Composition and injection molded article

By coating magnetic powder with a layer and rationally selecting the powder diameter and ratio in the injection molding method, the problems of high core loss and powder deformation in pressure molding are solved, resulting in high-performance magnetic injection molded bodies suitable for magnetic cores of magnetic components.

CN118749014APending Publication Date: 2024-10-08TOKIN CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280090040.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-24
Filing Date
2022-12-20
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When using magnetic powder from iron-based nanocrystalline alloys to produce molded bodies through pressure molding, core loss is significant and the magnetic powder is prone to deformation.

Method used

A composition comprising magnetic powder and thermoplastic resin is used, wherein the magnetic powder portion has a coating layer, which may contain glass, silicone resin and coupling agent. The composition uses iron-based nanocrystalline alloy and Fe-Si alloy, and the powder diameter and ratio are controlled. The molded body is prepared by injection molding.

Benefits of technology

An injection-molded part with excellent magnetic properties was obtained, core loss was reduced, mechanical strength and flowability were improved, powder deformation during pressure molding was avoided, and it is suitable for magnetic cores of various magnetic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749014A_ABST
    Figure CN118749014A_ABST
Patent Text Reader

Abstract

Provided are a composition suitable for injection molding, from which a molded article having excellent magnetic properties and an injection molded article having excellent magnetic properties can be obtained. A composition includes a magnetic powder (10), at least a portion of which has a coating layer (20), and a thermoplastic resin (30).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition and an injection molded product. Background Art

[0002] As a magnetic core for various magnetic elements such as choke coils and inductors, a molded body containing a composition of a binder and a magnetic powder is known. As a method for manufacturing a molded body, a press molding method using a thermosetting resin as a binder is well known (for example, Patent Document 1).

[0003] As magnetic powders having excellent magnetic properties, Fe-based nanocrystalline alloys having magnetic properties such as low coercive force, low magnetostriction, high magnetic permeability, and high saturation magnetic flux density are disclosed in Patent Documents 2 to 4.

[0004] On the other hand, in Patent Document 5, a method for injection molding a composition containing a thermoplastic resin and a magnetic powder is disclosed.

[0005] Prior art documents

[0006] Patent Literature

[0007] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2010-10426

[0008] Patent Document 2: Japanese Unexamined Patent Application Publication No. 2012-12699

[0009] Patent Document 3: Japanese Unexamined Patent Application Publication No. 2010-150665

[0010] Patent Document 4: International Patent Publication No. WO2011 / 24580

[0011] Patent Document 5: Japanese Unexamined Patent Application Publication No. 2019-102713 Summary of the invention

[0012] Technical Problems Solved by the Invention

[0013] For example, in the case of producing a molded body by press-forming using magnetic powder of an iron-based nanocrystalline alloy, core loss (iron loss) can be larger than designed in some cases. As a result of extensive research, the inventors have found that in some cases, magnetic powders can deform during press-forming.

[0014] In order to solve the problem, an object of the present invention is to provide a composition suitable for injection molding and from which a molded body excellent in magnetic properties can be obtained, and an injection molded body excellent in magnetic properties.

[0015] Solutions to technical problems

[0016] The composition of the present invention comprises a magnetic powder and a thermoplastic resin, and at least a portion of the magnetic powder has a coating layer.

[0017] In the above composition, the coating layer may include at least one selected from glass, silicone resin and coupling agent.

[0018] In the above composition, the coating layer may include at least one selected from glass and silicone resin.

[0019] In the above composition, the coating layer may include a coupling agent.

[0020] In the above composition, the coating layer may include: a first layer, the first layer comprising one or more selected from glass and silicone resin; and a second layer, the second layer comprising a coupling agent.

[0021] In the above composition, the magnetic powder may include an iron-based nanocrystalline alloy.

[0022] In the above composition, the magnetic powder may include a Fe-Si alloy.

[0023] In the above composition, the magnetic powder may include a first magnetic powder having a median diameter of 1 μm to 50 μm and a second magnetic powder having a median diameter of 10 μm to 300 μm, and the median diameter of the second magnetic powder is larger than that of the first magnetic powder.

[0024] In the above composition, the first magnetic powder may be an Fe-based nanocrystalline alloy, and the second magnetic powder may be an Fe-Si alloy.

