Method for antimicrobial protection of leather during tanning comprising biocidal composition and luminescent additive allowing identification thereof
By using biocidal compositions and luminescent additives during the tanning process, the problem of microbial protection of leather and detection of biocidal compositions is solved, long-term antimicrobial effects and original identification are achieved, and the performance and use of leather are significantly improved. life.
Patent Information
- Application Number
- CN202380023565.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-23
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-08
AI Technical Summary
Existing technology makes it difficult to effectively protect tanned leather from microbial pathogens, and it is difficult to quickly and cheaply determine whether a biocidal composition has been applied to the leather. Traditional detection methods are complex and expensive.
A biocidal composition is used in the tanning process, the biocidal composition includes silver phosphate glass, silicone, aliphatic hydrocarbons and water, the luminescent additive is an aluminosilicate glass formed from rare earth ions, which is recognized by the luminescent effect and Verify the presence of the biocidal composition.
Long-term antimicrobial protection of leather is achieved, the detection of biocidal compositions is simplified, the originality of the product is visually recognized through luminescence characteristics, and the service life and performance of the leather are significantly increased.
Abstract
Description
Technical Field
[0001] The present invention discloses an antimicrobial protection method applied to leather during the tanning process combining a biocidal composition and an additive that allows the presence of the biocidal composition to be identified through a luminescent effect, so that it guarantees that the leather has been previously treated with said biocidal composition product, giving comfort to the user and ensuring the presence of the product, as well as proving its originality using luminescent encryption technology. Background Art
[0002] If the skin of some animals were not reused by the tannery, it would be a waste product, since it would enter a state of decomposition and become another waste product to be eliminated. Through the tanning process, the skin decomposition is stopped. The animal's skin acquires resistance, elasticity and softness, properties that are beneficial to its subsequent preparation. Leather thus becomes an extremely soft material, which can be used for different applications: from suitcases to shoes, from belts to jewelry, but also leather sofas and armchairs, mobile phones and flat cases, clothes and outerwear, among other items. Thanks to some modifications during the production process, it is possible to obtain certain characteristics better suited to certain uses: the end result will be a leather that is more or less soft and malleable, or of a specific color shade.
[0003] In the leather tanning process, basically two methods are used: one based on chromium salts and the other based on vegetable agents. 80% of the industry dedicated to tanning leather uses the method based on chromium salts.
[0004] Tannins are able to bind to proteins in a stable way: once the tanning process is complete, the tannins remain permanently attached to the fibers of the leather. This is a very important detail, since it is this tannin that gives these leathers their absorbent and breathable properties.
[0005] During the tanning process, animal collagen, which represents the main component of the skin, is modified so that the leather resulting from the tanning exhibits resistance to heat and microorganisms, together with the fact that after drying it retains the flexibility of tanned leather. There are essentially three tanning methods used today, each based on a different cross-linking strategy:
[0006] Mineral tanning is carried out with metal salts (eg chromium salts, titanium, iron, aluminum, zirconium). Stabilization thus results in a state in which the metal ions are bound in the form of a complex or by means of ionic interactions of the amino acid chains to the main chain of the collagen peptides.
[0007] Vegetable tanning is carried out with plant extracts such as mimosa, quebracho, chestnut and tara. Stabilization is mainly based on hydrogen bonding between the tanning phenols and the peptide bonds in the collagen backbone.
[0008] Synthetic tanning with reactive organic compounds (especially with aldehydes such as, for example, glutaraldehyde, isocyanates). Stabilization occurs primarily by covalent binding to the lysine residues of collagen.
[0009] The chrome tanning method, with a global proportion of over 90%, is the most widely used worldwide. The hydrated chromium complex arranged between the carboxyl groups of the glutamic and aspartic acids of the collagen peptide backbone produces a resistant and soft leather. In addition to the good quality of the leather to be obtained, a fast and economical process management has been established by chrome tanning.
[0010] The tanning method based on chromium salts is the most commonly used, but the most polluting due to the toxic effects of Cr. This method allows the use of mineral tanning agents to stabilize the collagen of the skin, thereby transforming the skin into leather. In mineral tanning, different types of chromium salts are used in very different proportions. Before entering the tanning process, the skin is drained in order to eliminate as much moisture content as possible. In order to carry out this process, the skin is introduced into a machine called a splitter. The action of trivalent chromium in an acidic medium (hydrochloric acid) allows the skin to become leather (stabilized material), preventing it from degrading. The duration of the tanning process is 8 to 24 hours. The chromium that is not absorbed by the leather is reused. Once the leathers are dry, they are subjected to different softening processes, thereby producing a product combined with a mechanical process, rendering these leathers more durable and resistant.
