Composite resin molded article and method for producing same

By using natural fibers to carry spores and nutrients in biodegradable plastics, and increasing the defibrillation parts through melting and mixing, the problems of slow decomposition speed and insufficient mechanical strength of biodegradable plastics in humid environments have been solved, and high-quality plastics have been achieved. Rigid and rapidly decomposing composite resin molded bodies suitable for a variety of industrial and domestic applications.

CN118749015APending Publication Date: 2024-10-08PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092567.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2022-09-21
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Biodegradable plastics decompose slowly in humid environments and have insufficient mechanical strength, which limits their application in mechanical products and industrial products such as automobiles. Moreover, existing technology is difficult to accelerate their decomposition in environments with few microorganisms such as oceans.

Method used

It adopts a composite resin molded body, containing the main agent resin and natural fibers dispersed in it. At least part of the natural fibers is loaded with spores and nutrients, and the defibrillation parts of the fibers are increased through melting and mixing to promote water absorption and absorption in humid environments. break down.

Benefits of technology

It maintains high rigidity and accelerates biodegradation in humid environments, improves the mechanical strength and decomposition speed of biodegradable plastics, and is suitable for industrial products and daily necessities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749015A_ABST
    Figure CN118749015A_ABST
Patent Text Reader

Abstract

A composite resin molded body which contains a base resin and a plurality of natural fibers dispersed in the base resin, and which is characterized in that spores and nutrients are supported on at least some of the plurality of natural fibers, and when the composite resin molded body is taken as 100 mass%, the content of the spores and the nutrients is less than or equal to 100 mass%. The content of the plurality of natural fibers is 10 mass% or more and 99 mass% or less, and a portion of the plurality of natural fibers is exposed on the surface of the composite resin molded article.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a composite resin molded body having excellent mechanical properties and a controlled biodegradation rate in a high-humidity environment, and a method for producing the same. Background Art

[0002] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very cheap, but also easy to shape and lightweight, with a weight only a fraction of that of metals or ceramics. Therefore, general-purpose plastics are used as materials for a variety of daily necessities such as bags, various packages, various containers, and sheets, as well as for industrial parts such as automobile parts and electrical parts, and as materials for daily necessities and sundry goods.

[0003] Due to such circumstances, the amount of plastic waste after use is increasing year by year. Plastic waste is a substance with the characteristic of being difficult to decompose and accumulates in the natural environment, thus causing public nuisance problems such as damage and pollution of the natural environment. In recent years, as one of the strategies to solve these problems, biodegradable plastics that can be decomposed into water and carbon dioxide in the natural environment have been proposed, and it is expected that they will replace general-purpose plastics using petroleum-based raw materials and expand their applications.

[0004] However, biodegradable plastics have disadvantages such as insufficient mechanical strength compared to general-purpose plastics. Therefore, the current situation is that biodegradable plastics do not have sufficient properties required for materials used in various industrial products such as mechanical products such as automobiles and electrical / electronic / information products, and their application range is limited.

[0005] On the other hand, the environment has a great influence on the biodegradation rate of discarded biodegradable plastics. In an environment with few microorganisms such as the ocean, it takes a long time to achieve complete decomposition, and the biodegradability cannot be fully utilized. In order to solve this problem, various methods have been proposed to accelerate the decomposition of discarded biodegradable plastics.

[0006] In order to solve such problems, products in which microorganisms having enzyme activity that decomposes the material are compounded with biodegradable plastics (for example, see Patent Document 1) and methods in which spores having a cell structure that exhibits high durability against external pressure such as high temperature conditions are compounded with biodegradable plastics (for example, see Patent Document 2) are disclosed.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-209587

[0010] Patent Document 2: International Publication No. 2013 / 180124 Summary of the invention

[0011] A composite resin molded body according to one embodiment of the present invention is a composite resin molded body comprising a main resin and a plurality of natural fibers dispersed in the main resin, at least a portion of the plurality of natural fibers carry spores and nutrients, and when the composite resin molded body is set to 100 mass %, the content of the plurality of natural fibers is greater than 10 mass % and less than 99 mass %, and a portion of the plurality of natural fibers are exposed on the surface of the composite resin molded body.