[0025] The mass ratio between the first magnetic powder and the second magnetic powder of the above composition may be 95:5 to 50:50.

[0026] In the above composition, the glass may include phosphate glass.

[0027] The composition may have a melt flow rate of 80 g / 10 min or more at 330° C.

[0028] The above composition can be used for injection molding.

[0029] The injection molded article of the present invention is an injection molded article of the composition of the present invention.

[0030] The core loss of the injection molded body measured at a frequency of 20 kHz and an applied magnetic flux density of 100 mT can be 350 kW / m 3 the following.

[0031] The core loss of the injection molded body measured at a frequency of 100 kHz and an applied magnetic flux density of 100 mT can be 2800 kW / m 3 the following.

[0032] The magnetic permeability maintenance rate of the injection molded article under the conditions of a frequency of 100 kHz and a magnetic field intensity of 8 kA / m may be 83% or more.

[0033] The radial crushing strength of the injection molded body may be 40 MPa or more.

[0034] The resistance value of the injection molded body can be 1×10 13 Ω or more.

[0035] Effects of the Invention

[0036] The present invention provides a composition suitable for injection molding, a molded body having excellent magnetic properties obtained from the composition, and an injection molded body having excellent magnetic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 is a schematic cross-sectional view showing an example of a magnetic powder having a coating layer.

[0038] Figure 2 is another schematic cross-sectional view showing an example of the magnetic powder having a coating layer.

[0039] Figure 3 is a schematic cross-sectional view showing an example of an injection molded body.

[0040] Figure 4 This is a SEM (scanning electron microscope) image of a schematic cross section of the injection molded article in Example 1.

[0041] Figure 5 This is a SEM image of a schematic cross section of the injection molded article in Example 1. DETAILED DESCRIPTION

[0042] Hereinafter, the present invention will be described by way of embodiments of the present invention, although the present invention according to the claims is not limited to the following embodiments.

[0043] For the convenience of explanation, the following description and drawings are appropriately simplified. For the purpose of explanation, the scale of each element in the drawings may be greatly different.

[0044] In addition, unless otherwise stated, the term "to" expressing a numerical range includes both the lower limit and the upper limit.

[0045] [Composition]

[0046] The composition according to the present invention includes a magnetic powder and a thermoplastic resin, and at least a portion of the magnetic powder has a coating layer.

[0047] By using the magnetic powder with a coating layer, the present composition improves the fluidity of the composition when the thermoplastic resin is heated to a melting point or above. Therefore, the composition is suitable for injection molding. Since the molded body can be formed by injection molding, the deformation problem of the magnetic powder that may occur during the press molding does not occur, so that a molded body with excellent magnetic properties can be obtained. Further, by using the magnetic powder with a coating layer to improve the adhesion between the magnetic powder and the thermoplastic resin, the effect of improving the mechanical strength (such as radial crushing strength) of the molded body can also be obtained.

[0048] The composition includes at least a magnetic powder having a coating layer and a thermoplastic resin, and may further include other components within the range in which the effects of the present invention are exerted. Each component will be described below.

[0049] <Magnetic powder>

[0050] The magnetic powder can be appropriately selected from known magnetic powders used for cores of magnetic elements according to the required magnetic properties. From the viewpoint of magnetic properties, soft magnetic powders such as soft magnetic powders containing iron (Fe) as a main component (50 at % or more) are preferred.

[0051] The composition of the magnetic powder can be iron alone or an alloy containing iron and other elements. Examples of other elements include boron (B), nitrogen (N), carbon (C), oxygen (O), phosphorus (P), silicon (Si), nickel (Ni), chromium (Cr), aluminum (Al), copper (Cu), titanium (Ti), zirconium (Zr), hafnium (Hf), niobium (Nb), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), cobalt (Co), manganese (Mn), silver (Ag), zinc (Zn), tin (Sn), arsenic (As), antimony (Sb), bismuth (Bi), yttrium (Y) and rare earth elements such as samarium (Sm).

[0052] Specific examples of soft magnetic powders include carbonyl iron, Fe-Si alloys, Fe-Ni alloys, Fe-Si-Cr alloys, Fe-Si-Al alloys, iron-based amorphous alloy powders containing at least Fe-B, and iron-based nanocrystalline alloys containing at least Fe-BP-Cu. Here, the iron-based amorphous alloy refers to an amorphous iron-based alloy without a crystal structure. Furthermore, the iron-based nanocrystalline alloy refers to an alloy obtained by heat-treating the iron-based amorphous alloy to precipitate fine α-Fe crystals in the amorphous phase. The magnetic powder can be used alone or in combination of two or more.

