PDA-coated MIL-101 functionalized ultrafiltration membrane and application thereof in treatment of algae-laden water

Through the design of PDA@MIL-101 functionalized ultrafiltration membrane, the problems of low organic matter removal efficiency and irreversible membrane fouling in high algae water were solved, efficient water treatment was achieved, and the anti-pollution ability and flux recovery rate of the membrane were improved.

CN118751065AActive Publication Date: 2024-10-11SHENZHEN INSTITUTE OF INFORMATION TECHNOLOGY

Patent Information

Application Number
CN202410927253.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-11
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing ultrafiltration membranes have low organic matter removal efficiency when treating high-algae water and serious irreversible membrane pollution, leading to deterioration of water quality. Existing modification methods are complex and may destroy algae cells, affecting the treatment effect.

Method used

PDA@MIL-101 functionalized ultrafiltration membrane is used. By blending PDA@MIL-101 nanomaterials with polyethersulfone, it is prepared through non-solvent-induced phase separation to form an ultrafiltration membrane with a porous structure and improve the hydrophilicity of the membrane. properties and electronegativity, reducing the contact between pollutants and the membrane, and enhancing anti-pollution capabilities.

Benefits of technology

The pure water flux and UV254 rejection rate of the ultrafiltration membrane are increased, and irreversible pollution is reduced. The pure water flux is increased by 1.53 times, the UV254 rejection rate is increased by 17%, and the flux recovery rate is increased by 15%, significantly improving the treatment of high algae water. Effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751065A_ABST
    Figure CN118751065A_ABST
Patent Text Reader

Abstract

The invention discloses a PDA-coated MIL-101 functionalized ultrafiltration membrane and application thereof in treatment of algae-laden water, and belongs to the technical field of ultrafiltration membranes and water treatment. The PDA-coated MIL-101 nanometer material and the polyether sulfone are used as raw materials, the PDA-coated MIL-101 nanometer material is rich in hydroxyl functional groups, the hydrophilicity and the electronegativity of the ultrafiltration membrane are improved, the improvement of the hydrophilicity is beneficial to formation of a hydration layer on the surface of the membrane, a pollution layer formed by contact of pollutants and the membrane is reduced, and the electronegativity of the ultrafiltration membrane is improved. The improvement of the electronegativity increases the repulsive interaction between pollutants and the surface of the membrane, so that the anti-pollution capacity of the membrane is improved. The pure water flux of the PDA-coated MIL-101 functionalized ultrafiltration membrane provided by the invention can reach 440L / (m < 2 >. H), the UV254 retention rate can reach 45%, and the irreversible pollution in three periods is 16%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ultrafiltration membranes and water treatment, and in particular relates to a PDA@MIL-101 functionalized ultrafiltration membrane and application thereof in treating high-algae water. Background Art

[0002] In recent years, with the frequent occurrence of algal blooms in surface water, it has posed a huge challenge to drinking water safety. Suspended pollutants in high-algae water bodies, algal cells and their secreted extracellular organic matter, are the main causes of the deterioration of effluent water quality due to their easy solubility, easy dispersion, and complex composition, affecting the operation effect of conventional water treatment processes. Ultrafiltration has been proven to be an efficient, reliable, and feasible technology for treating high-algae water. Ultrafiltration technology can maintain the integrity of algal cells and avoid the problem of deterioration of effluent water quality caused by algal cell fragmentation, but there are still problems such as low organic matter retention rate and serious membrane fouling. In order to solve the above problems, many scholars have conducted extensive research on pre-membrane pretreatment, such as pre-coagulation and pre-oxidation. However, pretreatment inevitably complicates the process, and even excessive addition of reagents will cause algal cell rupture, leading to deterioration of water quality and aggravating membrane pollution.