[0012] A method for manufacturing a composite resin molded body according to one embodiment of the present invention includes: a step of preparing spores, nutrients, natural fibers, and a main resin; a step of causing the spores and nutrients to be loaded on the natural fibers; a step of melt-kneading the natural fibers loaded with spores and nutrients together with the main resin to defibrate the natural fibers from the ends in the fiber length direction to obtain a composite resin material having an enlarged specific surface area of ​​the defibrated portion at the ends; and a step of molding the composite resin material to obtain a composite resin molded body. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram showing a cross-sectional structure of a composite resin molded body according to an embodiment.

[0014] Figure 2 It is a schematic diagram showing the cross-sectional structure of natural fibers which are a constituent material of the composite resin molded body according to the embodiment.

[0015] Figure 3 It is a schematic cross-sectional view of a composite resin molded body containing natural fibers having a defibrated portion according to an embodiment.

[0016] Figure 4 It is a schematic diagram of a production process of a composite resin molded body according to an embodiment.

[0017] Figure 5 The figures show the structures and measurement results of composite resin molded bodies of Examples and Comparative Examples of the embodiment. DETAILED DESCRIPTION

[0018] In the method described in Patent Document 1, since microorganisms are directly kneaded into biodegradable plastics, the material is limited to biodegradable plastics that can be molded at a temperature at which the microorganisms can survive.

[0019] On the other hand, the method described in Patent Document 2 has a problem that the molded body needs to be physically destroyed in order to allow the spores to germinate by contacting with water.

[0020] An object of one embodiment of the present disclosure is to solve the above-mentioned conventional problems and to provide a composite resin molded body that maintains high rigidity during use and promotes biodegradation in a humid environment such as the ocean or soil after disposal.

[0021] The first mode of the composite resin molded body is a composite resin molded body containing a main resin and a plurality of natural fibers dispersed in the main resin, at least a portion of the plurality of natural fibers carry spores and nutrients, and when the composite resin molded body is set to 100 mass %, the content of the plurality of natural fibers is greater than 10 mass % and less than 99 mass %, and a portion of the plurality of natural fibers are exposed on the surface of the molded body.

[0022] In the above-mentioned first aspect, at least a part of the plurality of natural fibers in the composite resin molded body of the second aspect may have a moisture content of 5% or more as determined by the method specified in JIS L0105:2020.

[0023] In the first or second aspect described above, the composite resin molded product of the third aspect may be a biodegradable resin containing any one selected from the group consisting of polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylates, and modified starches.

[0024] In any one of the first to third aspects described above, the nutrients of the composite resin molded body of the fourth aspect may include either peptones or extracts.

[0025] In any one of the first to fourth aspects described above, at least a part of the plurality of natural fibers in the composite resin molded body of the fifth aspect may carry spores and nutrients on the surface of the fibers.

[0026] In any one of the first to fifth aspects described above, at least a part of the plurality of natural fibers in the composite resin molded body of the sixth aspect may be cellulose.

[0027] In any one of the first to sixth aspects described above, at least a part of the plurality of natural fibers in the composite resin molded body of the seventh aspect may have a defibrated portion at an end portion in the fiber length direction.

[0028] The manufacturing method of the composite resin molded body of the eighth embodiment includes: the step of preparing spores, nutrients, natural fibers, and a main resin; the step of causing the spores and nutrients to be carried on the natural fibers; the step of melt-kneading the natural fibers carried with the spores and nutrients together with the main resin to defibrate the natural fibers from the ends in the fiber length direction to obtain a composite resin material with an enlarged specific surface area of ​​the defibrated portion at the end; and the step of molding the composite resin material to obtain a composite resin molded body.

[0029] Hereinafter, a composite resin molded body and a method for producing the same according to an embodiment will be described with reference to the drawings. In the following description, the same components are denoted by the same reference numerals, and the description thereof will be appropriately omitted.