[0053] In the present composition, the magnetic powder preferably comprises an iron-based nanocrystalline alloy and / or an Fe-Si alloy, and more preferably comprises an iron-based nanocrystalline alloy. In the iron-based nanocrystalline alloy, the highly magnetized α-Fe phase is in the form of fine nanocrystals.

[0054] The mixed phase including the amorphous phase having positive magnetostriction and the α-Fe phase having negative magnetostriction exists to reduce magnetocrystalline anisotropy, and reduces magnetostriction, thereby making it possible to obtain good magnetic characteristics with high saturation magnetic flux density (Bs) and low loss.

[0055] (Iron-based nanocrystalline alloy)

[0056] An iron-based nanocrystalline alloy containing at least Fe, B, P and Cu is preferred. Specifically, from the perspective of magnetic properties and ease of manufacture, an iron-based nanocrystalline alloy having a composition satisfying the following formula (1) or (2) is preferred. In addition, B, P, Si and C are elements that contribute to the formation of an amorphous phase, and Cu is an element that contributes to nanocrystallization.

[0057] Fe w B x P y Cu z (1)

[0058] Fe a B b Si c P d C e Cu f (2)

[0059] In formula (1), w is 76 at% to 88 at%, x is 4 at% to 13 at%, y is 1 at% to 10 at%, z is 0.5 at% to 1.5 at%, and w+x+y+z is 100 at%,

[0060] In formula (2), a is 76 at % to 88 at %, b is 4 at % to 13 at %, c is 0 at % to 8 at %, d is 0.1 to 10, e is 0 at % to 5 at %, f is 0.4 at % to 1.4 at %, and a+b+c+d+e+f is 100 at %.

[0061] Similar to formulas (1) and (2), other elements such as Ti, Zr, Hf, Nb, Ta, Mo, W, Cr, Co, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, Y, N, O, S and rare earth elements may be contained in an amount of 3 at% or less relative to the entire composition. In this case, w in formula (1) and a in formula (2) represent the total content ratio of iron and other elements.

[0062] From the perspective of magnetic properties, injection moldability and ease of production of the alloy, the shape of the iron-based nanocrystalline alloy is preferably spherical. In the present embodiment, spherical means that the aspect ratio of the alloy observed from the cross-sectional SEM (scanning electron microscope) image of the injection molded body is 1 to 3, preferably 1 to 2.

[0063] Further, from the perspective of magnetic properties, injection moldability and ease of production of the alloy, the median diameter (D50) of the iron-based nanocrystalline alloy is preferably 1 μm to 50 μm. In addition, in this embodiment, the median diameter is a value calculated from the particle size distribution measured by laser diffraction.

[0064] The iron-based nanocrystalline alloy can be produced with reference to, for example, Japanese Unexamined Patent Application Publication No. 2012-12699, Japanese Unexamined Patent Application Publication No. 2010-150665, and International Patent Publication No. WO2011 / 24580. Specifically, it can be produced by preparing an alloy composition satisfying formula (1) or (2) and having an amorphous phase as a main phase, pulverizing the composition by atomization, etc., and heat-treating the powder at a predetermined temperature. According to the above method, spherical particles with a median diameter of 1 μm to 50 μm can be obtained.

[0065] (Fe-Si alloy)

[0066] As the magnetic powder, it is preferable to use Fe-Si alloy alone or to use Fe-Si in combination with an alloyed Fe-based nanocrystalline alloy. By using Fe-Si alloy, an injection molded body having higher magnetic permeability and lower loss can be obtained.

[0067] The ratio of Si in the Fe-Si alloy is preferably 2% by mass to 10% by mass, more preferably 3% by mass to 7% by mass, relative to the total amount of the Fe-Si alloy.

[0068] The Fe-Si alloy may further contain other elements such as Cr, Al, Mn, Ni, C, O, N, S, P, B and Cu. The content of other elements is preferably 3% by mass or less, more preferably 1% by mass or less, relative to the total amount of the Fe-Si alloy.

