the metallocene may be in the range of 0.5:1 to 10:1 mol / mol, preferably in the range of 1:1 to 10:1, especially in the range of 1:1 to 5:1 mol / mol.
[0255] The molar ratio of Al in the aluminoxane to the metal ion in the metallocene may be in the range of 1:1 to 2000:1 mol / mol, preferably in the range of 10:1 to 1000:1, and more preferably in the range of 50:1 to 500:1 mol / mol.
[0256] Catalyst manufacturing
[0257] The metallocene catalyst complex can be used as a catalyst for propylene polymerization in combination with a suitable cocatalyst, for example in a solvent such as toluene or an aliphatic hydrocarbon (ie for polymerization in solution), as is well known in the art. Preferably, the polymerization of propylene occurs in the condensed phase or gas phase.
[0258] The catalyst of the present invention can be used in supported or unsupported form. The particulate support material used is preferably an organic or inorganic material, such as silicon dioxide, aluminum oxide or zirconium oxide or a mixed oxide, such as silicon dioxide-alumina, in particular silicon dioxide, aluminum oxide or silicon dioxide-alumina. It is preferred to use a silicon dioxide support. The skilled person knows the procedures required for supporting the metallocene catalyst.
[0259] Particularly preferably, the support is a porous material so that the complex can be loaded into the pores of the support, for example using methods similar to those described in WO 94 / 14856, WO 95 / 12622 and WO 2006 / 097497. The particle size is not critical, but is preferably in the range of 5 to 200 pm, more preferably in the range of 20 to 80 pm. The use of these supports is conventional in the art.
[0260] Alternatively, no support is used at all. Such catalysts can be prepared in solution, for example in an aromatic solvent such as toluene, by contacting the metallocene (as a solid or as a solution) with a cocatalyst such as methylaluminoxane or borane or a borate predissolved in an aromatic solvent, or by adding the dissolved catalyst components sequentially to the polymerization medium.
[0261] Furthermore, no external carrier may be used, but the catalyst is still present in the form of solid particles. Thus, no external support material, such as an inert organic or inorganic carrier, for example silica as described above, is used.
[0262] In order to provide the catalyst in solid form, but without the use of an external support, it is preferred to use a liquid / liquid emulsion system. The full disclosure of the necessary process can be found in WO 03 / 051934, which is incorporated herein by reference.
[0263] The most preferred catalyst system is defined in the Examples section below (Single Site Catalyst System 1 (SSCS1)).
[0264] The polymerization conditions in the sequential polymerization of the first polypropylene (PP1) and the second polypropylene (PP2) of the α-nucleated polypropylene composition (n-PP) are not specific and are well known to the skilled person. Typically, the first polypropylene (PP1) is produced in a slurry reactor, while the second polypropylene (PP2) is produced in a gas phase reactor in the presence of the first polypropylene (PP1). For such a multistage process, a preferred process is a "loop-gas phase" process, such as the one developed by Borealis A / S of Denmark (known as Technology) is described, for example, in patent literature, such as EP 0 887 379, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479, WO 00 / 68315, WO 2015 / 082379 or WO 2015 / 011134.
[0265] As is known, a prepolymerization may take place prior to the main polymerization.
[0266] The prepolymerization can be carried out in any type of continuously operating polymerization reactor. The prepolymerization can be carried out in a slurry polymerization or a gas phase polymerization reactor, preferably in a loop prepolymerization reactor.
[0267] In a preferred embodiment the prepolymerization is carried out as a bulk slurry polymerization in liquid propylene, ie the liquid phase comprises mainly propylene with minor amounts of other reactants and optionally inert components dissolved therein.
[0268] The prepolymerization is carried out in a continuously operated reactor with an average residence time of 5 to 90 minutes. Preferably, the average residence time is in the range of 10 to 60 minutes, more preferably in the range of 15 to 45 minutes.
[0269] The prepolymerization reaction is usually carried out at a temperature of 0 to 50°C, preferably 10 to 45°C, more preferably 15 to 35°C.
[0270] The pressure in the prepolymerization reactor is not critical, but must be high enough to keep the reaction mixture in the liquid phase, and is generally selected so that the pressure is higher than or equal to the pressure in the subsequent polymerization. Thus, the pressure may be from 20 to 100 bar, for example from 30 to 70 bar.
[0271] If a prepolymerization step is carried out, all of the catalyst mixture is introduced into the prepolymerization step.
[0272] Exact control of the prepolymerization conditions and reaction parameters is within the skill of the art.
[0273] As mentioned above the first polypropylene (PP1) is preferably produced in a slurry phase polymerisation step, ie in liquid phase.
[0274] The temperature in the slurry polymerization is typically from 50 to 110° C., preferably from 60 to 100° C., in particular from 65 to 95° C. The pressure is from 1 to 150 bar, preferably from 10 to 100 bar.
[0275] The slurry polymerization can be carried out in any known reactor for slurry polymerization. Such reactors include continuous stirred tank reactors and loop reactors. Particularly preferably, the polymerization is carried out in a loop reactor. Loop reactors are generally known in the art and examples are given, for example, in US-A-4582816, US-A-3405109, US-A-3324093, EP-A-479186 and US-A-5391654.
[0276] The residence time may vary within the reactor zones identified above. In one embodiment, the residence time in a slurry reactor (e.g., a loop reactor) is in the range of 0.5 to 5 hours, e.g., 0.5 to 2 hours, while the residence time in a gas phase reactor is typically in the range of 1 to 8 hours, e.g., 1.5 to 4 hours.