[0030] (Implementation Method)

[0031] Figure 1 It is a schematic diagram showing a cross-sectional structure of a composite resin molded body 10 according to the embodiment. Figure 2 Schematic diagram showing a cross-sectional structure of natural fibers as a constituent material of the composite resin molded body 10 according to the embodiment.

[0032] The composite resin molded body 10 of the embodiment is formed by a melt-kneaded product of a main resin 1 and a natural fiber 2 carrying spores 3 and nutrients 4. In the composite resin molded body 10, Figure 1 As shown in the schematic diagram showing the cross-sectional structure of FIG. 1 , the natural fibers 2 carrying the spores 3 and the nutrients 4 are dispersed in the main component resin 1 of the composite resin molded body 10 .

[0033] In addition, at least one of the natural fibers 2 is exposed on the surface of the composite resin molded body 10 .

[0034] Furthermore, if Figure 3 As shown in the schematic diagram of the cross-sectional structure of the composite resin molded body 10 containing the natural fiber 2 having the defibration site according to the embodiment, by having the defibration site at the end of the natural fiber 2, the specific surface area of ​​the defibration site increases, and the contact points between the natural fibers 2 increase. As a result, water can be absorbed into the interior of the composite resin molded body 10 through the contact points between the natural fibers 2 in a humid environment.

[0035] According to the composite resin molded body 10, at least one natural fiber 2 is exposed on the surface of the composite resin molded body, and since the natural fibers 2 have contact points with each other, the composite resin molded body has high elastic modulus and high water absorption. In a humid environment, the water absorption of the natural fibers 2 causes the spores 3 to germinate, and the decomposition of the main resin 1 is promoted. Therefore, a composite resin molded body 10 can be realized which maintains high rigidity during use and has excellent biodegradability in a humid environment such as the ocean or soil after disposal.

[0036] Hereinafter, each material constituting the composite resin molded body will be described.

[0037] <Main resin>

[0038] In this embodiment, the main resin 1 is preferably a biodegradable plastic selected from polyhydroxy acid, polyhydroxyalkanoate, polyalkylene dicarboxylate, and modified starch. In addition, in order to ensure good formability, it is preferably a thermoplastic resin, and the above resins can be used alone or in combination of two or more. It should be noted that the main resin 1 is not limited to the above materials as long as it is biodegradable.

[0039] In the present embodiment, "biodegradable plastic" refers to "a resin that has the same function as existing petroleum-derived resins when used, and is ultimately decomposed into water and carbon dioxide by microorganisms in the soil and ocean in nature after use". Specifically, it includes polyhydroxyalkanoates such as polyhydroxybutyrate and polyhydroxyvalerate, polyhydroxy acids such as polylactic acid, polyglycolic acid, and polycaprolactone, polyester resins such as polyalkylene dicarboxylates such as polybutylene adipate terephthalate, polyethylene succinate, and polybutylene succinate, polyamides, modified starch, and the like. In addition to homopolymers of the monomers of the above-mentioned resins, biodegradable plastics may also include copolymers of the monomers of the above-mentioned resins such as poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and copolymers of the monomers of the above-mentioned resins with other copolymerizable monomers.

[0040] <Natural Fiber>

[0041] Next, the natural fiber 2 is described. The first main purpose of adding the natural fiber 2 (hereinafter, sometimes simply referred to as "fiber") contained in the composite resin molded body 10 of the present embodiment is that when the composite resin molded body 10 is discarded after use, it does not impose a load on the environment, and absorbs water in the soil or the ocean, so that the spores 3 come into contact with water and germinate. For this purpose, the natural fiber 2 preferably has high water absorption, and the moisture content of the natural fiber 2 is preferably 5% or more according to the method specified in JIS L0105:2020. Specifically, pulp, cellulose, cellulose nanofiber, wood cellulose, wood cellulose nanofiber, cotton, silk or hemp is preferred.