[0069] From the viewpoints of magnetic properties and injection moldability, the shape of the Fe-Si alloy is preferably spherical.

[0070] Further, from the viewpoints of magnetic characteristics and injection moldability, the median diameter (D50) of the Fe-Si alloy is preferably 1 μm to 500 μm.

[0071] The Fe-Si alloy can be obtained by preparing the above-mentioned composition and pulverizing it by an atomization method, etc. A commercial product having a desired composition and particle size can also be used.

[0072] In this embodiment, the magnetic powder used may be a combination of a first magnetic powder having a median diameter of 1 μm to 50 μm and a second magnetic powder having a median diameter of 10 μm to 300 μm, preferably 60 μm to 300 μm. By combining a second magnetic powder having a larger median diameter than the first magnetic powder, the composition can obtain excellent fluidity and injection moldability even with a high proportion of magnetic powder. In the case of combining the first magnetic powder and the second magnetic powder, the proportion of the magnetic powder in the composition may be 70% to 85% by volume, preferably 70% to 80% by volume.

[0073] Furthermore, the ratio between the median diameter d502 of the second magnetic powder and the median diameter d501 of the first magnetic powder (d502 / d501) is preferably 1.5 or more. When d502 / d501 is 1.5 or more, the composition tends to have improved fluidity.

[0074] In this case, for ease of production, the first magnetic powder is preferably an Fe-based nanocrystalline alloy, and the second magnetic powder is preferably an Fe-Si alloy.

[0075] From the viewpoint of magnetic properties and fluidity, the mass ratio between the first magnetic powder and the second magnetic powder is preferably 95:5 to 50:50, more preferably 80:20 to 70:30.

[0076] On the other hand, when the proportion of the magnetic powder in the composition is less than 70% by volume, it is preferred to use the iron-based nanocrystalline alloy alone from the viewpoint of magnetic properties.

[0077] When an iron-based nanocrystalline alloy is used alone, from the perspective of balancing injection moldability and magnetic properties, the proportion of magnetic powder in the composition is preferably 60 volume % to 70 volume %, more preferably 62 volume % to 68 volume %, relative to 100 volume % of the composition.

[0078] <Coating layer>

[0079] In the present embodiment, at least a portion of the magnetic powder has a coating layer. Figure 1 and Figure 2 is a schematic cross-sectional view showing an example of a magnetic powder 100 having a coating layer. Figure 1 and Figure 2 In the example shown in FIG. 1 , the coating layer 20 is formed on the surface of the magnetic powder 10. The coating layer 20 may be Figure 1 The single layer of the example in, or the coating layer 20 can be as Figure 2 Thus, it has a laminated structure of two or more layers including the first layer 1 and the second layer 2. In addition, the coating layer 20 may be a single layer including two or more components. Further, the coating layer 20 may cover the entire surface of the magnetic powder, or may have intermittent portions.

[0080] The material of the coating layer is preferably selected from materials having at least one or more functions including improved fluidity, improved insulation properties, and improved adhesion to a thermoplastic resin.

[0081] Specific examples thereof include glass, silicone resin, and coupling agents.

[0082] From the viewpoint of insulation, the coating layer preferably contains glass or silicone resin. By providing the coating layer containing glass or silicone resin, direct contact between magnetic particles is suppressed, thereby improving insulation performance.

[0083] Examples of glass include silicate glass, borate glass, borosilicate glass and phosphate glass. Among them, phosphate glass is preferred. By providing a coating layer containing phosphate glass, the fluidity of the composition is improved. In addition, phosphate glass may contain other inorganic oxides such as ZnO, SiO2, Bi2O3 and Al2O3.

[0084] The coating amount of the glass and the silicone resin is preferably 0.3% to 5% by volume, more preferably 0.5% to 3% by volume, relative to 100% by volume of the present composition.

[0085] From the perspective of improving adhesion to the thermoplastic resin and improving the mechanical strength of the injection molded body, the coating layer preferably contains a coupling agent. Examples of the coupling agent include silane coupling agents, titanium coupling agents, and zirconium coupling agents, and silane coupling agents are preferred. Considering affinity, the organic group of the silane coupling agent can be appropriately selected corresponding to the type of the thermoplastic resin.Specific examples of the silane coupling agent include methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, dimethoxydiphenylsilane, trifluoropropyltrimethoxysilane, n-propyltriethoxysilane, vinyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, and 3-methacryloxypropylmethyldimethoxysilane. ne), N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-ureidopropyltrialkoxysilane, 3-isocyanatopropyltriethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate and 3-mercaptopropylmethyldimethoxysilane, which can be used alone or in combination of two or more.

