All-solid-state battery
By using spinel structure compounds and γ-Li3PO4 type crystal structure solid electrolytes in all-solid-state batteries, combined with Ag or Ag alloys, and designing the laminated structure of the sintered body, the problem of high internal resistance in all-solid-state batteries is solved, which is significant. Improved battery performance and efficiency.
Patent Information
- Application Number
- CN202280092564.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-08
AI Technical Summary
Existing all-solid-state batteries have the problem of high internal resistance.
A compound with a spinel structure is used as the cathode material, and a solid electrolyte with a γ-Li3PO4 crystal structure is used in the solid electrolyte layer, combined with Ag or Ag alloy, and the internal resistance is reduced through the stacked structure design of the sintered body.
The internal resistance of the all-solid-state battery is reduced and the performance and efficiency of the battery are improved.
Smart Images

Figure CN118749147A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid-state battery. This application claims priority based on Japanese Patent Application No. 2022-029457 filed on February 28, 2022, and the contents thereof are cited herein. Background Art
[0002] In recent years, electronic technology has developed significantly, achieving small, light, thin, and multifunctional portable electronic devices. Along with this, there is a strong desire to make batteries that serve as power sources for electronic devices smaller, lighter, thinner, and more reliable, and all-solid batteries using solid electrolytes as electrolytes have attracted much attention.
[0003] All-solid batteries are available in thin film and bulk types. Thin film types are made using thin film technologies such as physical vapor deposition (PVD) and sol-gel methods. Bulk types are made using powder forming methods, sintering methods, and the like. Different all-solid batteries can be used with different materials or have different performances due to different manufacturing methods. For example, bulk types that use sintered bodies require materials that can withstand sintering. On the other hand, since each layer can be thickened, it has a high capacity.
[0004] For example, a sintered all-solid battery using an oxide-based solid electrolyte as a solid electrolyte is disclosed in Patent Document 1. In the all-solid battery described in Patent Document 1, several materials that can be applied to the positive electrode active material layer and the solid electrolyte layer are presented.
[0005] Prior art literature
[0006] Patent Literature
[0007] [Patent Document 1] International Publication No. 2007 / 135790 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] Among the all-solid batteries described in Patent Document 1, some have high internal resistance.
[0010] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an all-solid-state battery having low internal resistance.
[0011] Means for solving technical problems
[0012] In order to solve the above technical problems, the following means are provided.
[0013] (1) A first embodiment of a fully solid-state battery comprises a sintered body. The sintered body comprises: a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode. The positive electrode comprises a compound having a spinel structure. The solid electrolyte layer comprises a solid electrolyte having a γ-Li3PO4 type crystal structure. The compound having a spinel structure is composed of Li α M β Mn 2-β O4...(1) In the formula (1), M is one or more atoms selected from transition metals, and satisfies 0.8≤α≤1.2 and 0.1≤β≤0.9.
[0014] (2) In the all-solid-state battery of the above embodiment, M may be Ni. α Ni β Mn 2-β O4……(2) indicates that 0.4≤β≤0.6 is satisfied.
[0015] (3) In the all-solid-state battery of the above aspect, the positive electrode may further contain Ag or an Ag alloy.
[0016] (4) In the all-solid-state battery of the above aspect, the positive electrode may include a first layer and a second layer, wherein the first layer includes the compound and Ag or an Ag alloy, and the second layer is in contact with at least one main surface of the first layer.
[0017] (5) In the all-solid-state battery of the above aspect, the volume ratio of Ag and the Ag alloy in the first layer may be 40% or more and 85% or less.
[0018] (6) In the all-solid-state battery of the above embodiment, the solid electrolyte contained in the solid electrolyte layer may contain Li 3+x Si x P 1-x O4(0.2≤x≤0.6).
[0019] Effects of the Invention
[0020] The all-solid-state battery of the above embodiment has low internal resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a cross-sectional view of the all-solid-state battery according to the first embodiment.
[0022] Figure 2 This is an enlarged cross-sectional view of a characteristic portion of the all-solid-state battery of the first embodiment.
[0023] Figure 3 This is an enlarged cross-sectional view of a characteristic portion of another example of the all-solid-state battery of the first embodiment.
[0024] Figure 4 This is an enlarged cross-sectional view of a characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment.
[0025] Figure 5 This is an enlarged cross-sectional view of a characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment.
[0026] Figure 6 This is an enlarged cross-sectional view of a characteristic portion of another example of the all-solid-state battery of the first embodiment.
[0027] Explanation of symbols
[0028] 1……positive electrode;
[0029] 1A, 1C, 1D, 1E...positive electrode current collector layer;
[0030] 1B……positive electrode active material layer;
[0031] 1F…Middle floor;
[0032] 2. 2D…negative electrode;
[0033] 2A, 2C...negative electrode current collector layer;
[0034] 2B……Negative electrode active material layer;
[0035] 3...Solid electrolyte layer;
[0036] 4...Laminated body;
[0037] 5, 6……terminal electrodes;
[0038] 10……All-solid-state batteries;
[0039] 11……positive electrode current collector;
[0040] 12……positive electrode active material;
[0041] 13... oxides;
[0042] 21……negative electrode current collector;
[0043] 22……Negative electrode active material;
[0044] 23……Solid electrolyte. DETAILED DESCRIPTION
[0045] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings as appropriate. In the accompanying drawings used in the following description, in order to facilitate the understanding of the features of the present invention, the features are sometimes enlarged for convenience, and the dimensional ratios of the various components are sometimes different from the actual ones. The materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited thereto, and can be implemented by appropriately changing within the scope of not changing its purpose.