[0042] The second purpose of adding natural fiber 2 is to improve dimensional stability by improving mechanical properties and reducing linear expansion coefficient. For this purpose, natural fiber 2 preferably has a higher elastic modulus than main resin 1. Specifically, pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, cotton, silk, wool or hemp can be cited. In addition, among these, cellulose is particularly preferred from the viewpoint of availability, high elastic modulus and low linear expansion coefficient. It should be noted that natural fiber 2 is not limited to the above-mentioned materials as long as it can improve mechanical properties and has water absorption.

[0043] After the spores 3 and the nutrients 4 are carried on the natural fibers 2, when the composite resin molded body 10 is set to 100 mass%, the content of the natural fibers 2 carrying the spores 3 and the nutrients 4 in the composite resin molded body 10 is preferably 10 mass% or more and 99 mass% or less. When the content of the natural fibers 2 carrying the spores 3 and the nutrients 4 is less than 10 mass%, it is difficult for the natural fibers 2 to have contact points with each other inside the composite resin molded body 10, and the water absorption is not sufficient. On the other hand, when the content of the natural fibers 2 carrying the spores 3 and the nutrients 4 is greater than 99 mass%, the proportion of the main resin 1 becomes small, the effect of bonding the natural fibers 2 to each other disappears, and the moldability becomes poor.

[0044] The morphology of the natural fiber 2 in the composite resin molded body 10 is described. In order to improve the water absorbency of the composite resin molded body 10, it is preferred that a portion of the natural fiber 2 is exposed on the surface of the composite resin molded body 10. By exposing a portion of the natural fiber 2 on the surface of the composite resin molded body 10, the natural fiber 2 absorbs water from the exposed portion, and absorbs the water into the composite resin molded body 10 through the capillary phenomenon of the fibers constituting the natural fiber. The smaller the specific surface area of ​​the exposed portion of the natural fiber 2 on the surface of the composite resin molded body, the higher the water absorbency. This is because when the specific surface area of ​​the exposed portion of the natural fiber 2 exposed on the surface is large, the effect of fine concavo-convexity leads to improved water repellency. Furthermore, as Figure 3 As shown, by having the defibrated portion at the end of the natural fiber 2, the specific surface area of ​​the defibrated portion increases, and the contact points between the natural fibers 2 increase, thereby increasing the water absorption rate through the contact points of the natural fibers 2 in a humid environment.

[0045] The central portion of the natural fiber 2 having a small specific surface area and not defibrated is less entangled with the main resin 1 and is easily exposed on the surface of the composite resin molded body according to the molding conditions. On the contrary, the front end portion of the defibrated natural fiber 2 is more entangled with the main resin 1 and enters the interior together with the main resin 1. Thus, a composite resin molded body 10 can be obtained in which the central portion of the natural fiber 2, excluding the two end portions, is exposed on the surface.

[0046] The total length of the front end defibration sites at both ends of the natural fiber 2 is preferably 5% or more and 50% or less of the fiber length L of the entire natural fiber 2. When the defibration sites are less than 5% of the overall fiber length L, the elastic modulus cannot be improved due to the small specific surface area, and when the defibration sites are longer than 50% of the overall fiber length L, the defibration sites with a large aspect ratio are exposed on the surface of the composite resin molded body, and the water absorption becomes poor.

[0047] Next, the characteristics of natural fiber 2 are described. About the types of main agent resin 1 and natural fiber 2, as mentioned above, if natural fiber 2 is too soft relative to main agent resin 1, that is, the elastic modulus of natural fiber 2 is small, then the elastic modulus of composite resin molded body 10 as a whole becomes small, and the strength is reduced as a result. On the other hand, if natural fiber 2 is too hard relative to main agent resin 1, that is, the elastic modulus of natural fiber 2 is large, then the shock wave generated during impact cannot be propagated, and is absorbed at the interface between main agent resin 1 and natural fiber 2, so cracks and cracks are easily generated near the interface, and the impact resistance is reduced as a result. Therefore, the relationship between the elastic modulus of main agent resin 1 and the elastic modulus of natural fiber 2 is preferably: the elastic modulus of natural fiber 2 is higher than the elastic modulus of main agent resin 1, and the smaller their difference, the better. As the most suitable relationship, it can be calculated according to the simulation results, and the elastic modulus difference between main agent resin 1 and natural fiber 2 is preferably within 20GPa.