[0277] As is well known in the art, other components may also be introduced into the slurry polymerisation stage. Thus, hydrogen is added to control the molecular weight of the polymer.
[0278] The slurry polymerization stage is followed by a gas phase polymerization stage, in which the second polypropylene (PP2) is produced. Preferably, the slurry is introduced directly into the gas phase polymerization zone without a flash step between the stages. Such direct feeding is described in EP-A-887379, EP-A-887380, EP-A-887381 and EP-A-991684.
[0279] Ie the reaction product of the slurry phase polymerization preferably carried out in a loop reactor, ie the first polypropylene (PP1), is then transferred to a subsequent gas phase reactor, wherein a second polypropylene (PP2) is produced.
[0280] The polymerization in the gas phase can be carried out in a fluidized bed reactor, a fast fluidized bed reactor or a sedimentation bed reactor or any combination of these reactors. When a combination of reactors is used, the polymer is then transferred from one polymerization reactor to another polymerization reactor. However, it is preferred that the second polypropylene (PP2) is produced in a gas phase reactor.
[0281] Typically, the gas phase reactor is operated at a temperature in the range 50 to 100° C., preferably in the range 65 to 95° C. The pressure is suitably in the range 10 to 40 bar, preferably 15 to 30 bar.
[0282] According to the present invention the first polypropylene (PP1) is produced in a first step, i.e. in a first reactor, e.g. in a loop reactor, while the second polypropylene (PP2) is produced in a subsequent step, i.e. in a second reactor, e.g. in a gas phase reactor. In case the process for the polymerization of the first polypropylene (PP1) and the second polypropylene (PP2) further contains a prepolymerization step, then the first polypropylene (PP1) according to the present invention is the polymer produced in the prepolymerization as well as the polymer produced in the subsequent first step, in the first reactor, e.g. in a loop reactor, while the second polypropylene (PP2) is the product of the second reactor, e.g. in a gas phase reactor. The amount of polymer produced in the prepolymerization step is relatively small compared to the amount produced in the first reactor and thus has no large influence on the properties of the polypropylene from the first reactor.
[0283] The first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 15 to 90 g / 10 min, like in the range of 18 to 80 g / 10 min. 2 (230°C; 2.16kg).
[0284] Further, if the α-nucleated polypropylene composition (n-PP) contains a comonomer, the comonomer is required to be selected from the group consisting of ethylene, 1-butene and 1-hexene. Further, the comonomer content in the α-nucleated polypropylene composition (n-PP) should not exceed 0.75 mol%. Therefore, the first polypropylene (PP1) may also contain a comonomer selected from the group consisting of ethylene, 1-butene and 1-hexene. However, the comonomer content of the first polypropylene (PP1) does not exceed 1.25 mol%. It is particularly preferred that the first polypropylene (PP1) is a propylene homopolymer or a propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%. It is particularly preferred that the first polypropylene (PP1) is a propylene homopolymer.
[0285] Accordingly, it is especially preferred that the first polypropylene (PP1) is a propylene homopolymer having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min. 2 (230°C; 2.16 kg). It is particularly preferred that the first polypropylene (PP1) is a propylene homopolymer having a melt flow rate MFR measured according to ISO 1133 in the range of 15 to 90 g / 10 min, like in the range of 18 to 80 g / 10 min. 2 (230°C; 2.16kg).
[0286] Similar to the first polypropylene (PP1), the second polypropylene (PP2) may contain a comonomer. In this case, the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene. Further, the comonomer content in the α-nucleated polypropylene composition (n-PP) should not exceed 0.75 mol%. Therefore, the comonomer content of the second polypropylene (PP2) does not exceed 3.0 mol%. It is particularly preferred that the second polypropylene (PP1) is a propylene homopolymer or a propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%. It is particularly preferred that the second polypropylene (PP2) is a propylene homopolymer.
[0287] Accordingly, it is especially preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 55 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 20 to 90 g / 10 min. 2(230°C; 2.16 kg), and wherein further, the first polypropylene (PP1) and the second polypropylene (PP2) each themselves have a comonomer content in the range of 0.1 to 0.6 mol-% and both polymers contain the same comonomer selected from the group consisting of ethylene, 1-butene and 1-hexene. It is particularly preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 65 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 20 to 90 g / 10 min. 2 (230°C; 2.16 kg), and wherein further the first polypropylene (PP1) and the second polypropylene (PP2) are propylene-1-butene copolymers, each of the two polymers having a comonomer content in the range of 0.1 to 0.6 mol%.
[0288] It is particularly preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 55 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 20 to 90 g / 10 min. 2 (230°C; 2.16 kg), and wherein further both the first polypropylene (PP1) and the second polypropylene (PP2) are propylene homopolymers.
[0289] Melt flow rate MFR of α-nucleated polypropylene composition (n-PP) 2 (230° C.; 2.16 kg) substantially different from the melt flow rate MFR of the first polypropylene (PP1) 2 (230°C; 2.16 kg). Therefore, the α-nucleated polypropylene composition (n-PP) complies with equation 3, preferably equation 3a,
[0290] MFR (n-PP)- MFR (PP1)>35 g / 10min (3)
[0291] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0292] in
[0293] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2(230°C; 2.16 kg);
[0294] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0295] Thus, the melt flow rate MFR of the second polypropylene (PP2) is 2 (230°C; 2.16 kg) must be higher than the melt flow rate MFR of the first polypropylene (PP1) 2 (230°C; 2.16 kg). It is particularly preferred that the melt flow rate MFR of the second polypropylene (PP2) is 2 (230° C.; 2.16 kg) is in the range of 250 to 2000 g / 10 min, preferably in the range of 300 to 1800 g / 10 min. These values are calculated as mentioned in the experimental part.