[0046] Define the direction. The stacking direction of the stacked body 4 is set to the z direction, a direction in the plane perpendicular to the z direction is set to the x direction, and a direction perpendicular to the x direction and the z direction is set to the y direction. Hereinafter, a direction in the z direction is sometimes expressed as "up", and the direction opposite to the direction is expressed as "down". Up and down are not necessarily consistent with the direction in which gravity is applied.
[0047] Figure 1 1 is a schematic cross-sectional view of the all-solid battery 10 of the present embodiment. The all-solid battery 10 has a stack 4 and terminal electrodes 5, 6. The terminal electrodes 5, 6 are in contact with the opposite surfaces of the stack 4, respectively. The terminal electrodes 5, 6 extend in the z direction intersecting (orthogonal) with the stacking surface of the stack 4.
[0048] The laminate 4 has a positive electrode 1, a negative electrode 2 and a solid electrolyte layer 3. The laminate 4 is a sintered body formed by stacking the positive electrode 1, the negative electrode 2 and the solid electrolyte layer 3 and sintering them. There is no limit to the number of layers of the positive electrode 1 and the negative electrode 2. The solid electrolyte layer 3 is at least located between the positive electrode 1 and the negative electrode 2. Between the positive electrode 1 and the terminal electrode 6 and between the negative electrode 2 and the terminal electrode 5, for example, there is a solid electrolyte that is the same as the solid electrolyte layer 3. One end of the positive electrode 1 is connected to the terminal electrode 5. One end of the negative electrode 2 is connected to the terminal electrode 6.
[0049] The all-solid-state battery 10 is charged or discharged by transfer of ions between the positive electrode 1 and the negative electrode 2 via the solid electrolyte layer 3 . Figure 1 The all-solid battery 10 shown is a stacked battery, but the all-solid battery 10 may also be a wound battery. The all-solid battery 10 is used, for example, for laminated batteries, square batteries, cylindrical batteries, coin batteries, button batteries, etc. In addition, the all-solid battery 10 may also be a liquid injection type in which the solid electrolyte layer 3 is dissolved or dispersed in a solvent.
[0050] "positive electrode"
[0051] Figure 2It is an enlarged view of the characteristic part of the all-solid-state battery 10 of the first embodiment. The positive electrode 1 has, for example, a positive electrode collector layer 1A and a positive electrode active material layer 1B. The positive electrode collector layer 1A is an example of the first layer, and the positive electrode active material layer 1B is an example of the second layer. The second layer is in contact with at least one main surface of the first layer. The positive electrode 1 contains a compound having a spinel structure that satisfies the formula (1) described later. The positive electrode 1 may further contain Ag or an Ag alloy.
[0052] [Positive electrode current collector layer]
[0053] The positive electrode collector layer 1A includes, for example, a positive electrode collector 11 and a positive electrode active material 12. In this case, the area between the xy plane passing through the uppermost portion of the positive electrode collector 11 and the xy plane passing through the lowermost portion is considered to be the positive electrode collector layer 1A.
[0054] The positive electrode collector 11 is composed of a plurality of collector particles. The plurality of collector particles are interconnected and electrically connected in the xy plane. The positive electrode collector layer 1A, for example, comprises a metal or alloy containing one or more selected from Ag, Pd, Au, and Pt. These metals or alloys will not melt even if the stack 4 is heated in an atmospheric atmosphere and are difficult to oxidize. The positive electrode collector layer 1A preferably contains Ag or an Ag alloy. The positive electrode collector 11 is, for example, an AgPd alloy, Au, Pt, and a mixture thereof. There is no restriction on the composition ratio of each component of the alloy.
[0055] The total volume ratio (Va) of Ag and Ag alloy in the positive electrode collector layer 1A is, for example, greater than 40% and less than 85%. The volume ratio is roughly consistent with the area ratio in the cross section measured by a scanning electron microscope, for example. Therefore, the area ratio in the cross section measured by a scanning electron microscope can be directly regarded as the volume ratio. Ag and Ag alloy can be distinguished based on the contrast of the image obtained using a scanning electron microscope. In addition, in the case of extracting only the volume ratio of Ag from Ag and Ag alloy, the composition ratio is quantitatively analyzed by energy dispersive X-ray analysis (EDS), and the product of its ratio and the volume ratio of Ag and Ag alloy is obtained, thereby obtaining only the volume ratio of Ag.
[0056] The positive electrode active material 12 is mixed with the positive electrode current collector 11 and exists in the positive electrode current collector layer 1A. The positive electrode active material 12 is in contact with the positive electrode current collector 11. If the positive electrode current collector layer 1A contains the positive electrode active material 12, the transfer of lithium ions in the positive electrode current collector layer 1A becomes smooth. The positive electrode 1 contains a compound having a spinel structure as the positive electrode active material 12. The compound having a spinel structure is composed of Li α M β Mn 2-β O4……(1) indicates.
[0057] M in formula (1) is one or more atoms selected from transition metals. M in formula (1) is, for example, one or more atoms selected from Ni, Co, and Ti. M in formula (1) is, for example, Ni. When M in formula (1) is Ni, formula (1) is Li α Ni β Mn 2-β O4……(2) indicates.