[0086] The coating amount of the coupling agent is preferably 0.3 to 3 volume %, more preferably 0.5 to 2 volume %, and further preferably 0.6 to 1.2 volume %, based on 100 volume % of the present composition.

[0087] From the viewpoints of fluidity, insulation and improved adhesion to thermoplastic resins, the coating layer preferably has a laminated structure having a first layer comprising one or more selected from glass and silicone resins and a second layer comprising a coupling agent, and more preferably the first layer comprises glass. In this case, as Figure 2 In the example shown, the laminated structure includes magnetic powder 10, a first layer 1, and a second layer 2. The coupling agent in the second layer has excellent adhesion to the glass or silicone resin in the first layer and excellent affinity to the thermoplastic resin, thereby improving the adhesion between the magnetic powder and the thermoplastic resin, resulting in improved mechanical strength of the injection molded body.

[0088] The method for forming the coating layer can be appropriately selected according to the type of coating layer material. In the case of a glass agent, a glass layer can be formed on the surface of the magnetic powder by a thin film forming method such as a sol-gel method, or by a method of mixing magnetic powder and glass powder under mechanical stress. In the case of an organosilicon resin or a coupling agent, a solution or dispersion containing a coating layer material can be prepared and applied by various coating methods or impregnation methods.

[0089] <Thermoplastic resin>

[0090] The thermoplastic resin can be appropriately selected according to the injection moldability, heat resistance and mechanical strength required for the injection molded body. Specific examples of the thermoplastic resin include polyvinyl chloride, polystyrene, acrylonitrile-butadiene-styrene (ABS) resin, polyamide including aromatic polyamide, polyethylene, polypropylene, methacrylic resin, polycarbonate, polyimide, polyamide-imide, polyetheretherketone and polyphenylene sulfide, which can be used alone or in combination of two or more.

[0091] In the present embodiment, from the viewpoint of mechanical strength and the like, the thermoplastic resin preferably includes polyamide, polyphenylene sulfide, or polyetheretherketone, and more preferably includes polyamide.

[0092] From the viewpoint of both injection moldability and magnetic properties, the proportion of the thermoplastic resin in the composition is preferably 20% to 40% by volume, more preferably 25% to 35% by volume, and still more preferably 30% to 35% by volume, relative to 100% by volume of the present composition.

[0093] <Optional Ingredients>

[0094] The present composition may further contain other ingredients within the scope of the effects exhibited by the present invention. Examples of other ingredients include function-imparting agents such as antioxidants, lubricants, ultraviolet absorbers, metal deactivators, HALS, stabilizers such as stabilizers for PVC, plasticizers, flame retardants, nucleating agents, fillers, compatibilizers, curing agents, photoinitiators, antistatic agents, antifogging agents, conductive agents, transparent agents, lubricants, and antibacterial agents, which can be used alone or in combination of two or more.

[0095] From the viewpoint of injection moldability, the melt flow rate of the present composition at 330° C. is preferably 80 g / 10 minutes or more, more preferably 90 g / 10 minutes or more. The melt flow rate is a value measured using a melt indexer in accordance with JIS K 7210, using a mold (nozzle) having an inner diameter of 1.05 mm and a length of 4 mm, under the conditions of a measurement temperature of 330° C. and a test pressure of 20 kg.

[0096] The melt flow rate of the present composition can be adjusted according to the type and content ratio of the thermoplastic resin, the particle size and content ratio of the magnetic powder, and the like.

[0097] The method for producing the present composition is not particularly limited, and for example, the composition can be obtained by adding the magnetic powder having a coating layer and each component used as necessary to a heated thermoplastic resin and kneading the mixture.

[0098] The present composition has excellent injection moldability due to the combination of the magnetic powder having the coating layer and the thermoplastic resin, and is suitable as an injection molding composition for forming cores of various magnetic elements.