[0296] Accordingly, it is especially preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 55 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 15 to 90 g / 10 min. 2 (230° C.; 2.16 kg), and the second polypropylene (PP2) has a melt flow rate MFR in the range of 250 to 2000 g / 10 min, preferably in the range of 300 to 1800 g / 10 min 2 (230°C; 2.16 kg), and wherein further, the first polypropylene (PP1) and the second polypropylene (PP2) each themselves have a comonomer content in the range of 0.1 to 0.6 mol-%, and both polymers contain the same comonomer selected from the group consisting of ethylene, 1-butene and 1-hexene. It is particularly preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 55 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 15 to 90 g / 10 min. 2 (230° C.; 2.16 kg), and the second polypropylene (PP2) has a melt flow rate MFR in the range of 200 to 2000 g / 10 min, preferably in the range of 300 to 1800 g / 10 min 2(230°C; 2.16 kg), and wherein further the first polypropylene (PP1) and the second polypropylene (PP2) are propylene-1-butene copolymers, each of the two polymers having a comonomer content in the range of 0.1 to 0.6 mol%.
[0297] It is particularly preferred that the α-nucleated polypropylene composition (n-PP) comprises the first polypropylene (PP1) and the second polypropylene (PP2) in a weight ratio in the range of 75 / 25 to 55 / 45, wherein the first polypropylene (PP1) has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min, preferably in the range of 15 to 90 g / 10 min. 2 (230° C.; 2.16 kg), and the second polypropylene (PP2) has a melt flow rate MFR in the range of 200 to 2000 g / 10 min, preferably in the range of 300 to 1800 g / 10 min 2 (230°C; 2.16 kg), and wherein further both the first polypropylene (PP1) and the second polypropylene (PP2) are propylene homopolymers.
[0298] Therefore, the present invention particularly relates to an α-nucleated polypropylene composition (n-PP), which is an α-nucleated propylene homopolymer, wherein the α-nucleated polypropylene composition (n-PP) comprises
[0299] (a) a first polypropylene (PP1) which is a propylene homopolymer and has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0300] (b) a second polypropylene (PP2) which is a propylene homopolymer and optionally has a melt flow rate MFR in the range of 200 to 2000 g / 10 min. 2 (230°C; 2.16 kg), and
[0301] (c) an α-nucleating agent,
[0302] in
[0303] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0304] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0305] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0306] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0307] (ii) the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,
[0308] (iii) the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0309] (iv) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0310] (v) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR,
[0311] (vi) optionally a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0312] (vii) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0313] Wherein further, the nucleated polypropylene composition (n-PP) complies with
[0314] (x) Equation 1, preferably Equation 1a,
[0315] 22℃ <Tp,m-Tp,c<33℃ (1)
[0316] 23℃ <Tp,m-Tp,c<30℃ (1a)
[0317] in
[0318] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step)p,m [℃], and
[0319] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [°C], wherein still further, the α-nucleated polypropylene composition (n-PP) complies with
[0320] (xi) Equation 2, preferably Equation 2a,
[0321]
[0322] in
[0323] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0324] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0325] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0326] (xii) and further, optionally, conforming to Equation 3, preferably Equation 3a,
[0327] MFR(n-PP)-MFR(PP1)>35g / 10min (3)
[0328] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min(3a)
[0329] in
[0330] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0331] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0332] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase, even more preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol-%, most preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer.
[0333] Therefore, the present invention particularly relates to an α-nucleated polypropylene composition (n-PP), which is an α-nucleated propylene homopolymer, wherein the α-nucleated polypropylene composition (n-PP) comprises
[0334] (a) a first polypropylene (PP1) which is a propylene homopolymer and has a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0335] (b) a second polypropylene (PP2) which is a propylene homopolymer and optionally has a melt flow rate MFR in the range of 200 to 2000 g / 10 min. 2 (230°C; 2.16 kg), and
[0336] (c) 0.01 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent,
[0337] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0338] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°Cp,m , more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0339] in
[0340] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0341] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0342] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0343] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0344] (ii) the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,
[0345] (iii) the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0346] (iv) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0347] (v) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR,
[0348] (vi) optionally a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0349] (vii) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0350] Wherein further, the nucleated polypropylene composition (n-PP) complies with
[0351] (xiii) Equation 1, preferably Equation 1a,
[0352] 22℃ <Tp,m-Tp,c<33℃ (1)
[0353] 23℃ <Tp,m-Tp,c<30℃ (1a)
[0354] in
[0355] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step) p,m [℃], and
[0356] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [°C], wherein still further, the α-nucleated polypropylene composition (n-PP) complies with
[0357] (xiv) Equation 2, preferably Equation 2a,
[0358]
[0359] in
[0360] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0361] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0362] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0363] (xv) and further, optionally, conforming to Equation 3, preferably Equation 3a,
[0364] MFR(n-PP)-MFR(PP1)>35g / 10min (3)
[0365] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min (3a)
[0366] in
[0367] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0368] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0369] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase, even more preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol-%, most preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer.
[0370] As mentioned above the α-nucleated polypropylene composition (n-PP) must comprise an α-nucleating agent. α-Nucleating agents are well known in the art. Reference is made to "Plastics Additives Handbook", 6th edition, pages 967 to 990.
[0371] Generally, the α-nucleating agent promotes the formation of crystallization nuclei when the melt of polypropylene solidifies, thereby increasing the crystallization rate and temperature of the α-nucleated polypropylene compared to the non-α-nucleated polypropylene.