[0048] In addition, these natural fibers 2 are sometimes surface-treated for the purpose of improving their adhesion to the main resin 1 or improving their dispersibility in the composite resin molded body 10, but when the water absorption of the natural fibers 2 is impaired by the surface treatment, it is preferably not surface-treated in advance.

[0049] <Additives>

[0050] Additives may also be used as needed. For example, a compatibilizer may be added to improve the affinity between the main resin 1 and the natural fiber 2, or a water-soluble or hydrolyzable resin may be used to cover the spores 3 and nutrients 4 contained in the natural fiber 2 for the purpose of protecting them. Thus, during melt kneading in the manufacturing stage of the composite resin molded body, the spores and nutrients may be protected from heat damage from the molten main resin. It should be noted that commonly used additives may be used.

[0051] <Spores>

[0052] Next, the spores 3 are described. Spores refer to durable cells with a highly durable cell structure formed by bacteria when the growth environment deteriorates. Sometimes they are also called spores. The spores 3 of this embodiment are used for the purpose of accelerating the decomposition of the composite resin molded body 10 in a humid environment. For the spores 3 of this embodiment, specifically, spores of bacteria of the genus Bacillus, bacteria of the genus Paenibacillus, bacteria of the genus Brevibacillus, bacteria of the genus Clostridium, bacteria of the genus Sporosarcina (Japanese: スポルサルシナ), etc. can be cited. As spores for the decomposition of biodegradable plastics such as aliphatic polyesters and aliphatic aromatic polyesters, spores of bacteria of the genus Bacillus, bacteria of the genus Paenibacillus, bacteria of the genus Brevibacillus, etc. can be cited. The above-mentioned spores can be used alone or in combination of two or more. It should be noted that as long as the type of spore-forming species has decomposability against the main resin 1, it is not limited to the above-mentioned materials.

[0053] <Nutrients>

[0054] Next, the nutrient 4 is described. The nutrient 4 of the present embodiment is used for the purpose of promoting the germination of spores 3 in a humid environment. In order to promote the nutrient absorption of microorganisms, the nutrient 4 of the present embodiment is preferably a peptone or extract of a phosphorus source, a sulfur source, a mineral source, and a vitamin source. As peptones, casein peptone, animal peptone, fungal peptone, soy peptone, etc. can be mentioned. As extracts, meat extracts, yeast extracts, malt extracts, potato extracts, etc. can be mentioned. The above-mentioned nutrients can be used alone or in combination of two or more. It should be noted that as long as there is a component that promotes spore germination, it is not limited to the above-mentioned materials.

[0055] <Method for producing composite resin molded body>

[0056] Next, a method for producing the composite resin molded body 10 according to the embodiment will be described. Figure 4 1 is a flowchart illustrating a process for producing the composite resin molded body 10 according to the present embodiment.

[0057] (1) The spores 3 and nutrients 4 are supported on the surface of the natural fiber 2 in advance. Examples of methods for supporting the spores 3 and nutrients 4 include physical adsorption by dry mixing, impregnation of natural fibers with a dispersion solvent, crosslinking, and wrapping. The supporting method is not limited to the above methods as long as it can hold the spores 3 and nutrients 4 on the surface of the natural fiber 2.

[0058] (2) The main resin 1 and the natural fiber 2 carrying the spores 3 and the nutrient 4 are dry-mixed and then placed in a melt-kneading device for melt-kneading. A portion of the spores 3 and the nutrient 4 carried by the natural fiber 2 falls off the natural fiber 2 and is dispersed in the main resin 1. The shearing action of the device promotes the defibration of the agglomerated mass of the natural fiber 2, so that the natural fiber 2 can be finely dispersed in the main resin 1. At this time, by adjusting the shearing conditions, the ends of the natural fiber 2 can also be Figure 3 It should be noted that, for example, under the conditions of material temperature of 180°C and about 5 minutes as shown in Example 1 below, it is believed that spores and nutrients will not be damaged by heat from the molten main agent resin.