[0099] [Injection molded body]

[0100] The injection molded article of the present invention is a molded article obtained by injection molding the composition. Figure 3 : is a schematic cross-sectional view showing an example of an injection molded body. Figure 3 As shown in the example of FIG. 2 , the injection molded body 200 is formed in a state where the magnetic powder 100 having a coating layer is dispersed in the thermoplastic resin 30. The injection molded body is a molded body without applying pressure, has excellent magnetic characteristics, and does not have the problem of magnetic powder deformation that may occur during pressure molding.

[0101] Since various components that may be contained in the present injection molded body and their content ratios are the same as those of the above-mentioned composition, their description is omitted here.

[0102] The injection molding method is not particularly limited. For example, the injection molded body can be obtained by filling the cavity of the mold with a molten thermoplastic resin composition with a cylinder and cooling the composition. Alternatively, referring to Japanese Unexamined Patent Application Publication No. 2019-102713, etc., a molded body in which a coil is embedded can be formed.

[0103] The injection molded body can be a low-loss core. For example, the core loss of the injection molded body measured under the conditions of a frequency of 20 kHz and an applied magnetic flux density of 100 mT can be 350 kW / m 3 Below, preferably 310kW / m 3 Below, more preferably 300kW / m 3 the following.

[0104] Furthermore, for example, the core loss of the injection molded body measured under the conditions of a frequency of 100 kHz and an applied magnetic flux density of 100 mT can be 2800 kW / m 3 Below, preferably 2700kW / m 3 Below, more preferably 2400kW / m 3 the following.

[0105] The injection molded body has excellent DC superposition characteristics. For example, the magnetic permeability maintenance rate of the injection molded body under the conditions of a frequency of 100kHz and a magnetic field strength of 8kA / m can be 83% or more, preferably 83.5% or more, and more preferably 85% or more. Note that the magnetic permeability maintenance rate is a value calculated based on the following formula (3) based on the magnetic permeability μ measured under the condition of a magnetic field strength of 0 and the magnetic permeability μ' measured under the above conditions.

[0106] Maintenance rate (%) = (μ' / μ) × 100 (3)

[0107] The present injection molded body has excellent adhesion between the magnetic powder and the thermoplastic resin and has high mechanical strength. For example, the radial crushing strength of the injection molded body can be 35 MPa or more, preferably 40 MPa or more, and more preferably 42 MPa or more. In the present embodiment, the radial crushing strength is a value obtained according to the test method for radial crushing strength in JIS Z2507.

[0108] Furthermore, the injection molded body has excellent insulation properties. For example, the resistance value of the injection molded body can be 1×10 13 Ω or more.

[0109] The injection molded body having the above-mentioned characteristics can be suitably used for any conventionally known applications, for example, can be suitably used as a magnetic core of various magnetic components such as a choke coil and an inductor.

[0110] Example

[0111] The present invention will be specifically described below with reference to Examples and Comparative Examples. However, these descriptions do not limit the present invention.

[0112] (Example 1)

[0113] As magnetic powders, the following iron-based nanocrystalline alloy A and Fe-Si alloy (silicon content: 6.5 mass %, D50: 150 μm) were prepared, and each was coated with 1.9 volume % of phosphate glass relative to 100 volume % of the following composition, thereby forming a coating layer 1. Subsequently, a coating layer 2 was formed with 0.6 volume % of 3-aminopropyltriethoxysilane (silane coupling agent; KBE-903 produced by Shin-Etsu Chemical Co., Ltd.) relative to 100 volume % of the following composition, thereby obtaining a magnetic powder having a coating layer.

[0114] Subsequently, the Fe-based nanocrystalline alloy and the Fe—Si alloy were added to molten aromatic polyamide (thermoplastic resin; PA9T (N1000A) produced by Kuraray Co, Ltd.) at a mass ratio of 8:2 to obtain a composition having a magnetic powder ratio of 70 volume %.

[0115] The composition was injection molded using an injection molding apparatus (STX-10S2V) manufactured by Nissei Plastic Industrial Co., Ltd. to obtain a ring-shaped molded body having an outer diameter of 13 mm and an inner diameter of 8 mm.

[0116] (Examples 2 to 14)

[0117] A formed body having the above-mentioned shape was obtained in the same manner as in Example 1 except that the composition was changed as shown in Tables 1 to 3. In the table, coating layer 1 or coating layer 2 described as "-" means that coating layer 1 or coating layer 2 is not provided and the coating layer is a single layer.