[0372] The α-nucleated polypropylene composition (n-PP) typically contains up to 2.0 wt.% of α-nucleating agent. Preferably, the lower limit of the α-nucleating agent is 0.001 wt.%. Preferably, the polypropylene composition (n-PP) comprises 0.005 to 1.0 wt.%, more preferably 0.01 to 0.8 wt.%, still more preferably 0.1 to 0.8 wt.% of α-nucleating agent. The weight percentages in the preceding paragraph refer to the total amount of α-nucleating agent present in the α-nucleated polypropylene composition (n-PP).
[0373] Preferred examples of α-nucleating agents are disclosed in “Pasties Additives Handbook” by Hans Zweifel, 6th edition, pages 967-990.
[0374] Among all α-nucleating agents, bis[2,4,8,10-tetrakis(1,1-dimethylethyl)-6-hydroxy-12H-dibenzo-[d,g]-dioxaphosphat-6-oxy]hydroxyaluminum-based nucleating agents (such as ADK NA-21, NA-21E, NA-21F, etc., 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate (ADK NA-11), bis[2,2'-methylene-bis(4,6-di-tert-butylphenyl)-phosphoric acid]hydroxyaluminum), sorbitol-based nucleating agents (i.e., di(alkylbenzylidene)sorbitol, such as 1,3:2,4-25 dibenzylidene sorbitol, 1,3:2,4-di(4-methylbenzylidene)sorbitol, 1,3:2,4-di(4-ethylbenzylidene)sorbitol and l,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol), and nonitol derivatives (such as 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol), and benzyltriamide (such as substituted 1,3,5-benzenetricarboxamides, such as N,N',N"-tri-tert-butyl-1,3,5-benzenetricarboxamide, N,N',N"-tricyclohexyl-1,3,5-benzenetricarboxamide and N-[3,5-bis-(2,2-dimethyl-propionylamino)-phenyl]-2,2-dimethyl-propionamide), among which 1,3:2,4-di(4-methylbenzylidene)sorbitol and N-[3,5-bis-(2,2-dimethyl-propionylamino)-phenyl]-2,2-dimethyl-propionamide and polymer nucleating agents selected from the group consisting of vinylcycloalkane polymers and vinylalkane polymers are particularly preferred.
[0375] Particularly preferred are soluble nucleating agents such as Millad 3988 (1,3:2,4-di(4-ethylbenzylidene)sorbitol and 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol) and Millad NX8000 (1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol).
[0376] It is particularly preferred that the α-nucleating agent present in the α-nucleated polypropylene composition (n-PP) is selected from the group consisting of polyvinylcyclohexane (p-VCH), 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol and bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS), wherein further, the total amount of the α-nucleating agent is in the range of 0.1 to 0.8 wt.-%, based on the total amount of the α-nucleated polypropylene composition (n-PP).
[0377] Accordingly, the present invention in particular relates to an α-nucleated polypropylene composition (n-PP) comprising, preferably consisting of, the following components,
[0378] (a) a first polypropylene (PP1) having a melt flow rate MFR measured according to ISO 1133 in the range of 10 to 100 g / 10 min 2 (230°C; 2.16 kg),
[0379] (b) a second polypropylene (PP2),
[0380] (c) 0.1 to 0.8 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of an α-nucleating agent selected from the group consisting of polyvinylcyclohexane (p-VCH), 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol and bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS),
[0381] (d) 0.05 to 1.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of additives other than α-nucleating agents, and
[0382] (e) optionally 0.5 to 4.0 wt.-%, based on the α-nucleated polypropylene composition (n-PP), of one or more propylene homopolymers different from the polypropylenes (PP1) and (PP2), wherein the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min. 2 (230°C; 2.16 kg), preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), and a maximum melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m, more preferably, the one or more propylene homopolymers have a melt flow rate MFR measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min 2 (230°C; 2.16 kg), the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C p,m , and no detectable 13 C NMR measurement of 2,1-erythro regiodefects,
[0383] in
[0384] - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and
[0385] the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-based on the α-nucleated polypropylene composition (n-PP),
[0386] Wherein further, the α-nucleated polypropylene composition (n-PP) has
[0387] (i) Melt flow rate MFR measured according to ISO 1133 in the range of 40 to 190 g / 10 min 2 (230°C; 2.16 kg),
[0388] (ii) the highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,
[0389] (iii) the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c ,
[0390] (iv) a molecular weight distribution (MWD) in the range of 3.5 to 5.5, preferably in the range of 4.0 to 5.5,
[0391] (v) in the range of >0.35 to 0.85 mol %, preferably in the range of 0.50 to 0.85 mol % 13 2,1 red zone defects measured by CNMR,
[0392] (vi) optionally a pentad isotacticity [mmmm] of at least 99.0%, preferably at least 99.2%, and
[0393] (vii) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene,
[0394] Wherein further, the nucleated polypropylene composition (n-PP) complies with
[0395] (viii) Equation 1, preferably Equation 1a,
[0396] 22℃ <Tp,m-Tp,c<33℃ (1)
[0397] 23℃ <Tp,m-Tp,c<30℃ (1a)
[0398] in
[0399] “T p,m " is the highest melting peak temperature T measured by DSC (scanning rate of 10 °C / min; second heating step) p,m [℃], and
[0400] “T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [°C], wherein still further, the α-nucleated polypropylene composition (n-PP) complies with (ix) equation 2, preferably equation 2a,
[0401]
[0402] in
[0403] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0404] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0405] “[(PP1) / (n-PP)]” is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP);
[0406] (x) and further, optionally, conforms to Equation 3, preferably Equation 3a,
[0407] MFR(n-PP)-MFR(PP1)>35g / 10min (3)
[0408] 75g / 10min>MFR(n-PP)-MFR(PP1)>35g / 10min (3a)
[0409] in
[0410] "MFR(n-PP)" is the melt flow rate MFR of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133 2 (230°C; 2.16 kg);
[0411] "MFR(PP1)" is the melt flow rate MFR of the first polypropylene (PP1) measured according to ISO 1133 2 (230°C; 2.16kg).