[0058] α in the formula (1) and the formula (2) satisfies 0.8≤α≤1.2. β in the formula (1) and the formula (2) satisfies 0.1≤β≤0.9, and preferably satisfies 0.4≤β≤0.6.
[0059] The compound represented by formula (1) is, for example, LiNi 0.1 Mn 1.9 O4、LiNi 0.5 Mn 1.5 O4、LiNi 0.9 Mn 1.1 O4、LiCo 0.1 Mn 1.9 O4、LiCo 0.5 Mn 1.5 O4、LiCo 0.9 Mn 1.1 O4、LiTi 0.1 Mn 1.9 O4、LiTi 0.5 Mn 1.5 O4、LiTi 0.9 Mn 1.1 O4.
[0060] The positive electrode active material 12 may contain, in addition to the spinel structure compound represented by formula (1), a transition metal oxide containing at least one selected from Co, Ni, Mn, Fe, and V. For example, the positive electrode active material 12 may contain spinel structured LiNi 0.5 Mn 1.5 O4 and LiMn2O4.
[0061] exist Figure 2 In FIG. 1 , an example is shown in which the positive electrode current collector 11 is composed of a plurality of current collector particles, but the present invention is not limited to this case. Figure 3 This is an enlarged view of a characteristic portion of another example of the all-solid-state battery according to the first embodiment. Figure 3 The positive electrode current collector layer 1C shown is composed of a foil-shaped positive electrode current collector 11 extending in the xy plane. The positive electrode current collector 11 may be in the form of a stamped film or a rolled product extending in the xy plane. The positive electrode current collector layer 1C may be composed of the positive electrode current collector 11.
[0062] [Positive electrode active material layer]
[0063] The positive electrode active material layer 1B is formed on one or both sides of the positive electrode collector layer 1A. The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive additive, a binding material, and the above-mentioned solid electrolyte. When the positive electrode active material layer 1B contains a solid electrolyte, the outermost xy plane passing through the positive electrode active material is regarded as the boundary between the positive electrode active material layer 1B and the solid electrolyte layer 3.
[0064] (Positive electrode active material)
[0065] The positive electrode active material includes a spinel structure compound represented by formula (1). In addition to the spinel structure compound represented by formula (1), the positive electrode active material 12 may also include a transition metal oxide containing one or more selected from Co, Ni, Mn, Fe, and V. For example, the positive electrode active material 12 may include a spinel structure LiNi 0.5 Mn 1.5 O4 and LiMn2O4.
[0066] (Conductive additive)
[0067] The conductive aid is not particularly limited as long as it can improve the electron conductivity in the positive electrode active material layer 1B, and a known conductive aid can be used. The conductive aid is, for example, a carbon material such as graphite, carbon black, graphene, carbon nanotubes, a metal such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, iron, a conductive oxide such as ITO, or a mixture thereof. The conductive aid may be in the form of a powder or a fiber.
[0068] (Bonding material)
[0069] The binder bonds the positive electrode current collector layer 1A and the positive electrode active material layer 1B, the positive electrode active material layer 1B and the solid electrolyte layer 3 , and various materials constituting the positive electrode active material layer 1B.
[0070] The binding material can be used within the range that the function of the positive electrode active material layer 1B is not lost. The binding material may not be contained unless it is necessary. The content of the binding material in the positive electrode active material layer 1B is, for example, 0.5 volume % to 30 volume % of the positive electrode active material layer. If the content of the binding material is small enough, the resistance of the positive electrode active material layer 1B becomes low enough. Here, the volume % is roughly consistent with the area % in the cross section measured by a scanning electron microscope, for example. Therefore, the area ratio in the cross section measured by a scanning electron microscope can be directly regarded as the volume ratio.
[0071] As long as the bonding material can be joined as described above, for example, fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) can be cited. Furthermore, in addition to the above, as bonding materials, for example, cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, etc. can also be used. In addition, as bonding materials, conductive polymers with electronic conductivity and ionic conductive polymers with ionic conductivity can also be used. As conductive polymers with electronic conductivity, for example, polyacetylene can be cited. In this case, the bonding material also plays the function of a conductive auxiliary agent, so a conductive auxiliary agent may not be added. As an ionic conductive polymer with ionic conductivity, for example, an ionic conductive polymer that conducts lithium ions can be used, and a monomer of a polymer compound (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) can be cited with a lithium salt such as LiClO4, LiBF4, LiPF6 or an alkali metal salt with lithium as the main body, etc. The polymerization initiator used for the composite formation may be, for example, a photopolymerization initiator or a thermal polymerization initiator suitable for the above-mentioned monomers. The properties required of the adhesive material include oxidation and reduction resistance and good adhesiveness.
[0072] So far, a specific example of a positive electrode has been shown, but the positive electrode is not limited to these examples. For example, the positive electrode may be a single layer in which the positive electrode current collector 11 and the positive electrode active material 12 are mixed. In addition, for example, Figure 4 and Figure 5 This is a cross-sectional view of another example of the positive electrode according to the first embodiment.