[0118] (Comparative Example 1)

[0119] A formed body having the above-mentioned shape was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1.

[0120] (Comparative Example 2)

[0121] The composition was changed as shown in Table 3, and instead of injection molding, the 2 The molded product was press-molded at a molding pressure of , thereby obtaining a molded product having the same shape as that of Example 1. In addition, the phenolic resin is a thermosetting resin.

[0122] Regarding the compositions, the abbreviations in the table are as follows.

[0123] Alloy A: Iron-based nanocrystalline alloy A (Fe 84.3 B6P9Cu 0.7 (at%), D50: 30 μm)

[0124] Alloy B: Iron-based nanocrystalline alloy B (Fe 84.3 B9P6Cu 0.7 (at%), D50: 30 μm)

[0125] Fe-6.5Si: Fe-Si alloy (silicon content: 6.5 mass%, D50: 150 μm)

[0126] KBE-903: 3-Aminopropyltriethoxysilane

[0127] [evaluate]

[0128] <Melt flow rate (MFR)>

[0129] The melt flow rate of the composition before molding was measured using a melt indexer (melt indexer (C50590 model) produced by Toyo Seiki Seisaku-sho, Ltd.) in accordance with JIS K 7210, under the conditions of a measuring temperature of 330° C. and a test pressure of 20 kg, using a die (nozzle) having an inner diameter of 1.05 mm and a length of 4 mm.

[0130] <density>

[0131] As the density of the molded body, the apparent density is calculated from the volume and weight of the molded body.

[0132] <Radial crushing strength>

[0133] The compact was subjected to a compression test using a small tabletop testing machine (Little SENSTARLS C-02 / 300-2) manufactured by Tokyo Testing Machine Co., Ltd. The radial crushing strength was measured according to the radial crushing strength test method of JIS Z2507, and the radial crushing strength was calculated and evaluated according to formula (4).

[0134] K = [F × De)] / (L × e 2 ): Formula (4)

[0135] K: Radial crushing strength (Mpa)

[0136] F: Maximum load at failure (N)

[0137] L: Length of hollow cylinder (mm)

[0138] D: outer diameter of the hollow cylinder (mm)

[0139] E: Wall thickness of hollow cylinder (mm)

[0140] <Insulation resistance>

[0141] The insulation resistance of the formed body was measured using a resistance meter (B2985A) manufactured by Keysight Technologies by applying a voltage of 100 V between an electrode having a top diameter of 1 mm and the bottom of the formed body.

[0142] <Saturation magnetization Js>

[0143] The calculation was performed using a BH curve obtained by a BH analyzer (BH5501) manufactured by Denshijiki Industry Co., Ltd.

[0144] <Magnetic permeability μ, μ' and maintenance rate Δμ>

[0145] To measure the magnetic permeability, 10 turns of copper wire were wound around a ring-shaped body with an outer diameter of 13 mm and an inner diameter of 8 mm. The magnetic permeability μ or μ' was measured using an LCR meter (4284A) manufactured by HP at a frequency of 100 kHz and a magnetic field strength of 0 or 8 kA / m, and the maintenance rate Δμ was obtained according to formula (3).

[0146] <Core loss Pcv>

[0147] The core loss was measured using a BH analyzer (SY8219) manufactured by Iwatsu Electric Co, Ltd. under the following two conditions: Pcv1 and Pcv2 are described in order.

[0148] (1) Frequency: 20kHz, applied magnetic flux density: 100mT

[0149] (2) Frequency: 100kHz, applied magnetic flux density: 100mT

[0150] The evaluation results are shown in Tables 1 to 3.

[0151] Table 1

[0152]

[0153] Table 2

[0154]

[0155] Table 3

[0156]

[0157] In addition, the molded body in Example 1 was cut and the cut surface was observed using SEM. The SEM image is as follows: Figure 4 and 5 As shown. Figure 5 As shown, the molded body in Example 1 is excellent in wettability of the thermoplastic resin to the coating layer, so that the coating layer and the thermoplastic resin are in close contact with each other. Figure 4 As shown, although minute gaps were observed between the magnetic powder and the thermoplastic resin of the molded body in Example 1, it can be presumed that the magnetic powder and the thermoplastic resin as a whole were in close contact with each other, thereby improving the strength.