[0003] Studies have shown that hydrophilic modification of ultrafiltration membranes can effectively alleviate the irreversible fouling of ultrafiltration membranes. Usually, hydrophilic polymer blending, hydrophilic monomer grafting, coating, blending of hydrophilic nanoparticles and other methods are used to make mixed matrix membranes, including metal oxide nanoparticles, carbon nanomaterials, metal organic frameworks, etc. Recently, metal organic frameworks have been increasingly used in the membrane field. Metal organic frameworks are highly porous nanomaterials formed by the coordination between metal ions and organic ligands. They have great advantages such as large specific surface area, adjustable structure, and easy functionalization. They can effectively improve the hydrophilicity and filtration capacity of ultrafiltration membranes. Wang et al. (“Metal organic framework UiO-66 incorporated ultrafiltration membranes for simultaneous organic matter and heavy metal ions removal”) modified ultrafiltration membranes by blending UIO-66, improving the humic acid removal rate while alleviating the membrane fouling of ultrafiltration membranes. Shaeli et al. ("Long-term stable metal organic framework (MOF) based mixed matrix membranes for ultrafiltration") greatly improved the pure water flux and flux recovery rate of the membrane by adding metal organic frameworks (UiO-66 and UiO-66-NH2) to polyethersulfone and sulfonated polyethersulfone, showing enhanced anti-fouling effect. However, in the field of high algae water treatment, there are few reports on improving the removal efficiency of organic matter while alleviating irreversible fouling of ultrafiltration membranes.

[0004] Therefore, how to provide an ultrafiltration membrane that can improve the removal efficiency of organic matter in high-algae water while alleviating irreversible membrane fouling has become a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a PDA@MIL-101 functionalized ultrafiltration membrane and its application in treating high-algae water.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a PDA@MIL-101 functionalized ultrafiltration membrane. Raw materials for preparing the PDA@MIL-101 functionalized ultrafiltration membrane include PDA@MIL-101 nanomaterials and polyethersulfone.

[0008] Preferably, the mass ratio of the PDA@MIL-101 nanomaterial to polyethersulfone is (0.1-0.2):16.

[0009] Preferably, the structure of the PDA@MIL-101 functionalized ultrafiltration membrane includes a bottom layer void structure, a middle layer finger-like pore structure and a top layer sponge-like pore structure.

[0010] Preferably, the preparation method of the PDA@MIL-101 nanomaterial comprises: mixing a suspension of MIL-101 and dopamine hydrochloride, then adding Tris-HCl buffer, stirring, centrifuging and drying to obtain the PDA@MIL-101 nanomaterial.

[0011] Preferably, the preparation method of the MIL-101 comprises: mixing a CrCl3·6H2O solution and a terephthalic acid solution, heating the mixture, centrifuging, washing and drying to obtain the MIL-101.

[0012] The present invention provides a method for preparing the PDA@MIL-101 functionalized ultrafiltration membrane described in the above technical solution, using PDA@MIL-101 nanomaterial and polyethersulfone as raw materials, and preparing the PDA@MIL-101 functionalized ultrafiltration membrane through non-solvent induced phase separation.

[0013] Preferably, the preparation method of the PDA@MIL-101 functionalized ultrafiltration membrane comprises the following steps: adding polyethersulfone to an N-methylpyrrolidone solution of PDA@MIL-101 nanomaterial and polyvinylpyrrolidone, stirring evenly, and degassing to obtain an ultrafiltration membrane casting liquid; coating the ultrafiltration membrane casting liquid on a substrate, and then scraping the membrane, and then immersing the substrate in water to obtain the PDA@MIL-101 functionalized ultrafiltration membrane.

[0014] Preferably, the mass ratio of the polyethersulfone, PDA@MIL-101 nanomaterial, polyvinyl pyrrolidone and N-methyl pyrrolidone is 16:(0.1-0.2):1:(82.8-82.9).

[0015] Preferably, the soaking time is 10 minutes.

[0016] The present invention also provides the use of the PDA@MIL-101 functionalized ultrafiltration membrane described in the above technical solution in treating high-algae water.

[0017] Compared with the prior art, the present invention has the following advantages and technical effects:

[0018] The invention uses PDA@MIL-101 nanomaterial and polyethersulfone as raw materials. The PDA@MIL-101 nanomaterial is rich in hydroxyl functional groups, which helps to improve the hydrophilicity and electronegativity of the ultrafiltration membrane. The improvement of hydrophilicity is conducive to the formation of a hydration layer on the membrane surface, reducing the pollution layer formed by the contact between pollutants and the membrane. The improvement of electronegativity increases the repulsion between the pollutants and the membrane surface, thereby improving the anti-pollution ability of the membrane.