[0059] In the past, when fibers were compounded into resins, materials obtained by defibration of fibers in advance through pretreatments such as wet dispersion were used. However, when natural fibers were defibrated in the solvent used for wet dispersion, the fibers swelled due to the solvent. Therefore, in order to allow the natural fibers to fully absorb water and swell in the composite resin molded body, the solvent in the natural fibers needs to be dried before being mixed with the main resin. In addition, compared with defibration in molten main resin, the fibers are more easily defibrated by wet dispersion, so it is difficult to defibrate only the ends, resulting in a state where the natural fibers are defibrated as a whole. In addition, due to the incorporation of pretreatments, there are problems of increased processes and poor productivity.

[0060] In contrast, in the manufacturing process of the composite resin molded body 10 of the present embodiment, a pretreatment based on wet dispersion for the purpose of defibration of the natural fiber 2 is not performed, but a melt-kneading treatment (complete dry process) is performed together with the main resin 1. In this process, by not performing a wet dispersion treatment of the natural fiber 2, the swelling of the natural fiber 2 in the manufacturing process can be suppressed, and the water absorption rate of the natural fiber 2 in the composite resin molded body 10 can be increased. By drying the natural fiber 2 in advance or during kneading, the water absorption rate of the composite resin molded body 10 in a humid environment can be further increased. In addition, since the natural fiber 2 has a defibration site as described above, there are more contact points between the fibers inside the composite resin molded body 10, and the water absorption rate of the composite resin molded body 10 can be increased through the contact points between the fibers.

[0061] When utilizing the full dry process to make the natural fiber 2 of the present embodiment, preferably high shear stress is applied during mixing. As specific mixing method, single shaft mixer, double shaft mixer, roller mixer, Banbury mixer and their combination etc. can be enumerated. From the viewpoint that high shear is easily applied and mass production is also high, particularly preferably continuous double shaft mixer, continuous roller mixer. As long as the method that high shear stress can be applied, then the mixing method other than the above-mentioned can also be used.

[0062] (4) By subjecting the composite resin composition extruded from the melt-kneading device to injection molding, a composite resin molded body 10 as an injection molded product can be produced.

[0063] Hereinafter, each Example and each Comparative Example in the experiment performed by the inventors will be described.

[0064] (Example 1)

[0065] In Example 1, a cellulose composite poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) resin molded body was produced by the following production method.

[0066] As the starting material of natural fiber, conifer pulp (trade name: NBKP Celgar, manufactured by Mitsubishi Paper Co., Ltd.) was used. As PHBV decomposing spores, spores of Bacillus bacteria were used. As nutrients, casein peptone (manufactured by Nacalaitesque) was used. Conifer pulp, spores, and nutrients were dry-mixed so that the mass ratio was 97.8:1.1:1.1 to obtain a cellulose filler carrying spores and nutrients.

[0067] The cellulose filler loaded with spores and nutrients and PHBV (TianAn Biopolymer product name: Y1000P) as the main resin were weighed to a mass ratio of 90:10 and dry-mixed. Then, a twin-shaft kneader (KRC kneader manufactured by Kurimoto Iron Works) was used for melt kneading. The screw was of medium shear type. The conditions for melt kneading were set at a material temperature of 180°C and a rotation speed of 50 min. -1 The composite resin composition discharged from the twin-screw kneading machine was thermally cut to produce cellulose composite PHBV resin pellets having a mass ratio of main resin to natural fiber to spore to nutrient of 10:88:1:1.

[0068] Then, a test piece of cellulose composite PHBV resin molded body was made by injection molding machine (180AD manufactured by Nippon Steel Works). The test piece production conditions were set as the temperature of the main resin 200°C, the metal mold temperature 50°C, the injection speed 100mm / s, and the holding pressure 100Pa. At this time, the total heating time of the above-mentioned melt kneading and injection molding was set within 5 minutes. The shape of the test piece was changed according to the evaluation items described below.