[0158] The composition and molded body using magnetic powder without a coating layer in Comparative Example 1 are inferior to those of the examples in terms of melt flow rate, insulation resistance, DC superposition characteristics and core loss.

[0159] In Comparative Example 2, pressure molding was performed using a thermosetting resin, and the results showed that the core loss was particularly large even when the same magnetic powder as in Example 1 was used. This is presumably due to deformation of the magnetic powder during pressure molding.

[0160] The compact in Example 4 using the magnetic powder having the silane coupling agent coating layer showed particularly excellent radial crushing strength and suppression of core loss compared to Comparative Example 1.

[0161] Furthermore, the molded body using the magnetic powder having the phosphate glass coating layer in Example 3 particularly improved the melt flow rate as compared with Comparative Example 1, and was excellent in suppressing the core loss.

[0162] The injection molded bodies of Examples 1 to 2 and Examples 5 to 15, which were injection molded from the composition comprising the magnetic powder having two coating layers and the thermoplastic resin, exhibited excellent properties in radial crushing strength, insulation resistance, DC superposition characteristics, and core loss.

[0163] Therefore, the injection molded product of the present embodiment can be suitably used as a magnetic core of various magnetic components such as a choke coil and an inductor.

[0164] This application claims priority based on Japanese Patent Application No. 2022-8812 filed on January 24, 2022, and the entire disclosure of which is incorporated herein.

[0165] Reference numerals list

[0166] 1First layer (coating layer)

[0167] 2 Second layer (coating layer)

[0168] 10 Magnetic powder

[0169] 20 coating layer

[0170] 30 Thermoplastic resin

[0171] 100 Magnetic powder with coating

[0172] 200 Injection molded body

Claims

1. A composition comprising a magnetic powder and a thermoplastic resin, in, At least a portion of the magnetic powder has a coating layer.

2. The composition according to claim 1, wherein The coating layer comprises at least one selected from glass, silicone resin and coupling agent.

3. The composition according to claim 1 or 2, wherein The coating layer comprises at least one selected from glass and silicone resin.

4. The composition according to claim 1 or 2, wherein The coating layer includes a coupling agent.

5. The composition according to any one of claims 1 to 4, wherein The coating layer comprises: a first layer comprising one or more selected from glass and silicone resin; and a second layer comprising a coupling agent.

6. The composition according to any one of claims 1 to 5, wherein The magnetic powder includes an iron-based nanocrystalline alloy.

7. The composition according to any one of claims 1 to 6, wherein The magnetic powder includes a Fe-Si alloy.

8. The composition according to any one of claims 1 to 7, wherein The magnetic powder includes a first magnetic powder having a median diameter of 1 μm to 50 μm and a second magnetic powder having a median diameter of 10 μm to 300 μm, and the median diameter of the second magnetic powder is larger than the median diameter of the first magnetic powder.

9. The composition according to claim 8, wherein The first magnetic powder is an iron-based nanocrystalline alloy, and the second magnetic powder is an Fe-Si alloy. 10 . The composition according to claim 8 , wherein a mass ratio between the first magnetic powder and the second magnetic powder in the composition is 95:5 to 50:

50.

11. The composition according to any one of claims 2 to 10, wherein The glass comprises phosphate glass. 12 . The composition according to claim 1 , which has a melt flow rate at 330° C. of 80 g / 10 min or more.

13. The composition according to any one of claims 1 to 12, which is used for injection molding.

14. An injection-molded body of the composition according to any one of claims 1 to 13.

15. The injection molded body according to claim 14, wherein the core loss of the injection molded body measured under the conditions of a frequency of 20 kHz and an applied magnetic flux density of 100 mT is 350 kW / m 3 the following.

16. The injection molded body according to claim 14 or 15, wherein the core loss of the injection molded body measured under the conditions of a frequency of 100 kHz and an applied magnetic flux density of 100 mT is 2800 kW / m 3 the following. 17 . The injection molded article according to claim 14 , wherein the maintenance rate of magnetic permeability of the injection molded article under the conditions of a frequency of 100 kHz and a magnetic field intensity of 8 kA / m is 83% or more. 18 . The injection molded article according to claim 14 , which has a radial crushing strength of 40 MPa or more.

19. The injection molded article according to any one of claims 14 to 18, wherein the resistance value of the injection molded article is 1×10 13 Ω or more.