[0019] The pure water flux of the PDA@MIL-101 functionalized ultrafiltration membrane provided by the present invention can reach 440L / (m 2 h), UV 254 The retention rate can reach 45%, and the irreversible pollution in three cycles is 16%. Compared with the unmodified membrane, the pure water flux is increased by 1.53 times, UV 254 The rejection rate increased by 17% and the flux recovery rate increased by 15%, providing a solid foundation for the wide application of ultrafiltration membranes in high-algae water. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0021] Figure 1 TEM and digital photos of MIL-101 (a) and PDA@MIL-101 nanomaterial (b) in Example 1;

[0022] Figure 2 The XPS graphs (a) of the MIL-101 and PDA@MIL-101 nanomaterials in Example 1 and the FTIR spectra (b) of the PDA, MIL-101 and PDA@MIL-101 nanomaterials in Example 1;

[0023] Figure 3 The SEM images of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2;

[0024] Figure 4 The cross-sectional SEM images of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 at different magnifications;

[0025] Figure 5 FTIR spectra of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2;

[0026] Figure 6 The water contact angles of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 (a) and the Zeta potential diagrams of the ultrafiltration membranes in Example 1 and Comparative Example 1 (b);

[0027] Figure 7The pure water flux and UV of the ultrafiltration membrane in Examples 1-3 and Comparative Examples 1-2 254 Retention rate graph;

[0028] Figure 8 A diagram of the experimental setup for testing the anti-fouling performance of the ultrafiltration membrane;

[0029] Fig. 9 The three circulation flow total graphs (a), membrane pollution resistance graph (b), water flux recovery graph after cleaning (c) of the ultrafiltration membrane in Examples 1-3 and Comparative Examples 1-2, and the surface SEM graph (d) of the ultrafiltration membrane before and after pollution in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] The embodiment of the present invention provides a PDA@MIL-101 functionalized ultrafiltration membrane. The raw materials for preparing the PDA@MIL-101 functionalized ultrafiltration membrane include PDA@MIL-101 nanomaterial and polyethersulfone.

[0033] The invention uses PDA@MIL-101 nanomaterial and polyethersulfone as raw materials. The PDA@MIL-101 nanomaterial is rich in hydroxyl functional groups, which helps to improve the hydrophilicity and electronegativity of the ultrafiltration membrane. The improvement of hydrophilicity is conducive to the formation of a hydration layer on the membrane surface, reducing the pollution layer formed by the contact between pollutants and the membrane. The improvement of electronegativity increases the repulsion between the pollutants and the membrane surface, thereby improving the anti-pollution ability of the membrane.

[0034] In a preferred embodiment, the mass ratio of the PDA@MIL-101 nanomaterial to polyethersulfone is (0.1-0.2): 16, more preferably (0.1-0.15): 16. The present invention controls the amount of the PDA@MIL-101 nanomaterial within the above range, which is conducive to obtaining an ultrafiltration membrane with excellent water permeability and anti-pollution ability. If the amount of the PDA@MIL-101 nanomaterial is too much, it will agglomerate on the membrane surface, resulting in a decrease in the membrane porosity and inhibiting the formation of a straight pore structure, affecting the membrane's water permeability and anti-pollution ability.

[0035] In a preferred embodiment, the structure of the PDA@MIL-101 functionalized ultrafiltration membrane includes a bottom layer void structure, a middle layer finger-like pore structure and a top layer sponge-like pore structure.

[0036] In a preferred embodiment, the preparation method of the PDA@MIL-101 nanomaterial comprises: mixing a suspension of MIL-101 and dopamine hydrochloride, then adding Tris-HCl buffer, stirring, centrifuging and drying to obtain the PDA@MIL-101 nanomaterial.

[0037] In a preferred embodiment, the usage ratio of MIL-101, dopamine hydrochloride and Tris-HCl buffer is 0.1 g:0.1 g:20 mL.

[0038] In a preferred embodiment, the preparation process of the MIL-101 suspension includes: dispersing MIL-101 in a mixture of water and ethanol, and obtaining the MIL-101 suspension by ultrasound; the dosage ratio of MIL-101 to the mixture of water and ethanol is 0.1g:60mL; the volume ratio of water to ethanol in the mixture of water and ethanol is 1:1; and the ultrasound time is 10min.

[0039] In a preferred embodiment, the concentration of the Tris-HCl buffer is 0.01 mol / L, and the pH is 8.5.

[0040] In a preferred embodiment, the preparation method of the MIL-101 comprises: mixing a CrCl3·6H2O solution and a terephthalic acid solution, heating the mixture, centrifuging, washing and drying to obtain the MIL-101.