[0073] Figure 4 The positive electrode shown has a positive electrode collector layer 1D and a positive electrode active material layer 1B. The positive electrode collector layer 1D has a positive electrode collector 11, a positive electrode active material 12 and an oxide 13. The oxide 13 is, for example, an oxide containing Ag, such as AgCoO2, AgMn2O4. The oxide 13 contains, for example, both the constituent elements of the positive electrode collector 11 and the constituent elements of the positive electrode active material 12. The oxide 13 prevents oxidation of Ag contained in the positive electrode collector 11. If the oxide 13 is present between the positive electrode collector 11 and the positive electrode active material 12, the cycle characteristics of the all-solid-state battery 10 are improved.
[0074] Figure 5 The positive electrode shown has a positive electrode collector layer 1E, an intermediate layer 1F, and a positive electrode active material layer 1B. The positive electrode collector layer 1E has a positive electrode collector 11 and an oxide 13. The intermediate layer 1F is composed of the oxide 13. Figure 5 The example shown corresponds to an oxide thickness ratio of 13 Figure 4The example shown is thick. The oxide 13 prevents oxidation of Ag contained in the positive electrode current collector 11, and the cycle characteristics of the all-solid-state battery 10 are improved.
[0075] "Solid electrolyte layer"
[0076] The solid electrolyte layer 3 includes a solid electrolyte. A solid electrolyte is a substance that can move ions by an electric field applied from the outside. For example, the solid electrolyte layer 3 conducts lithium ions and blocks the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.
[0077] The solid electrolyte layer 3 includes, for example, a solid electrolyte having a γ-Li3PO4 type crystal structure. The solid electrolyte having a γ-Li3PO4 type crystal structure has excellent ion conductivity. The solid electrolyte is, for example, Li 3+x Si x P 1-x O4、Li 3+x Si x V 1- x O4、Li 3+x Ge x P 1-x O4、Li 3+x Ge x V 1-x O4, etc., preferably Li 3+x Si x P 1-x O4. x satisfies 0.4≤x≤0.8, and preferably satisfies 0.2≤x≤0.6. In addition, the solid electrolyte may be a ternary lithium oxide containing Si, V, Ge, etc.
[0078] "negative electrode"
[0079] The negative electrode 2 includes, for example, a negative electrode current collector layer 2A and a negative electrode active material layer 2B containing a negative electrode active material.
[0080] [Negative electrode current collector]
[0081] The negative electrode current collector layer 2A includes, for example, a negative electrode current collector 21 and a negative electrode active material 22. In this case, the portion between the xy plane passing through the uppermost portion of the negative electrode current collector 21 and the xy plane passing through the lowermost portion is considered to be the negative electrode current collector layer 2A.
[0082] The negative electrode current collector 21 includes, for example, a metal or alloy selected from any one of Ag, Pd, Au, and Pt. The negative electrode current collector 21 is, for example, Ag, an AgPd alloy, a Li-Ag alloy, and a mixture thereof. The negative electrode current collector 21 may be the same as or different from the positive electrode current collector 11. The negative electrode current collector 21 also functions as a negative electrode active material.
[0083] like Figure 3 As shown, the negative electrode current collector layer 2C may be composed of the negative electrode current collector 21. In this case, the negative electrode current collector 21 may be a foil extending in the xy plane, or may be in the form of a pressed product or an extended product.
[0084] [Negative Electrode Active Material Layer]
[0085] The negative electrode active material layer 2B is formed on one or both sides of the negative electrode collector layer 2A. The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may contain a conductive additive, a binder, and the above-mentioned solid electrolyte. When the negative electrode active material layer 2B contains a solid electrolyte, the xy plane passing through the uppermost part of the negative electrode active material and the xy plane passing through the lowermost part are regarded as the negative electrode active material layer 2B.
[0086] (Negative electrode active material)
[0087] The negative electrode active material is a compound that can absorb and release ions. The negative electrode active material is a compound that exhibits a lower potential than the positive electrode active material. The negative electrode active material includes, for example, Li4Ti5O 12 , LiTiO2, Li2TiO3, Li2TiSiO5. The negative electrode active material may contain a plurality of active material materials.
[0088] (Conductive additive)
[0089] The conductive additive improves the electron conductivity of the negative electrode active material layer 2B. The conductive additive can be made of the same material as that of the positive electrode active material layer 1B.
[0090] (Bonding material)
[0091] The binder binds the negative electrode current collector layer 2A and the negative electrode active material layer 2B, the negative electrode active material layer 2B and the solid electrolyte layer 3, and various materials constituting the negative electrode active material layer 2B. The binder can use the same material as the positive electrode active material layer 1B. The content ratio of the binder can also be the same as that of the positive electrode active material layer 1B. As long as the binder is not needed, the binder may not be contained.
[0092] exist Figure 2 In FIG. 1 , an example is shown in which the negative electrode 2 is composed of the negative electrode collector layer 2A and the negative electrode active material layer 2B, but the present invention is not limited to this case. Figure 6 This is an enlarged view of a characteristic portion of another example of the all-solid-state battery according to the first embodiment. Figure 6The negative electrode 2D shown has a negative electrode collector 21 and a solid electrolyte 23. The negative electrode collector 21 is, for example, an Ag alloy. The Ag alloy is, for example, an AgPd alloy or a Li-Ag alloy. The Ag alloy also functions as an active material. If the Ag alloy functions as a negative electrode active material, the all-solid battery becomes high-capacity and the energy density of the all-solid battery is improved.
[0093] "Method for manufacturing all-solid-state batteries"
[0094] Next, a method for manufacturing the all-solid-state battery 10 is described. First, the stacked body 4 is produced. The stacked body 4 is produced by, for example, a simultaneous firing method or a sequential firing method.