[0069] (Evaluation of water absorption of fibers)

[0070] The water absorption of the fiber is evaluated by measuring the moisture content of the fiber according to the method specified in JIS L0 105:2020. Specifically, the weight of the fiber dried at 80°C for 24 hours is measured and used as the base weight. Then, the weight of the fiber maintained at a temperature of 20°C and a humidity of 65% for 24 hours is measured. The increase in weight from the base weight is taken as the moisture content, and the moisture content is calculated. A moisture content of less than 5% is recorded as B, and a moisture content of more than 5% is recorded as A. For the composite resin molded body of Example 1, the moisture content of coniferous pulp is 6.5%, which is evaluated as A.

[0071] (Fiber end defibrillation)

[0072] The obtained cellulose composite PHBV resin molded body was immersed in chloroform to dissolve PHBV, and the remaining cellulose fibers were observed for their fiber shapes using SEM. In the composite resin molded body of Example 1, the fiber ends were in a defibrated state.

[0073] (Evaluation of Elastic Modulus of Composite Resin Molded Article)

[0074] The obtained dumbbell-shaped test piece of JIS K7139 type A12 size was used to perform a three-point bending test. As a method for evaluating the elastic modulus, a value less than 200 MPa was recorded as B, and a value greater than 200 MPa was recorded as A. In the composite resin molded body of Example 1, the elastic modulus of the test piece was 683 MPa, and the evaluation was A.

[0075] (Evaluation of Biodegradability of Composite Resin Molded Articles)

[0076] A biodegradation test was conducted using a rod-shaped test piece made from the obtained cellulose composite resin molded body. 50 g of a composting inoculum source (YK-11 manufactured by Yawata Bussan) was placed in a plastic container, and a rod-shaped test piece with a height of 20 mm, a width of 10 mm, and a thickness of 3 mm, which had been weighed in advance, was buried in the inoculum source. The weight reduction after being kept at a temperature of 58°C and a humidity of 50% for 2 months was evaluated. As a method for evaluating the biodegradability, a weight reduction value of 50% or more was recorded as AA, a weight reduction value of 40% or more and less than 50% was recorded as A, and a weight reduction value of less than 40% was recorded as B. In the composite resin molded body of Example 1, the biodegradability of the test piece was 42%, and it was evaluated as A.

[0077] (Example 2)

[0078] In Example 2, the mass ratio of the main resin to the natural fiber to the spores to the nutrients was changed to 60:38:1:1, and the other material conditions and process conditions were the same as those in Example 1 to produce a cellulose composite PHBV resin molded body.

[0079] (Comparative Example 1)

[0080] In Comparative Example 1, no natural fiber was used and the mass ratio of the main resin to spores to nutrients was changed to 98:1:1. The material conditions and process conditions other than these were the same as those in Example 1 to produce a PHBV resin molded body. The same evaluation as in Example 1 was also performed.

[0081] (Comparative Example 2)

[0082] In Comparative Example 2, PET fibers with a fiber diameter of 20 μm and a fiber length of 100 μm were used instead of conifer pulp to produce PET fibers carrying spores and nutrients. The material conditions and process conditions other than these were the same as those in Example 1 to produce a PET fiber composite PHBV resin molded body. The same evaluation as in Example 1 was also performed.

[0083] (Comparative Example 3)

[0084] In Comparative Example 3, a cellulose composite PHBV resin molded body was prepared in the same manner as in Example 1 except that no nutrients were used and the mass ratio of the main resin to the natural fiber to the spores was changed to 11:88:1. The other material conditions and process conditions were the same as in Example 1. The same evaluation as in Example 1 was also performed.

[0085] The compositions and measurement results of the composite resin molded bodies in Examples 1 and 2 and Comparative Examples 1 to 3 are as follows: Figure 5 shown.

[0086] like Figure 5As explained, in Examples 1 and 2, where natural fibers supported spores and nutrients, the elastic modulus was as high as 200 MPa or more, and Example 1, where the proportion of natural fibers was large, showed a higher elastic modulus than Example 2. Biodegradation was promoted compared to Comparative Example 1.