[0041] In a preferred embodiment, the solvents of the CrCl3·6H2O solution and the terephthalic acid solution are both water; the dosage ratio of CrCl3·6H2O to water in the CrCl3·6H2O solution is 2.66 g:45 mL; the dosage ratio of terephthalic acid to water in the terephthalic acid solution is 1.66 g:45 mL.

[0042] In a preferred embodiment, the volume ratio of the CrCl3·6H2O solution to the terephthalic acid solution is 1:1.

[0043] In a preferred embodiment, the heating temperature is 210° C. and the heating time is 12 hours.

[0044] In a preferred embodiment, the cleaning is specifically cleaning with water and ethanol alternately.

[0045] The present invention provides a method for preparing the PDA@MIL-101 functionalized ultrafiltration membrane described in the above technical solution, using PDA@MIL-101 nanomaterial and polyethersulfone as raw materials, and preparing the PDA@MIL-101 functionalized ultrafiltration membrane through non-solvent induced phase separation.

[0046] In a preferred embodiment, the preparation method of the PDA@MIL-101 functionalized ultrafiltration membrane comprises the following steps: adding polyethersulfone to an N-methylpyrrolidone solution of PDA@MIL-101 nanomaterial and polyvinylpyrrolidone and stirring evenly, degassing to obtain an ultrafiltration membrane casting liquid; coating the ultrafiltration membrane casting liquid on a substrate, then scraping the membrane, and then immersing the substrate in water to obtain the PDA@MIL-101 functionalized ultrafiltration membrane.

[0047] In a preferred embodiment, the mass ratio of the polyethersulfone, PDA@MIL-101 nanomaterial, polyvinyl pyrrolidone and N-methyl pyrrolidone is 16:(0.1-0.2):1:(82.8-82.9).

[0048] In a preferred embodiment, the pretreatment method of the polyethersulfone is: vacuum drying the polyethersulfone powder at 80° C. for 24 hours.

[0049] In a preferred embodiment, the degassing method is static degassing for 12 hours.

[0050] In a preferred embodiment, the substrate is a glass plate; the scraper used for scraping the film is a 150 μm scraper.

[0051] In a preferred embodiment, the soaking time is 10 minutes.

[0052] The present invention also provides the use of the PDA@MIL-101 functionalized ultrafiltration membrane described in the above technical solution in treating high-algae water.

[0053] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0054] Polyethersulfone (PES) (Mn = 100000) was purchased from BASF AG, Germany, analytical grade; N-methylpyrrolidone (NMP) was purchased from Shanghai Aladdin Reagent, analytical grade; polyvinylpyrrolidone (PVP) K30 was purchased from Tianjin Zhonglian Chemical Reagent Co., Ltd., analytical grade; dopamine hydrochloride was purchased from Shanghai McLean Reagent, purity 98%; Tris-HCl buffer was purchased from Xiamen Aimimanni Biotechnology Co., Ltd., analytical grade. CrCl3·6H2O was purchased from Shanghai Aladdin Reagent, purity 98%; terephthalic acid (PTA) was purchased from Shanghai Aladdin Reagent, purity 99%.

[0055] Example 1

[0056] A method for preparing a PDA@MIL-101 functionalized ultrafiltration membrane:

[0057] (1) Dissolve 2.66 g of CrCl3·6H2O in 45 mL of deionized water and stir on a magnetic stirrer for 20 min to completely dissolve to obtain a CrCl3·6H2O solution; dissolve 1.66 g of terephthalic acid (PTA) in 45 mL of deionized water and stir on a magnetic stirrer for 20 min to completely dissolve to obtain a PTA solution; mix the CrCl3·6H2O solution and the PTA solution in a volume ratio of 1:1, place the mixture in an oven at 210°C for drying for 12 h, cool the mixture to room temperature, centrifuge the mixture, wash the precipitate with deionized water and ethanol alternately, and then dry the mixture in an oven at 80°C overnight to obtain a green powder, namely MIL-101.

[0058] (2) 0.1 g of the MIL-101 obtained in step (1) was dispersed in 60 mL of a mixture of deionized water and ethanol in a volume ratio of 1:1, and ultrasonicated for 10 min to obtain a suspension of MIL-101; 0.1 g of dopamine hydrochloride was added to the above MIL-101 suspension, magnetically stirred for 2 min, and then 20 mL of Tris-HCl buffer (0.01 mol / L, pH = 8.5) was injected. After stirring for 24 h, centrifugation was performed, and PDA@MIL-101 nanomaterials were obtained after vacuum drying.