[0095] The simultaneous firing method is a method of manufacturing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of firing each layer each time it is formed. The simultaneous firing method can manufacture the laminate 4 with fewer operation steps than the sequential firing method. In addition, the laminate 4 manufactured by the simultaneous firing method is denser than the laminate 4 manufactured by the sequential firing method. The following is an example of the case where the simultaneous firing method is used.
[0096] First, the materials constituting the positive electrode current collector layer 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, the negative electrode active material layer 2B, and the negative electrode current collector layer 2A of the stacked body 4 are made into pastes. Figure 4 In the example shown, the positive electrode current collector 11 is coated with the oxide 13 and then the paste is formed. Figure 5 In the case of the example shown, the material constituting the intermediate layer 1F is also in the form of a paste.
[0097] The method of making each material into a paste is not particularly limited, and for example, a method of mixing powders of each material in a vehicle to obtain a paste can be used. Here, the vehicle is a general term for a medium in a liquid phase. The vehicle includes a solvent and a binder.
[0098] Next, a green sheet is prepared. The green sheet is obtained by applying the paste prepared according to each material on a substrate such as a PET (polyethylene terephthalate) film, drying it as needed, and then peeling off the substrate. The method for applying the paste is not particularly limited, and for example, a known method such as screen printing, coating, transfer, and scraper can be used.
[0099] Next, the green sheets made from each material are stacked in the desired order and number of layers to make a laminated sheet. When stacking the green sheets, alignment and cutting are performed as needed. For example, in the case of making a parallel type or a series-parallel type battery, the green sheets are stacked by aligning the end face of the positive electrode collector layer 1A and the end face of the negative electrode collector layer 2A in a manner that is inconsistent.
[0100] The laminated sheet can be produced by a method of producing a positive electrode unit and a negative electrode unit and stacking these units. The positive electrode unit is a laminated sheet obtained by stacking a solid electrolyte layer 3, a positive electrode active material layer 1B, a positive electrode collector layer 1A, and a positive electrode active material layer 1B in this order. Figure 5 In the case of the example shown, the intermediate layer 1F is stacked between the positive electrode collector layer 1A and the positive electrode active material layer 1B. The negative electrode unit is a laminated sheet in which the solid electrolyte layer 3, the negative electrode active material layer 2B, the negative electrode collector layer 2A, and the negative electrode active material layer 2B are stacked in this order. The solid electrolyte layer 3 of the positive electrode unit and the negative electrode active material layer 2B of the negative electrode unit are stacked in a manner opposite to each other, or the positive electrode active material layer 1B of the positive electrode unit and the solid electrolyte layer 3 of the negative electrode unit are stacked in a manner opposite to each other.
[0101] Next, the prepared laminated sheets are pressurized together to improve the adhesion of each layer. Pressing can be performed, for example, by a molding machine, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during crimping is, for example, set to 40°C to 95°C. Next, the pressurized laminate is cut into chips using a cutting device. Then, the chips are debonded and sintered to obtain a laminated body 4 consisting of a sintered body.
[0102] The debinding process can be performed as a process different from the firing process. If the debinding process is performed, the binder component contained in the chip is heated and decomposed before the firing process, which can inhibit the rapid decomposition of the binder component in the firing process. The debinding process is performed, for example, by heating at a temperature of 300°C to 800°C for 0.1 hours to 10 hours in an atmospheric atmosphere. The atmosphere of the debinding process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not undergo oxidation and reduction or are difficult to undergo oxidation and reduction, and the gas type can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not react with the atmospheric gas. For example, it can be performed in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere obtained by mixing them.
[0103] The firing process is carried out, for example, by placing the chip on a ceramic table. The firing is carried out, for example, by heating to a temperature of 600° C. to 1000° C. in an atmospheric atmosphere. The firing time can be, for example, 0.1 to 3 hours. The atmosphere of the sintering process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode, and the solid electrolyte do not undergo oxidation-reduction or are difficult to undergo oxidation-reduction, and the gas type can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode, and the solid electrolyte do not react with the atmospheric gas. For example, it can be carried out in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere in which they are mixed.
[0104] In addition, the sintered laminate 4 (sintered body) can also be placed in a cylindrical container together with abrasive materials such as aluminum oxide and drum-ground. Thus, the chamfering of the corners of the laminate can be performed. Grinding can be performed using sandblasting. Sandblasting can only remove specific parts, so it is preferred.
[0105] Terminal electrodes 5 and 6 are formed on the mutually opposite sides of the manufactured stacked body 4. The terminal electrodes 5 and 6 can be formed by means of sputtering, dipping, screen printing, spraying, etc. By going through the above steps, a full solid-state battery 10 can be manufactured. When the terminal electrodes 5 and 6 are formed only in the specified parts, they are covered with tape or the like and the above treatment is performed.
[0106] The internal resistance of the all-solid-state battery of this embodiment is low. It is believed that this is because the compound represented by formula (1) used in the positive electrode active material 12 is difficult to react with the solid electrolyte used in the solid electrolyte layer 3. For example, when the positive electrode active material 12 does not contain the compound represented by formula (1) and is composed of LiMn2O4, an intermediate product is generated between the solid electrolyte layer 3 and the positive electrode active material 12. The intermediate product is LiMn2O4 and Li2MnO3 containing excess Li, and is formed by the diffusion and reaction of Li in the solid electrolyte. The intermediate product and the Li-deficient solid electrolyte become the reasons for the increase in the internal resistance of the all-solid-state battery. In contrast, the compound represented by formula (1) used in the positive electrode active material 12 is difficult to react with the solid electrolyte used in the solid electrolyte layer 3, and it is not easy to produce an intermediate product.