[0412] Preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase, even more preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol-%, most preferably, the α-nucleated polypropylene composition (n-PP) as defined in the preceding paragraph is single-phase and is an α-nucleated propylene homopolymer.
[0413] The present invention also relates to a thin wall injection molded article consisting of the α-nucleated polypropylene composition (n-PP) as defined above, wherein the thin wall injection molded article has a wall thickness of at most 1.0 mm, preferably in the range of 0.1 to 1.0 mm, more preferably in the range of 0.3 to 0.9 mm, yet more preferably in the range of 0.4 to 0.7 mm. The manufacture of thin wall injection molded articles is well known in the art, for example as described in Nello Pasquini "Polypropylene Handbook", 2nd edition, pages 441 / 442.
[0414] Hereinafter, the present invention is further described by way of examples.
[0415] A. Measurement Method
[0416] Unless defined otherwise, the following definitions of terms and assays apply to the above general description of the invention including the claims, as well as to the following examples.
[0417] Quantification of microstructure by NMR spectroscopy
[0418] Quantitative nuclear magnetic resonance (NMR) spectroscopy is used to quantify the isotacticity and regioregularity of the propylene homopolymers.
[0419] Use for 1 H and 13 Quantitative measurements were recorded in solution on a Bruker Advance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz, respectively. 13 C{ 1 H} NMR spectroscopy. Nitrogen was used for all pneumatics and all spectra were 13 C-optimized 10 mm extended temperature probe recorded at 125 °C.
[0420] For propylene homopolymer, approximately 200 mg of the material was dissolved in 1,2-tetrachloroethane-d 2 (TCE-d 2 ). To ensure a homogeneous solution, the NMR tube was further heated in a rotary oven for at least 1 hour after initial sample preparation in a heating block. After insertion into the magnet, the tube was rotated at 10 Hz. This setting was chosen primarily for the high resolution required for quantification of stereoregularity distribution (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V.; Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251). Standard single pulse excitation was used, using NOE and double-layer WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 11289). A total of 8192 (8k) transient values were collected for each spectrum.
[0421] Quantification was performed using a dedicated computer program 13 C{ 1 H} NMR spectra are processed, integrated, and relevant quantitative properties are determined from the integrals.
[0422] For propylene homopolymers, all chemical shifts are internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.
[0423] Characteristic signals corresponding to regio defects (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253; Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157; Cheng, HN, Macromolecules 17 (1984), 1950) or comonomers were observed.
[0424] The stereoregularity distribution is quantified by integrating the methyl region between 23.6 and 19.7 ppm, correcting for any sites not associated with the stereo sequence of interest (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V., Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251).
[0425] Specifically, the quantitative effects of regio defects and comonomers on the tacticity distribution were corrected by subtracting representative regio defect and comonomer integrals from a specific integrated region of the stereo sequence.
[0426] Isotacticity is determined at the pentad level and is reported as the percentage of isotactic pentad (mmmm) sequences relative to all pentad sequences:
[0427] [mmmm]% = 100*(mmmm / sum of all pentads)
[0428] The presence of the 2,1 erythro regio defect is indicated by the presence of two methyl sites at 17.7 and 17.2 ppm and confirmed by other characteristic sites. No characteristic signals corresponding to other types of regio defects were observed (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253).
[0429] The amount of 2,1-erythro regiodefects was quantified using the average integral of the two characteristic methyl sites at 17.7 and 17.2 ppm:
[0430] P 21e =(I e6 +I e8 ) / 2
[0431] 1,2 The amount of primary insertion propene was quantified based on the methyl region and corrections were made for sites not involved in the primary insertion and for primary insertion sites not included in the region:
[0432] P 12 =I CH3 +P 12e
[0433] The total amount of propene is quantified as the sum of the primary inserted propene and all other regio defects present:
[0434] P 总 =P 12 +P 21e
[0435] The mole percentage of 2,1 erythro regio defects relative to all propylene is quantified:
[0436] [21e] mol% = 100*(P 21e / P 总 )
[0437] The method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) was used to 13 C{ 1 The comonomer fraction is quantified by integrating multiple signals over the entire spectral area in the H} spectrum. This approach was chosen for its robustness and ability to account for the presence of regio defects when required. The integration area was slightly adjusted to improve applicability over the entire range of comonomer content encountered.
[0438] For systems where only isolated ethylene in the PPEPP sequence is observed, the method of Wang et al. was modified to reduce the effect of non-zero integrals at sites known to be absent. This approach reduces the overestimation of ethylene content in such systems and is achieved by reducing the number of sites used to determine absolute ethylene content to:
[0439] E=0.5(Sββ+Sβγ+Sβδ+0.5(Sαβ+Sαγ)).
[0440] Using this set of sites, the corresponding integral equation becomes:
[0441] E=0.5(I H +I G +0.5(I C +I D )).
[0442] The same symbols used in the article by Wang et al. are used (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). The equations for absolute propylene content are not modified.
[0443] Calculate the mole percentage of comonomer incorporation from the mole fraction:
[0444] E[mol %]=100*fE.