[0059] (3) vacuum drying polyethersulfone (PES) powder at 80° C. for 24 h to obtain dry PES; dissolving polyvinyl pyrrolidone (PVP) and the PDA@MIL-101 obtained in step (2) in N-methylpyrrolidone, adding the above-mentioned dry PES after ultrasonic treatment for 30 min, magnetically stirring for 12 h, standing for 12 h to degas, and obtaining an ultrafiltration membrane casting solution; coating the above-mentioned ultrafiltration membrane casting solution on a clean glass plate, and then scraping the film on the clean glass plate with a 150 μm scraping knife, and then soaking it in deionized water for 10 min to remove excess reagents in the membrane, thereby obtaining a PDA@MIL-101 functionalized ultrafiltration membrane; wherein the mass ratio of polyethersulfone, PDA@MIL-101 nanomaterial, polyvinyl pyrrolidone and N-methylpyrrolidone is 16:0.1:1:82.9.

[0060] Example 2

[0061] The difference from Example 1 is that in step (3), the mass ratio of polyethersulfone, PDA@MIL-101 nanomaterial, polyvinylpyrrolidone and N-methylpyrrolidone is 16:0.15:1:82.85.

[0062] Example 3

[0063] The difference from Example 1 is that in step (3), the mass ratio of polyethersulfone, PDA@MIL-101 nanomaterial, polyvinylpyrrolidone and N-methylpyrrolidone is 16:0.2:1:82.8.

[0064] Comparative Example 1

[0065] The difference from Example 1 is that in step (3), the mass ratio of polyethersulfone, PDA@MIL-101 nanomaterial, polyvinyl pyrrolidone and N-methylpyrrolidone is 16:0:1:83.

[0066] Comparative Example 2

[0067] The difference from Example 1 is that in step (3), the mass ratio of polyethersulfone, PDA@MIL-101 nanomaterial, polyvinylpyrrolidone and N-methylpyrrolidone is 16:0.05:1:82.95.

[0068] The components of the ultrafiltration membrane casting solution in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.

[0069] Table 1 Composition of ultrafiltration membrane casting solution in Examples 1-3 and Comparative Examples 1-2

[0070] Film No. PES (wt%) PVP (wt%) NMP (wt%) PDA@MIL-101 (wt%) Comparative Example 1 M0 16 1 83 -- Comparative Example 2 M1 16 1 82.95 0.05 Example 1 M2 16 1 82.90 0.1 Example 2 M3 16 1 82.85 0.15 Example 3 M4 16 1 82.80 0.2

[0071] The morphology and structure of the MIL-101 and PDA@MIL-101 nanomaterials in Example 1 were characterized by field emission transmission electron microscopy (TEM, Talos-F200X, USA). Figure 1 .

[0072] Figure 1 TEM and digital photos of MIL-101 (a) and PDA@MIL-101 nanomaterial (b) in Example 1. Figure 1 From the TEM image (a), it can be observed that MIL-101 exhibits an octahedral morphology, a particle size between 200-400nm, and a smooth lattice plane with sharp edges and corners, which are typical characteristics of MIL-101 crystals. Figure 1 In the TEM image (b), it can be observed that PDA@MIL-101 exhibits a similar octahedral morphology, with little change in particle size, but the lattice plane is slightly rough, and is a structure that is clearly wrapped in a shell by polydopamine. Figure 1 From the digital photo (inset), it can be seen that MIL-101 has a green powder appearance, which is also the typical color of the metal organic framework MIL-101. The PDA@MIL-101 obtained after polydopamine modification has a brown powder appearance, indicating that polydopamine has been successfully loaded.

[0073] The elemental composition of MIL-101 and PDA@MIL-101 nanomaterials in Example 1 was analyzed using an X-ray photoelectron spectrometer (XPS, EscaLabXi+, USA), and the functional group composition of MIL-101 and PDA@MIL-101 nanomaterials in Example 1 was analyzed using a Fourier transform infrared spectrometer (FTIR, BrukerInvenioS, Germany) with a scanning range of 4000-500 cm -1 , the results are shown in Figure 2 .