[0011] Conventionally, when raw hides are tanned to produce leather, a biocidal composition is added to the tanning drum to prevent the leather from deteriorating during storage and transportation, which is done by a batch process, however, this method does not ensure that the treated skin can remain protected for much longer than is associated with transportation, on the other hand, in order to prove that the biocide (such as a fungicide) has been applied to the leather piece, the leather piece must be removed from the drum and analyzed with reagents. This is a laborious and specialized test that only a few tanning plants perform. Once the leather is stored, determining whether the biocidal composition has been applied is only available by extraction and high performance liquid chromatography (HPLC) analysis, which requires complex equipment, is expensive and time consuming.
[0012] However, in any leather tanning process, there is no relevant method that allows to protect the leather produced by the tanning from microbial pathogens, which are present on the surface for an indefinite period of time. Therefore, there is a need for relevant steps in the tanning process to protect the leather and prevent the spread of diseases caused by microbial pathogens beyond the storage period of the leather. In addition, there is a need for a method that makes it easier, faster and cheaper to determine whether a biocidal composition has been applied to a leather piece, and optionally, such leather remains protected for a long time.
[0013] Prior art U.S. patent application US20190249360 discloses a method and system for marking leather or tanned leather treated with a biocide and its identification, wherein the method is performed by applying a biocide and one or more detectable tags to the leather or tanned leather. The detectable tag can be detected to indicate one or more data fragments, such as whether the biocide has been applied to the leather or tanned leather and / or other data. Information or other data about the biocide and the tannery where the biocide is applied can be distinguished from the detection of the detectable tag or one or more of the detectable tags (if they are used). A system for marking leather or tanned leather and applying a biocide, as well as a method and system for detecting the mark are also provided. The method includes: applying a biocide to leather or leather goods; and applying one or more detectable tags to the leather or leather goods, wherein the one or more detectable tags convey: a) whether the biocide has been applied, and / or b) the tanning process to which the biocide was applied, and / or c) what type of biocide was applied, and / or d) the supplier of the biocide, and / or e) the time when the biocide was applied, and / or f) whether sufficient biocide (concentration) has been applied, and / or g) whether the biocide has been evenly applied to the leather or leather or any combination thereof. Summary of the invention
[0014] The invention discloses a method for the antimicrobial protection of leather during the tanning process, in which the transformation of skin into leather is used, the method being validated in the presence of Cr(III) and / or Ti(IV) salts, so that by adding a controlled amount of a biocidal composition, the leather is equipped with antimicrobial (antibacterial and antiviral) characteristics that extend the useful life of the material and improve the performance of the articles made therewith. In addition, the biocidal composition incorporates a luminescent additive during the tanning process that allows to prove that the piece has been treated with the original biocidal product and that it is free of microorganisms, pathogens, viruses, etc. DETAILED DESCRIPTION
[0015] The present invention discloses a method for antimicrobial protection of leather during tanning, the method comprising a biocidal composition and a luminescent additive which allows identification and authentication of the biocidal composition.
[0016] The tanning step in the leather processing is based on the reaction of leather collagen with metal cations. When the cation used is Cr(III), the tanning method is called "wet blue". When Ti(IV) is used, the tanning process is called "wet white".
[0017] Most of the chromium or titanium in the leather is strongly bound to collagen during the tanning process. This phenomenon is the reason for the selection of both elements in this process. Once the chromium or titanium is fixed to the fibers, the availability of its balance Cr(III) and Cr(VI) in the case of chromium decreases drastically. Only the extractable part of the Cr(III) in the leather is fully available for the balance. Only at temperatures equal to or greater than 800°C, oxidation reactions start to shift towards Cr(VI). This does not represent any type of risk in normal hiding conditions.
[0018] The high thermal stability of chrome-tanned leathers is justified by the acceptance that bonds containing chromium atoms are formed between adjacent protein chains. This greater cross-linking of the protein chains increases their stability to heat (e.g. with respect to their swelling or even with respect to possible hydrolysis). Today, it is accepted that chromium aggregates form bonds between protein chains as the main mechanism of chrome tanning. Nevertheless, a portion of the fixed chromium is bound to other chromium atoms by esterification or oxalation, or by hydrogen bonding to other collagen reactive groups. It seems likely that less than half of the available carboxyl groups have reacted with chromium salts during normal tanning.