[0445] Calculate the weight percent comonomer incorporation from the mole fractions:
[0446] E[weight%]=100*(fE*28.06) / ((fE*28.06)+((1-fE)*42.08)).
[0447] Melt flow rate
[0448] The melt flow rate (MFR) is determined according to ISO 1133 and is expressed in g / 10 min. The MFR indicates the flowability of a polymer and, therefore, its processability. The higher the melt flow rate, the lower the viscosity of the polymer. MFR of polypropylene 2 It was measured at a temperature of 230°C and a load of 2.16 kg.
[0449] Calculate the melt flow rate MFR of the second polypropylene (PP2) 2 (230℃):
[0450]
[0451] in
[0452] w(PP1) is the weight fraction [in wt. %] of the first polypropylene (PP1),
[0453] w(PP2) is the weight fraction [in wt. %] of the second polypropylene (PP2),
[0454] MFR(PP1) is the melt flow rate MFR of the first polypropylene (PP1) 2 (230℃) [g / 10min],
[0455] MFR(PP) is the melt flow rate MFR of the reactor powder of polypropylene (PP) 2 (230°C) [in g / 10 min], MFR(PP2) is the calculated melt flow rate MFR of the second polypropylene (PP2) 2 (230℃) [in g / 10min].
[0456] Molecular weight
[0457] The molecular weight averages (Mz, Mw and Mn) and molecular weight distribution (MWD) (i.e., Mw / Mn) are determined by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99 using the following formula:
[0458]
[0459] where Ai and Mi are the chromatographic peak slice area and the molecular weight (MW) of the polyolefin.
[0460] The PolymerChar GPC instrument equipped with an infrared (IR) detector was used with 3×Olexis and 1×Olexis guard columns from Polymer Laboratories and 1,2,4-trichlorobenzene (TCB, stabilized with 250 mg / l of 2,6-di-tert-butyl-4-methyl-phenol) as solvent at 160°C and with a constant flow rate of 1 ml / min. 200 μL of sample solution was injected for each analysis. Universal calibration (according to ISO 16014-2:2003) was used to calibrate the column set using at least 15 narrow MWD polystyrene (PS) standards in the range of 0.5 kg / mol to 11500 kg / mol. The MarkHouwink constants of PS, PE and PP used were as described according to ASTM D 6474-99. All samples were prepared by dissolving 5.0 to 9.0 mg of polymer in 8 ml (at 160 °C) stabilized TCB (same as mobile phase) in the autosampler of the GPC instrument at 160 °C with constant gentle shaking for 2.5 h (for PP) or 3 h (for PE).
[0461] Flexural modulus
[0462] The flexural modulus was determined according to ISO 178 method A (3-point bending test) on 80 mm x 10 mm x 4 mm test specimens. According to this standard, a test speed of 2 mm / min and a span length of 16 times the thickness were used. The test temperature was 23 ± 2 °C. Injection molding was performed according to ISO 19069-2, and for all materials a melt temperature of 200 °C was used, regardless of the material melt flow rate.
[0463] Haze
[0464] Haze is measured according to ASTM D1003-00 at a melt temperature of 230°C on a 60×60×1 mm2 molded according to EN ISO 1873-2 3 Measured on plate.
[0465] DSC analysis, melting peak temperature (T p,m ) and heat of fusion (H f ), crystallization peak temperature (T p,c ) and heat of crystallization (H c ): Measurements were performed on 5 to 7 mg samples using a TA Instrument Q200 Differential Scanning Calorimeter (DSC). The DSC was run according to ISO 11357 / Part 3 / Method C2 with a heating / cooling / heating cycle in the temperature range of -30 to +225°C at a scanning rate of 10°C / min. The highest crystallization peak temperature (T p,c ) and heat of crystallization (H c ) is determined by the cooling step, while the maximum melting peak temperature (T p,m ) and heat of fusion (H f ) is determined by the second heating step.
[0466] Xylene soluble fraction at room temperature (XCS, weight %):
[0467] The amount of polymer soluble in xylene is determined according to ISO 16152; 5th edition; 2005-07-01 at 25°C.
[0468] B. Preparation
[0469] Catalysts used in the examples of the present invention
[0470] Catalyst complex
[0471] The following metallocene complexes have been used as described in WO 2019 / 179959:
[0472]
[0473] Preparation of MAO-silica supports
[0474] A steel reactor equipped with a mechanical stirrer and a filter screen was flushed with nitrogen, and the reactor temperature was set to 20°C. Next, silica (5.0 kg) of the grade DM-L-303 of AGC Si-Tech Company, pre-calcined at 600°C, was added from the feed bucket, followed by careful nitrogen pressurization and decompression using a manual valve. Then, toluene (22 kg) was added. The mixture was stirred for 15 min. Next, a 30 wt % solution (9.0 kg) of MAO from Lanxess in toluene was added through the feed line at the top of the reactor within 70 min. Then, the reaction mixture was heated to 90°C and stirred for another two hours at 90°C. The slurry was allowed to settle and the mother liquor was filtered off. At 90°C, the catalyst was washed twice with toluene (22 kg), followed by settling and filtering. The reactor was cooled to 60°C and the solid was washed with heptane (22.2 kg). Finally, the SiO treated with MAO was concentrated to 400°C and the solid was washed with heptane (22.2 kg). 2 Drying was carried out at 60°C under nitrogen flow for 2 hours and then under vacuum (-0.5 barg) with stirring for 5 hours.The MAO treated support was collected as a free flowing white powder which was found to contain 12.2% Al by weight.