[0074] Figure 2 The XPS graph (a) of the MIL-101 and PDA@MIL-101 nanomaterials in Example 1 and the FTIR spectra (b) of the PDA, MIL-101 and PDA@MIL-101 nanomaterials in Example 1 are shown in FIG. Figure 2 (a) It can be seen that MIL-101 contains Cr, O, and C elements. The N element appears in the spectrum after dopamine oxidation self-healing, further indicating that the PDA coating is successfully coated on MIL-101. The C1s spectrum of MIL-101 shows characteristic peaks at binding energies of 284eV and 288eV, representing CC and OC=O, respectively. The binding energies of 577eV and 587ev show Cr 2p3 / 2 and Cr 2p1 / 2 (Cr 3+ ), and the peak becomes weaker after modification. The O1s spectrum peaks with binding energies of 531.7eV and 533.4eV correspond to the oxygen molecules and HOH of the organic ligands, respectively. Figure 2 (b) It can be seen that the OC=O symmetry leads to the -1 A high-intensity absorption peak appears at 1622 cm -1 The absorption peaks at 1018 and 748 cm are caused by the vibrational stretching of the carbonyl group of the ligand terephthalic acid. -1 The characteristic peak appears due to the vibration of the benzene ring inside the nanoparticles. -1 The absorption peak at 1265cm is due to the stretching vibration of Cr-O. -1 The weak absorption peak at 3400cm is caused by the vibration of the amide bond. -1 The broad absorption peak is caused by the vibration of the hydroxyl -OH or -NH functional groups in dopamine. The above results show that the modification of nanoparticles is successful.

[0075] The microstructure morphology of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 was analyzed by scanning electron microscopy (SEM, TESCAN MIRALMS, Czech Republic). Figure 3-4 .

[0076] Figure 3 1-3 and Comparative Example 1-2 are SEM images of the ultrafiltration membranes. Figure 3 It can be seen that when a small amount of PDA@MIL-101 nanomaterial is added, such as M1 and M2, the membrane surface shows a smooth and flat morphology; with the further addition of nanomaterials, nanoparticles gradually appear on the surface of M3 and M4 membranes, which further proves the successful addition of nanoparticles. Figure 3 In M2, the nanoparticles are evenly dispersed and the surface is smooth and flat, which is because polydopamine increases the compatibility between the membrane matrix and the nanoparticles. However, when the addition amount is greater than 0.1wt%, the nanoparticles agglomerate on the surface, which is due to the uneven dispersion of nanoparticles in the casting solution and the increased viscosity of the casting solution caused by excessive addition, which leads to the agglomeration of nanoparticles.

[0077] Figure 4 The cross-sectional SEM images of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 at different magnifications are shown in FIG. Figure 4 It can be seen that all ultrafiltration membranes are composed of three parts: the bottom void structure, the middle finger-like pore structure and the dense sponge-like pore structure at the top of the membrane. From M0 to M2, with the addition of nanoparticles, the pore structure changes from an inclined state to a straight state. The straight pore structure is more conducive to the passage of water molecules, thereby improving the water permeability of the ultrafiltration membrane. From M2 to M4, with the continued addition of nanoparticles, the pore structure continues to change to an inclined state, and the bottom voids of the ultrafiltration membrane are improved. This enhanced structure can improve the mechanical properties of the ultrafiltration membrane and is more conducive to practical applications. The pore structure of the M0 membrane varies in size, while the pores of the modified membrane are more uniform. The above improvements in the membrane pore structure can be analyzed from the thermodynamic and kinetic aspects of the phase transformation process. When a small amount of PDA@MIL-101 nanomaterial is added, the hydrophilicity increases, resulting in the dominance of thermodynamic factors and accelerating the phase separation process; while excessive addition will increase the viscosity of the casting solution, and the phase separation process dominated by kinetics will be transformed into delayed separation, inhibiting the formation of straight finger-like pores.

[0078] The ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 were analyzed using a Fourier transform infrared spectrometer (FTIR, Bruker InvenioS, Germany) with a scanning range of 4000-500 cm -1 , the results are shown in Figure 5 .