[0019] The method comprises: solid chromium salt is introduced into a rotary drum, wherein the acid-washed skin is positioned and they are rolled for a specific time so that they dissolve, and then the alkalizing product is added once or in multiple doses in a solid state. Although the newly dissolved chromium salt is masked with sulfate and is less sensitive to alkali, there are molecules that are strongly alkalized. The important characteristic of alkaline chromium salts is that they are easy to combine because the OH-groups attached to the chromium tend to form bonds between the chromium atom and the skin collagen. In the case of very high alkalinity (occurring when the external OH-group is attached to the chromium atom), for each chromium atom present, two, at most three bonds are formed between the OH-groups of the macromolecule. The larger the number of OH-groups that work by forming these bonds between two chromium atoms, the greater the stability that the chromium salt used will have and the greater the tolerance to acid.
[0020] The biocidal composition of the present invention is added immediately after the addition of chromium or titanium salts during the tanning process and is combined with a source of silver ions, which is preferably formed of a silver phosphate glass of partially soluble material, capable of acting as a unique system for supplying silver ions in a controlled manner. This allows the antimicrobial capacity to act during the tanning process. The silver ions from the silver phosphate glass can coordinate with the OH-groups attached to the chromium, which tend to form bonds between the chromium atoms and the skin collagen, so that in combination they show a synergistic effect with effectiveness against all Gram-positive and Gram-negative bacteria. This fact, in addition to improving the bactericidal capacity of the leather treated in this method, also allows greater stability of the bond between the skin collagen and the chromium salt. When combined with the chromium salt bound to the skin collagen, the mechanism of action of silver acts in unison to reduce the risk of infection through a silver concentration-dependent effect, effectively resisting growing cells and dormant cells through multiple targets in the cell structure, and a time-dependent effect of silver, effectively resisting growing cells through a single target on the cell.
[0021] The biocidal composition, due to its action in the tanning process, comprises: between 3% and 5% of silver phosphate glass; silicone in an amount between 1% and 3.5%; aliphatic hydrocarbons between 0.1% and 0.30%; and water between 90% and 95%. The biocidal composition is added during the tanning process in an amount between 0.1% and 5% by weight of the material to be tanned. The biocidal composition provides a sufficient amount of silver ions to maintain the bactericidal effect of the Ag(+) ions throughout the useful life of the material.
[0022] The amount of composition used will vary according to the type of process. It is estimated that between 0.5% and 1.0% (always referring to the weight of the leather to be treated in each process) is sufficient for the composition to achieve its antimicrobial function.
[0023] During the tanning process, a luminescent additive is incorporated to indicate that the skin has been previously treated with a biocidal composition. A luminescent additive formed by a metal oxide (aluminosilicate glass containing rare earth ions, by means of a dopant) is incorporated into the biocidal composition, which allows the detection and identification of the coating of said composition by infrared light inducing an easily detectable luminescence (green light). This luminescent additive presents a codable emission light pattern that allows the compound to be unavoidably identified, thus proving its authenticity, which distinguishes it with respect to other similar products on the market.
[0024] The luminescent additive acting as a marker allowing the identification of the biocidal composition comprises between 20% and 40% of silicon dioxide and between 10% and 30% of aluminum oxide and between 30% and 50% by weight of calcium fluoride. Materials doped with luminescent "rare earth" ions are added to this mixture, such as between 0.5% and 3% of erbium (III) fluoride; between 5% and 15% of ytterbium (III) fluoride; a maximum of 5% of thulium (III) fluoride; and a maximum of 5% of europium (III) fluoride. All these percentages are with respect to the total weight of the luminescent additive.
[0025] Silicon dioxide is used as luminescent coatings, i.e. they do not involve heat generation, and are particularly useful in the main physical phenomena that allow the generation of light with characteristics such as phosphorescence and fluorescence. In addition, it is used as an insulating coating, forming a thin layer similar to a laminate on the coated surface, protecting and preserving the surface from the action of water, from scratches or other wear damage. Aluminum oxide is used as a selective adsorbent, allowing the level of fluoride in the mixture to be adjusted downward.