[0475] Preparation of single active site catalyst system 1 (SSCS1)
[0476] 30 wt % MAO in toluene (0.7 kg) was added via a burette to a nitrogen blanketed steel reactor at 20°C. Toluene (5.4 kg) was then added under stirring. The metallocene complex (93 g) as described above under 2a) was added from a metal cylinder, followed by a rinse with 1 kg of toluene. The mixture was stirred at 20°C for 60 minutes. Trityl tetrakis(pentafluorophenyl)borate (91 g) was then added from a metal cylinder, followed by a rinse with 1 kg of toluene. The mixture was stirred at room temperature for 1 h. The resulting solution was added over 1 hour to the stirred cake of MAO-silica support prepared as described above. The cake was left for 12 hours, followed by a slurry at 60°C under N 2 Dry under flow for 2 h and dry under vacuum (-0.5 bar gauge) with stirring for a further 5 h.
[0477] The dried catalyst was sampled as a pink free-flowing powder containing 13.9% Al and 0.11% Zr.
[0478] Preparation of single active site catalyst system 2 (SSCS2)
[0479] Single-site catalyst system 2 (SSCS2) was prepared according to comparative example (CCS4) of WO 2020 / 239602A1.
[0480] Table 1: Polymerization conditions
[0481]
[0482]
[0483] Table 2: α-nucleated polypropylene composition (n-PP)
[0484] IE1 IE2 IE3 IE4 IE5 IE6 CE1 CE2 Poly1 [weight%] 99.55 97.55 99.35 0 - - - - Poly2 [weight%] - - - 97.55 - - - - Poly3 [weight%] - - - - - - 97.55 - Poly4 [weight%] - - - - - - - 99.35 Poly5 [weight%] - - - - 99.65 - - - Poly6 [weight%] - - - - - 99.65 - - AN1 [weight%] 0.30 0.30 0.50 0.30 - - 0.30 0.50 AN2 [weight%] - - - - 0.20 0.20 - - GE [weight%] 0.10 0.10 0.10 0.10 0.10 0.10 0.10 0.10 AO [weight%] 0.05 0.05 0.05 0.05 0.05 0.05 0.05 0.05 HF955MO [weight%] - 2.00 - 2.00 - - 2.00 - XCS [weight%] 0.84 0.85 0.84 0.80 0.75 0.72 0.58 0.75 2,1 Akashi [mol %] 0.70 0.64 0.71 0.63 0.71 0.72 0.98 0.65 mmmm [%] 99.6 99.6 99.6 99.5 99.32 99.23 99.3 99.5 MWD [-] 4.8 4.8 4.8 4.6 5.5 6.1 3.1 2.8 <![CDATA[MFR 2 ]]> [g / 10min] 138 119 138 136 60 79 65 77 <![CDATA[T p,c ]]> [℃] 130 130 130 129 130 130 126 128 <![CDATA[T p,m ]]> [℃] 158 158 158 157 156 156 154 156 <![CDATA[T p,m -T p,c ]]> [℃] 28 28 28 28 26 26 28 28 FM [MPa] 2070 2077 2114 2036 2014 2074 1780 1835 Haze [%] 8.4 8.5 5.6 8.4 12.8 12.8 7.5 5.0 FM / Fog [MPa / %] 246.4 244.4 377.5 242.4 157.3 162.0 237.3 367.0
[0485] Table 3: α-nucleated polypropylene composition (n-PP); Equation 2
[0486]
[0487] The results of Tables 2 and 3 clearly show that the present invention is superior to the comparative examples in terms of combining high stiffness, high clarity, low solubles content and good processability represented by both high melt flow rate and limited difference between melting temperature and crystallization temperature. The effect of the present invention is achieved by combining a suitable single-site catalyst with a bimodal design of molecular weight distribution by producing polymers with different melt flow rates in consecutive polymerization stages, i.e. loop reactor and gas phase reactor.
[0488] "AN1" is Milliken's commercially available α-nucleating agent Millad NX8000, which contains 1,2,3-trideoxy-4,6:5,7-bis-O-((4-propylphenyl)methylene)nonitol;
[0489] "AN2" is Milliken's commercially available α-nucleating agent Millad 3988, which contains bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS);
[0490] "GE" is a compound with the molecular formula HOCH 2 -CH(OH)-CH 2 -OC(=O)-(CH 2 ) 16 -CH 3 Glycerides;
[0491] "AO" is an antioxidant package consisting of 1 part of pentaerythritol tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate and 2 parts of tris(2,4-di-tert-butylphenyl)phosphite;
[0492] "HF955MO" is a commercially available polypropylene homopolymer from Borealis AG having a melt flow rate MFR of 20 g / 10 min measured according to ISO 1133 2(230° C.; 2.16 kg) and a maximum melting peak temperature T of 165° C. measured by DSC (scanning rate of 10° C. / min; second heating step) p,m .
Claims
1. An α-nucleated polypropylene composition (n-PP), comprising (a) a first polypropylene (PP1) having a melt flow rate MFR2 (230°C; 2.16 kg) measured according to ISO 1133 in the range of 10 to 100 g / 10 min, (b) a second polypropylene (PP2), and (c) an α-nucleating agent, in - a weight ratio between the first polypropylene (PP1) and the second polypropylene (PP2) [(PP1) / (PP2)] is in the range of 75 / 25 to 55 / 45, and - the total amount of the first polypropylene (PP1) and the second polypropylene (PP2) together is at least 94 wt.-%, based on the α-nucleated polypropylene composition (n-PP); Further, the α-nucleated polypropylene composition (n-PP) has (i) a melt flow rate MFR2 (230° C.; 2.16 kg) measured according to ISO 1133 in the range of 40 to 190 g / 10 min; (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 3.5 to 6.5; (iii) in the range of >0.35 to 0.85 mol% 13 2,1 erythro regiodefects measured by C NMR; and (iv) a comonomer content of not more than 0.75 mol %, wherein the comonomer is selected from the group consisting of ethylene, 1-butene and 1-hexene.