[0079] Figure 5 FTIR spectra of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2. Figure 5 It can be seen that all films have high peaks at 1244, 1152 and 1105 cm -1The three characteristic peaks at 3400 cm-1 are attributed to the ether bond and sulfone bond of PES, and the peaks show a weakening trend, which may be related to the reduction of the proportion of relevant surface functional groups. -1 There is an enhanced characteristic peak at the pores, which is the rich hydroxyl group (OH peak) provided by polydopamine. The characteristic peak of M4 is not obvious, which may be due to the agglomeration of nanoparticles, so the increase of surface functional groups is not significant. The FTIR spectrum characterization results can prove the successful incorporation of nanoparticles, and the nanomaterials rich in hydroxyl functional groups help to increase the hydrophilicity and electronegativity of the ultrafiltration membrane.

[0080] The porosity and average pore size of the ultrafiltration membrane were measured by dry and wet weight method. The results are shown in Table 2.

[0081] Wet film (4cm 2 ) was first weighed, and then dried at 100°C for 12 hours to obtain the weight of the dry film. The porosity (ε) was calculated as follows:

[0082]

[0083] Where W1 and W2 are the weights of wet and dry films, respectively; ρ is the density of water, g / cm 3 ; A is the membrane area, cm 2 ; l is the thickness of the film, cm.

[0084] The calculation formula for the average pore size r of the ultrafiltration membrane is:

[0085]

[0086] Where η is the viscosity of water, pa·s; Q is the volume of permeated water, m 3 / s; ΔP is the working pressure, Pa.

[0087] Table 2 Porosity and average pore size of ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2

[0088] Film No. Porosity (%) Pore ​​size (nm) Comparative Example 1 M0 45 43.87 Comparative Example 2 M1 50 42.96 Example 1 M2 62 42.82 Example 2 M3 55 42.49 Example 3 M4 52 42.84

[0089] It can be seen from Table 2 that with the increase of PDA@MIL-101 nanomaterial content, the highest porosity increased from 45% of the original membrane M0 to 62% of M2, and the average pore size of all membranes was between 42-44nm. Compared with the original membrane, the average pore size of the modified membrane was slightly reduced, which is related to the faster phase separation process. Table 2 shows that the PDA@MIL-101 nanoparticle blending significantly increased the porosity of the PES ultrafiltration membrane, but due to the high hydrophilicity of the nanoparticles, excessive addition will increase the viscosity of the casting solution, affect the phase separation, and thus reduce the porosity, which is consistent with the change trend of the cross-sectional SEM image.

[0090] The water contact angle of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 was analyzed using a contact angle / surface tension meter (Lauda Scientific LSA100, Germany). The surface Zeta potential of the ultrafiltration membranes in Examples 1-3 and Comparative Examples 1-2 was analyzed using a solid surface Zeta potential tester (Anton Paarsurpass, Austria). The results are shown in Table 1. Figure 6 .

[0091] Figure 6 The water contact angle (a) of the ultrafiltration membrane in Examples 1-3 and Comparative Examples 1-2 and the Zeta potential (b) of the ultrafiltration membrane in Example 1 and Comparative Example 1. Figure 6 As can be seen in (a), the water contact angle of the M0 membrane is 71°. After adding different amounts of PDA@MIL-101 nanomaterials, the membrane contact angle shows a trend of first decreasing and then increasing, with the M2 membrane having the lowest contact angle of 57.8°. Since polydopamine-modified MIL-101 has good hydrophilicity, the addition of nanoparticles can improve the hydrophilicity of the membrane surface. The rich hydroxyl functional groups of the composite material are conducive to forming hydrogen bonds with water molecules, thereby forming a hydration layer, reducing the direct contact between the hydrophobic components of high algae water and the membrane, and improving the anti-pollution ability of the ultrafiltration membrane. Due to the characteristics of the composite material, the trend of hydrophilicity changes is consistent with the trend of changes in the porosity membrane pore structure. From Figure 6 As can be seen in (b), the membrane surface has a negative charge at pH = 7. This is due to the increase in hydroxyl groups in the modified membrane (e.g. Figure 5 ), the hydroxyl functional groups increase the electronegativity of the membrane surface. As the pH changes from 5 to 9, the Zeta potential of the original membrane decreases from -19mV to -41mV, while the M2 membrane decreases from -20mV to -53mV. Compared with the unmodified membrane, the electronegativity of the modified membrane Zeta potential increases by 1.5 times. This is related to the abundant hydroxyl groups provided by polydopamine. The increased electronegativity can better repel negatively charged pollutants and provide better anti-pollution ability.