[0107] The embodiments of the present invention have been described in detail above with reference to the drawings, but each structure in each embodiment and their combination are merely examples, and addition, omission, replacement and other changes of structures are possible without departing from the gist of the present invention.
[0108] [Example]
[0109] "Example 1"
[0110] (Production of positive electrode paste)
[0111] In the preparation of the positive electrode current collector layer paste, Ag, Pd and LiNi were mixed in a volume ratio of 40:10:50. 0.5 Mn 1.5 O4 powder. Ethyl cellulose and dihydroterpineol are added to the powder and mixed. Ethyl cellulose is a binder and dihydroterpineol is a solvent.
[0112] The positive electrode active material layer paste is LiNi 0.5 Mn 1.5 It is prepared by adding ethyl cellulose and dihydroterpineol to O4 and mixing them.
[0113] (Preparation of Solid Electrolyte Layer Paste)
[0114] Li2CO3, SiO2 and Li3PO4 were used as starting materials and mixed at a molar ratio of 2:1:1. The mixture was wet mixed for 16 hours using water as a dispersion medium using a ball mill. The mixed material was calcined at 950°C for 2 hours to produce Li 3.5 Si 0.5 P 0.5 Then, 100 parts by mass of the calcined powder, 100 parts by mass of ethanol, and 200 parts by mass of toluene were added to a ball mill for wet mixing. Then, 16 parts of a polyvinyl butyral binder and 4.8 parts by mass of butyl benzyl phthalate were further added and mixed to prepare a solid electrolyte layer paste.
[0115] (Preparation of negative electrode paste)
[0116] The negative electrode paste uses Ag, Pd and Li mixed in a volume ratio of 40:10:50. 3.5 Si 0.5 P 0.5 Ethyl cellulose and dihydroterpineol were added to the powder and mixed.
[0117] (Fabrication of all-solid-state batteries)
[0118] Next, the positive electrode unit and the negative electrode unit were made according to the following process. First, on the above-mentioned solid electrolyte layer sheet, the positive electrode active material paste was printed with a thickness of 5μm using screen printing. Then, the printed positive electrode active material paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode active material paste, the positive electrode collector paste was printed with a thickness of 5μm using screen printing. Next, the printed positive electrode collector paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode collector paste, the positive electrode active material paste was printed again with a thickness of 5μm using screen printing and dried. Then, the PET film was peeled off. In this way, a positive electrode unit in which the positive electrode active material layer / positive electrode collector layer / positive electrode active material layer were stacked in sequence on the main surface of the solid electrolyte layer was obtained.
[0119] Next, the negative electrode paste was printed on the main surface of the solid electrolyte layer to a thickness of 10 μm, and then the printed negative electrode paste was dried at 80° C. for 5 minutes.
[0120] In the laminate, a solid electrolyte unit was made by overlapping 5 solid electrolyte layer sheets. It was made by alternately stacking 50 electrode units (25 positive electrode units and 25 negative electrode units) in a manner of clamping the solid electrolyte unit. At this time, the units were stacked staggered so that the collector layer of the odd-numbered electrode units extended only to one end face, and the collector layer of the even-numbered electrode units extended only to the end face on the opposite side. Six solid electrolyte layer sheets were stacked on the stacked unit. Then, it was formed by hot pressing and cut to make a laminated chip. Then, the stacked chips were fired simultaneously to obtain a laminate. Simultaneous firing is to heat up to a firing temperature of 800°C at a heating rate of 200°C / hour in an atmospheric atmosphere, keep at this temperature for 2 hours, and cool naturally after firing.
[0121] By a known method, terminal electrodes 5 and 6 are provided on the sintered laminate (sintered body) to produce a solid-state battery. Figure 6 The volume ratio of each layer does not change between the paste state before sintering and the state after sintering. Ag exists in the form of Ag alone and in the form of being included as a contained element of AgPd alloy.
[0122] 100 identical samples were made and the internal resistance was calculated. The internal resistance was calculated as the average of these samples. The internal resistance was calculated as follows: At 60°C, constant current charging (CC charging) was performed at a constant current of 100μA until the battery voltage reached 3.9V, and then, after stopping for 1 minute, the battery voltage was discharged (CC discharge) at a constant current of 100μA until the battery voltage reached 0V. This process was set as 1 cycle, and the voltage drop (V) from the time of stopping to the start of discharge in the tenth cycle after repeating the process for 10 cycles was divided by the discharge current (A). In addition, the samples made under the same conditions were decomposed, and the volume ratio (Va) of Ag and Ag alloy in the negative electrode collector layer was also calculated.
[0123] "Examples 2 to 5"
[0124] In Examples 2 to 5, LiNi 0.5 Mn 1.5 O4 and LiMn2O4 were used as positive electrode active materials, which was different from Example 1. The internal resistance and the like were obtained under the same conditions as in Example 1. When the positive electrode collector layer and the positive electrode active material layer in Examples 2 to 5 were prepared, the volume ratio of the powders in preparing the paste was set as follows.