[0087] As described above, it was confirmed that a composite resin having a high elastic modulus and high biodegradability can be obtained when natural fibers supporting spores and nutrients are composited, the fibers are exposed on the surface of a composite resin molded body, and the water absorption rate of the natural fibers is high.

[0088] Comparative Example 1 produced without using natural fibers had a low elastic modulus and was evaluated as B. Since water was not absorbed into the composite resin molded body by the natural fibers, germination of spores was not promoted, and the biodegradation rate was low compared to the examples and was evaluated as B.

[0089] Comparative Example 2, which was prepared using PET fibers instead of softwood pulp, did not promote spore germination in the biodegradability evaluation because the PET fibers had a low moisture content and no water absorption. The biodegradation rate was lower than that of Example 1 and was evaluated as B.

[0090] Comparative Example 3 prepared without using nutrients did not promote germination of spores, and the biodegradation rate was lower than that of Example 1, and was evaluated as B.

[0091] Based on the above evaluation, it was confirmed that as long as water-absorbent natural fibers and biodegradable plastics are used, spores and nutrients are carried on the surface of the natural fibers, and the fibers are exposed on the surface of the composite resin molded body, a composite resin molded body with high elastic modulus and high biodegradability can be obtained.

[0092] It should be noted that the present disclosure includes solutions obtained by appropriately combining any of the various embodiments and / or examples described above, which can achieve the effects of each embodiment and / or example.

[0093] According to the composite resin molded article of one embodiment of the present disclosure, it is possible to realize a composite resin molded article having not only a high elastic modulus but also an accelerated biodegradation rate in a high-humidity environment, compared with a resin alone.

[0094] Industrial Applicability

[0095] According to a composite resin molded body of one embodiment of the present disclosure, a composite resin molded body can be provided that can control the mechanical strength and biodegradation rate compared to conventional biodegradable plastics. According to one embodiment of the present disclosure, since the properties of the main resin can be improved, it can be used as a substitute for general-purpose plastics derived from petroleum. As a result, the environmental load of various industrial products or daily necessities made of general-purpose plastics derived from petroleum can be greatly reduced. Furthermore, it can be used for packaging materials, daily necessities, home appliance housings, building materials, etc.

[0096] Description of Reference Numerals

[0097] 1 Main resin

[0098] 2 Natural Fibers

[0099] 3 Spores

[0100] 4 Nutrients

[0101] 10 Composite resin molded body

Claims

1. A composite resin molded body comprising a main resin and a plurality of natural fibers dispersed in the main resin, At least a portion of the plurality of natural fibers carries spores and nutrients, When the composite resin molded body is taken as 100 mass %, the content rate of the plurality of natural fibers is 10 mass % or more and 99 mass % or less, A part of the plurality of natural fibers is exposed on the surface of the composite resin molded body.

2. The composite resin molded article according to claim 1, wherein At least a part of the plurality of natural fibers has a moisture content of 5% or more according to the method specified in JIS L0105:2020.

3. The composite resin molded body according to claim 1 or 2, wherein The main resin is a biodegradable resin selected from polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylates, and modified starches.

4. The composite resin molded article according to any one of claims 1 to 3, wherein The nutrients include any of peptones or extracts.

5. The composite resin molded article according to any one of claims 1 to 4, wherein At least a portion of the plurality of natural fibers carries the spores on the surface of the fibers.

6. The composite resin molded article according to any one of claims 1 to 5, wherein At least a portion of the plurality of natural fibers are cellulosic.

7. The composite resin molded article according to any one of claims 1 to 6, wherein At least a portion of the plurality of natural fibers has a defibrated portion at an end portion in the fiber length direction.

8. A method for producing a composite resin molded body, comprising: Steps for preparing spores, nutrients, natural fibers, and main agent resin; A step of allowing the spores and the nutrients to be carried on the natural fibers; The step of melt-kneading the natural fibers carrying the spores and the nutrients together with the main resin to defibrinate the natural fibers from the ends in the fiber length direction to obtain a composite resin material having an increased specific surface area of ​​the defibrinated portion at the ends; The step of molding the composite resin material to obtain a composite resin molded body.