[0026] Calcium fluoride significantly increases its fluorescence, with a broad emission that occurs within an acceptable target range. The optically active compound of the additive is formed by a luminescent "rare earth" ion. Ytterbium fluoride increases the absorption of infrared light and the subsequent conversion to visible light by the remaining luminescent elements in the marker composition (erbium fluoride, thulium fluoride and europium fluoride). Erbium-doped silica glass fibers are active elements that amplify the luminescence effect, and in addition, their homogenization is increased due to the presence of aluminum oxide. Ytterbium fluoride also increases the amplification of the material as a luminescent marker, and thulium (III) fluoride is used to improve the up-conversion fluorescence from infrared to ultraviolet and visible in fluoride glass. Europium fluorescence is used to improve the emission color coding effect of the marking additive.
[0027] During the tanning process, the luminescent additive used as an identification marker for the biocidal composition is applied at between 0.1% and 5% by weight of the material treated.
[0028] This luminescent additive (visible only under IR excitation) is formulated to be integrated into the formulation of the material being treated and acts as a marker when illuminated by IR light in the 900 to 990 nanometer range.
[0029] Different tests have established that the luminescent additive of the product presents emission only under invisible infrared light with high intensity brightness, due to the lack of background noise due to zero autofluorescence of the fabric matrix or the surface to which it has been applied. Furthermore, the luminescence intensity ratio between the different visible emission bands (blue, green and red) observed after the conversion of the invisible infrared reading light can be adjusted as desired (by varying the concentration level and type of dopant "rare earth" ions). In other words, by designing and synthesizing on demand at the source, the emitted light is encoded with an irrefutable code, providing a novel and disruptive proof of concept for optical cryptographic security mode.
[0030] The tests applied to obtain results during the tanning process are:
[0031] ASTM E2149-20: Standard Test Method for Determining the Activity of Immobilized Antimicrobials under Dynamic Contact Conditions.
[0032] - UNE-EN ISO 18184 - Test methods for determining the antiviral activity of products against specific viruses.
[0033] A bactericidal surface protection of between 12 and 18 months has been determined, so it allows to maintain long-term protection of hard non-porous surfaces with a single application. The product is effective for the bactericidal protection of leather during the conversion of skin into leather, against different microorganisms such as Escherichia coli, Staphylococcus aureus, Enterococcus hilarii, Pseudomonas aeruginosa, Candida albicans, and certain types of viruses with and without an outer shell.
[0034] As an added value, the luminescence feature of the present invention clearly distinguishes the present invention with respect to the prior art, as it allows the user to visualize where the product is applied and to identify the coded light pattern to indicate that the product is original. A simple and compact portable handheld device (pocket spectrometer / App for smartphone camera) will allow the end user to detect the coded luminescence pattern by illuminating it with a low-cost commercial infrared laser pointer, thus verifying that the applied product is protected with the original biocidal composition. This luminescence technology using infrared light and color coding using "rare earth" ions is at the forefront of anti-counterfeiting light technology, in the line of technology for secure encryption of certification documents (passports, security inks) and for legal tender banknotes. Therefore, its application in the original identification of biocidal composition products undoubtedly constitutes an absolute novelty, which defines a clear and significant difference from other products with similar characteristics on the market.
Claims
1. A method for the antimicrobial protection of leather during tanning, comprising a biocidal composition and a luminescent additive allowing its identification, characterized in that The biocidal composition is added during the tanning process immediately after the addition of chromium or titanium salts, in an amount of between 0.1% and 5% by weight of the material to be tanned, and comprises: between 3% and 5% of silver phosphate glass; between 1% and 3.5% of silicone; between 0.1% and 0.30% of aliphatic hydrocarbons; and between 90% and 95% of water, and the luminescent additive is added in an amount of between 0.1% and 5% by weight of the material to be tanned, the luminescent additive comprising between 20% and 40% of silicon dioxide relative to the total weight of the luminescent additive; between 10% and 30% of aluminum oxide; between 30% and 50% of calcium fluoride; between 0.5% and 3% of erbium (III) fluoride; between 5% and 15% of ytterbium (III) fluoride; a maximum of 5% of thulium (III) fluoride; and a maximum of 5% of europium (III) fluoride.
2. Method for the antimicrobial protection of leather during tanning according to claim 1, comprising a biocidal composition and a luminescent additive allowing its identification and verification, characterized in that The luminescent additive acts as a marker when illuminated by IR light in the range of 900 to 990 nanometers.
Citation Information
Patent Citations
Method And System For Tagging Leather Or Hides Treated With Biocide And Identifying Same