[0125] (Example 2)
[0126] Positive electrode current collector layer = Ag:Pd:LiNi 0.5 Mn 1.5O4:LiMn2O4=40:10:40:10
[0127] Positive electrode active material layer = LiNi 0.5 Mn 1.5 O4:LiMn2O4=80:20
[0128] (Example 3)
[0129] Positive electrode current collector layer = Ag:Pd:LiNi 0.5 Mn 1.5 O4:LiMn2O4=40:10:30:20
[0130] Positive electrode active material layer = LiNi 0.5 Mn 1.5 O4:LiMn2O4=60:40
[0131] (Example 4)
[0132] Positive electrode current collector layer = Ag:Pd:LiNi 0.5 Mn 1.5 O4:LiMn2O4=40:10:20:30
[0133] Positive electrode active material layer = LiNi 0.5 Mn 1.5 O4:LiMn2O4=40:60
[0134] (Example 5)
[0135] Positive electrode current collector layer = Ag:Pd:LiNi 0.5 Mn 1.5 O4:LiMn2O4=40:10:10:40
[0136] Positive electrode active material layer = LiNi 0.5 Mn 1.5 O4:LiMn2O4=20:80
[0137] "Examples 6 to 10"
[0138] In Examples 6 to 10, the solid electrolyte is Li 3.5 Si 0.5 P 0.5 O4 changed to Li 3.5 Si 0.5 V 0.5 O4 is different from each of Examples 1 to 5 in this point. The internal resistance and the like were obtained in the same manner as in Example 1 under the other conditions.
[0139] "Comparative Example 1"
[0140] Comparative Example 1 is different from Example 1 in the following points. In Comparative Example 1, the internal resistance and the like were obtained in the same manner as in Example 1.
[0141] Difference 1: In the preparation of the positive electrode current collector layer paste, a powder obtained by mixing Ag and Pd at a volume ratio of 80:20 was used.
[0142] Difference 2: LiMn2O4 is used instead of LiNi in the preparation of the positive electrode active material layer paste. 0.5 Mn 1.5 O4.
[0143] Difference 3: The negative electrode paste is made into two layers: negative electrode current collector layer paste and negative electrode active material layer paste. The negative electrode current collector layer paste uses a powder obtained by mixing Ag and Pd in a volume ratio of 80:20. The negative electrode active material layer paste is made of Li4Ti5O 12 (Li 4 / 3 Ti 5 / 3 O4) was added with ethyl cellulose and dihydroterpineol and mixed to obtain a paste.
[0144] "Comparative Example 2"
[0145] Comparative Example 2 is different from Example 1 in that the positive electrode active material is LiMn2O4. In Comparative Example 2, the internal resistance and the like are obtained in the same manner as in Example 1.
[0146] The results of Examples 1 to 10 and Comparative Example 1 or Comparative Example 2 are summarized in the following Table 1. " / " in Table 1 indicates the ratio at the time of production, and the existence ratio after production is substantially the same as the ratio at the time of production.
[0147] [Table 1]
[0148]
[0149] Comparing Example 1 with Comparative Example 1, the internal resistance of Example 1 was lower than that of Comparative Example 1. This is considered to be because the positive electrode active material in Comparative Example 1 reacted with the solid electrolyte to generate an intermediate product.
[0150] "Examples 11 to 18"
[0151] Examples 11 to 18 differ from Example 1 in that the composition ratio of the positive electrode active material was changed. The internal resistance and the like were obtained in the same manner as in Example 1 under the other conditions.
[0152] In Example 11, LiNi was used 0.1 Mn 1.9 This is different from Example 1 in that O4 is included as the positive electrode active material in the positive electrode active material layer.
[0153] In Example 12, LiNi was used. 0.9 Mn 1.1 This is different from Example 1 in that O4 is included as the positive electrode active material in the positive electrode active material layer.
[0154] In Example 13, LiNi was used 0.1 Mn 1.9 This is different from Example 1 in that O4 is included as the positive electrode active material in the positive electrode current collector layer.
[0155] In Example 14, LiNi was used 0.9 Mn 1.1 This is different from Example 1 in that O4 is included as the positive electrode active material in the positive electrode current collector layer.
[0156] In Example 15, LiNi was used 0.1 Mn 1.9 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0157] In Example 16, LiNi was used 0.4 Mn 1.6 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0158] In Example 17, LiNi was used 0.6 Mn 1.4 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0159] In Example 18, LiNi was used 0.9 Mn 1.1 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0160] "Examples 19 to 24"
[0161] Examples 19 to 24 are different from Example 1 in that the positive electrode active material is changed. The internal resistance and the like are obtained in the same manner as in Example 1 under the other conditions.
[0162] In Example 19, LiCo was used 0.1 Mn 1.9 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0163] In Example 20, LiCo 0.5 Mn1.5 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0164] In Example 21, LiCo was used 0.9 Mn 1.1 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0165] In Example 22, LiTi was used. 0.1 Mn 1.9 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0166] In Example 23, LiTi was used 0.5 Mn 1.5 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0167] In Example 24, LiTi was used 0.9 Mn 1.1 This is different from Example 1 in that O4 is used as the positive electrode active material contained in the positive electrode collector layer and the positive electrode active material layer.