2. The α-nucleated polypropylene composition (n-PP) according to claim 1, having (a) Highest melting peak temperature T measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 156 to 160°C p,m ,as well as (b) The highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) in the range of 127 to 135°C p,c , Further, the nucleated polypropylene composition (n-PP) satisfies equation 1 22 ℃ <Tp,m- Tp,c <33 ℃ (1) in "T p,m ” is the highest melting peak temperature T measured by DSC (scanning rate of 10° C. / min; second heating step) p,m [℃], and "T p,c ” is the highest crystallization peak temperature T measured by DSC (scanning rate of 10°C / min; cooling step) p,c [℃].
3. The α-nucleated polypropylene composition (n-PP) according to claim 1 or 2, which satisfies equation 2 in "MFR(n-PP)" is the melt flow rate MFR2 (230°C; 2.16 kg) of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133; "MFR(PP1)" is the melt flow rate MFR2 (230°C; 2.16 kg) of the first polypropylene (PP1) measured according to ISO 1133; "[(PP1) / (n-PP)]" is the amount of the first polypropylene (PP1) in the α-nucleated polypropylene composition (n-PP) divided by the amount of the α-nucleated polypropylene composition (n-PP).
4. The α-nucleated polypropylene composition (n-PP) according to any one of the preceding claims, which satisfies Equation 3 MFR (n-PP)- MFR (PP1)>35 g / 10min (3) in "MFR(n-PP)" is the melt flow rate MFR2 (230°C; 2.16 kg) of the α-nucleated polypropylene composition (n-PP) measured according to ISO 1133; "MFR(PP1)" is the melt flow rate MFR2 (230°C; 2.16 kg) measured according to ISO 1133 of the first polypropylene (PP1).
5. The α-nucleated polypropylene composition (n-PP) according to any one of the preceding claims, having (a) a xylene cold soluble fraction (XCS) measured at 25° C. according to ISO 16152 in the range of 0.1 to 1.0 wt.-%, and (b) optionally a pentad isotacticity [mmmm] of at least 98.0%.
6. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims having a melt flow rate MFR2 (230°C; 2.16 kg) measured according to ISO 1133 in the range of 45 to below 150 g / 10 min.
7. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, wherein the α-nucleated polypropylene composition (n-PP) is single-phase.
8. An α-nucleated polypropylene composition (n-PP) according to any one of the preceding claims having (a) a flexural modulus measured according to ISO 178 in the range of 1950 to 2250 MPa, preferably in the range of 500 to 2500 MPa, and (b) Optionally, a haze measured according to ASTM D1003-00 in the range of 5.0 to less than 10.0%.
9. The α-nucleated polypropylene composition (n-PP) according to any one of the preceding claims, wherein (a) the first polypropylene (PP1) and the second polypropylene (PP2) are propylene homopolymers, or (b) The first polypropylene (PP1) and the second polypropylene (PP2) are propylene-1-butene copolymers having a 1-butene content in the range of 0.1 to 0.6 mol%.
10. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, wherein the α-nucleated polypropylene composition (n-PP) is an α-nucleated propylene homopolymer or an α-nucleated propylene-1-butene copolymer having a 1-butene content in the range of 0.1 to 0.6 mol%, preferably an α-nucleated propylene homopolymer.
11. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, wherein the second polypropylene (PP2) has a melt flow rate MFR2 in the range of 250 to 2000 g / 10 min.
12. An α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, wherein the composition further comprises one or more propylene homopolymers having a melt flow rate MFR2 (230°C; 2.16 kg) measured according to ISO 1133 in the range of 1.0 to 25.0 g / 10 min and a maximum melting peak temperature T 20 measured by DSC (scanning rate of 10°C / min; second heating step) in the range of 162 to 169°C. p,m , wherein the total amount of the one or more propylene homopolymers is in the range of 0.5 to 4.0 wt.-%, based on the total amount of the α-nucleated polypropylene composition (n-PP).
13. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, comprising at least one α-nucleating agent selected from the group consisting of polymeric nucleating agents, sorbitol based nucleating agents, nonitol based nucleating agents and benzyltriamide based nucleating agents, wherein the total amount of α-nucleating agents is in the range of 0.001 to 2.0 wt.-%, based on the total amount of the α-nucleated polypropylene composition (n-PP).
14. The α-nucleated polypropylene composition (n-PP) according to anyone of the preceding claims, wherein the one or more α-nucleating agents present in the α-nucleated polypropylene composition (n-PP) are selected from the group consisting of polyvinylcyclohexane (p-VCH), 1,2,3-trideoxy-4,6;5,7-bis-O-[(4-propylphenyl)methylene]nonitol and bis-(3,4-dimethylbenzylidene)-sorbitol (DMDBS), wherein further the total amount of the one or more α-nucleating agents is in the range of 0.1 to 0.8 wt.-%, based on the total amount of the α-nucleated polypropylene composition (n-PP).
15. A thin walled injection moulded article comprising, preferably consisting of, the α-nucleated polypropylene composition (n-PP) according to any one of the preceding claims, wherein the thin walled injection moulded article has a wall thickness of at most 1.0 mm.