[0168] "Example 25"
[0169] In Example 25, the positive electrode has a single-layer structure of the positive electrode current collector layer instead of a laminated structure of the positive electrode current collector layer and the positive electrode active material layer, which is different from Example 1. Other conditions were similar to those in Example 1, and internal resistance and the like were obtained.
[0170] "Examples 26 to 29"
[0171] In Examples 26 to 29, the Ag, Pd and LiNi 0.5 Mn 1.5 The volume ratio of O4 is different from that of Example 1. The other conditions are the same as those of Example 1, and the internal resistance and the like are obtained.
[0172] In Example 26, the volume ratio of the positive electrode current collector layer was set to Ag:Pd=80:20. That is, in Example 26, LiNi was not added when preparing the negative electrode current collector layer paste. 0.5 Mn 1.5 O4.
[0173] In Example 27, the volume ratio of the positive electrode current collector layer was set to Ag:Pd:LiNi 0.5 Mn 1.5 O4=60:20:20.
[0174] In Example 28, the volume ratio of the positive electrode current collector layer was set to Ag:Pd:LiNi 0.5 Mn 1.5 O4=50:15:35.
[0175] In Example 29, the volume ratio of the positive electrode current collector layer was set to Ag:Pd:LiNi 0.5 Mn 1.5 O4=30:8:62.
[0176] "Examples 30 to 33"
[0177] Examples 30 to 33 differ from Example 1 in that the composition ratio of the solid electrolyte contained in the solid electrolyte layer was changed. The internal resistance and the like were obtained in the same manner as in Example 1 under the other conditions.
[0178] In Example 30, the solid electrolyte used in the solid electrolyte layer is Li 3.1 Si 0.1 P 0.9 O4.
[0179] In Example 31, the solid electrolyte used in the solid electrolyte layer is Li 3.2 Si 0.2 P 0.8 O4.
[0180] In Example 32, the solid electrolyte used as the solid electrolyte layer is Li 3.4 Si 0.4 P 0.6 O4.
[0181] In Example 33, the solid electrolyte used as the solid electrolyte layer is Li 3.6 Si 0.6 P 0.4 O4.
[0182] Next, in Examples 34 to 41, Li-Ag alloy was added to the negative electrode collector layer and the same study was performed. However, the treatment of the Li-Ag alloy was carried out in a glove box with a dew point of -50°C, and the sintering was carried out in an argon atmosphere at a heating rate of 1200°C / hour to a sintering temperature of 800°C, and the temperature was maintained for 20 minutes, and then naturally cooled after sintering.
[0183] "Example 34"
[0184] In Example 34, a portion of the Ag in the negative electrode current collector layer was made into a Li-Ag alloy (Li 3.1Ag) is different from Example 1. The amount of Li in the Li-Ag alloy is determined by quantitative analysis using X-ray diffraction (XRD). The Li-Ag alloy, Ag, Pd and Li 3.5 Si 0.5 P 0.5 The volume ratio of O4 was 2:38:10:50. The other conditions were the same as in Example 1, and the internal resistance of the all-solid-state battery was obtained.
[0185] "Example 35"
[0186] In Example 35, the Li-Ag alloy (Li 3.1 Ag) is changed to Li-Ag alloy (Li 4.7 Ag), which is different from Example 34. The other conditions are the same as in Example 34 to obtain the internal resistance of the all-solid-state battery.
[0187] "Examples 36 and 37"
[0188] In Example 36 and Example 37, Pd was not added when the negative electrode current collector layer was prepared, which is different from Example 34 and Example 35. The volume ratio of the negative electrode current collector layer in Example 36 and Example 37 is Li-Ag alloy:Ag:Li 3.5 Si 0.5 P 0.5 O4=2:48:50. The other conditions were the same as in Example 34, and the internal resistance of the all-solid-state battery was obtained.
[0189] "Examples 38 to 41"
[0190] In Examples 38 to 41, the composition of the solid electrolyte added to the solid electrolyte layer and the negative electrode current collector layer was Li 3.5 Si 0.5 V 0.5 O4 is different from each of Examples 34 to 37. The other conditions were the same as in Example 34, and the internal resistance of the all-solid-state battery was obtained.
[0191] [Table 2]
[0192]
[0193] [Table 3]
[0194]
[0195] [Table 4]
[0196]
Claims
1. An all-solid-state battery, in, A sintered body is provided, the sintered body having: a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode, The positive electrode comprises a compound having a spinel structure, The solid electrolyte layer includes γ-Li 3 PO 4 Type crystal structure solid electrolyte, The compound having a spinel structure is composed of Li α M β Mn 2-β O 4 ...(1) indicates that In the formula (1), M is one or more atoms selected from transition metals, and satisfies 0.8≤α≤1.2 and 0.1≤β≤0.
9.
2. The all-solid-state battery according to claim 1, in, The M is Ni, The formula (1) is composed of Li α Ni β Mn 2-β O 4 ...(2) indicates that In the above formula (2), 0.4≤β≤0.6 is satisfied.
3. The all-solid-state battery according to claim 1, in, The positive electrode further includes at least one selected from Ag or an Ag alloy.
4. The all-solid-state battery according to claim 1, in, The positive electrode comprises a first layer and a second layer, The first layer comprises one or more selected from the compound and Ag or an Ag alloy. The second layer is in contact with at least one major surface of the first layer.
5. The all-solid-state battery according to claim 4, in, The total volume ratio of Ag and the Ag alloy in the first layer is 40% or more and 85% or less.