[0092] Pure water flux and UV of ultrafiltration membrane 254 Retention rate test, the results are shown in Figure 7 .

[0093] Pure water flux test: Use Shanghai Mosu ultrafiltration cup for dead-end filtration. First, pre-press the membrane sample at 0.15MPa for 30 minutes. After the test system is stable, measure the pure water flux at 0.1MPa. The calculation formula of pure water flux is:

[0094]

[0095] Where JW is the pure water flux, L / (m 2 ·h); V is the volume of the filtrate during the measurement time, L; A is the effective filtration area of ​​the ultrafiltration membrane, m 2; t is the ultrafiltration membrane filtration time, h.

[0096] High algae solution interception rate test: A laboratory-cultured Microcystis aeruginosa solution was used as a simulated natural water body, where the concentration of Microcystis aeruginosa was OD 680 =0.100~0.130,UV 254 =0.030~0.035. Use UV-visible spectrophotometer at wavelength 254nm to measure the absorbance of the permeate, and obtain the concentration of the permeate and the original solution through the standard curve; where UV 254 The calculation formula of interception rate is:

[0097]

[0098] Where R is UV 254 Retention rate, %; Cp is the mass concentration of the original solution, μg / L; Cf is the mass concentration of the permeate, μg / L.

[0099] Figure 7 The pure water flux and UV of the ultrafiltration membrane in Examples 1-3 and Comparative Examples 1-2 254 Retention rate graph, in which the bar graph represents pure water flux and the line graph represents UV 254 Retention rate. Figure 7 It can be seen that with the addition of nanoparticles, the water flux of the modified membrane is related to UV 254 The retention rate is higher than that of the unmodified membrane. The water flux of M2 reaches 440L / (m 2 ·h), equivalent to the original membrane 287L / (m 2 ·h) is 1.53 times. The water flux of ultrafiltration membrane is often affected by many factors. M2 membrane has a straight pore structure, increased porosity, increased hydrophilicity, etc. In addition, metal organic frameworks are porous materials, and MIL-101 has Pore ​​size, much larger than the diameter of a water molecule This structure is conducive to the transmission of water molecules. The decrease in pure water flux of M3 and M4 can be attributed to the tilted membrane pore structure and reduced hydrophilicity. 254 The retention rate of the M2 membrane is only 28%, while that of the M2 membrane can reach up to 45%. There are a large number of small molecular organic matter in high algae water, which can easily pass through the membrane, resulting in the unmodified PES membrane being sensitive to UV rays. 254 The size repulsion effect is poor. Both the extracellular organic matter and the surface of the nanocomposite membrane are negatively charged. Compared with the pure PES membrane, the nanocomposite membrane has a stronger charge repulsion between the extracellular organic matter and the membrane surface. Figure 6 (b), thereby enhancing the repulsion of extracellular organic matter. In addition, the slightly reduced average pore size (Table 2) and increased hydrophilicity ( Figure 6 (a)) is also UV 254 Factors that increase the removal rate.

[0100] In order to test the anti-pollution performance of the ultrafiltration membrane, the test was carried out by alternating filtration of deionized water and high algae solution. The experimental device is as follows: Figure 8 As shown, 200 mL of pure water was first filtered at 0.1 MPa, and then the solution was replaced with 300 mL of high algae water solution. The electronic balance recorded the flux change; 200 mL of deionized water was then used for in-situ backwashing; the solution was converted to pure water again, and the membrane was filtered alternately for 3 times. The flux recovery rate FRR after three cycles of the membrane was calculated. The results are shown in Fig. 9 .

[0101]

[0102] R r =R t -R ir ×100%

[0103] Where FRR is the flux recovery rate, R ir is the irreversible pollution in the nth cycle, R t For reversible pollution, R r is the total pollution, J e(n) is the terminal flux at the end of the nth cycle, J s(n+1) is the initial flux of the n+1th cycle, J0 is the initial flux, J s4 is the initial flux of the 4th cycle.

[0104] Fig. 9 The three circulation flow total graphs (a), membrane pollution resistance graph (b), water flux recovery graph after cleaning (c) of the ultrafiltration membrane in Examples 1-3 and Comparative Examples 1-2, and the surface SEM graph (d) of the ultrafiltration membrane before and after pollution in Example 1 and Comparative Example 1. Fig. 9 (a) is the test result of five membrane circulation filtration. Due to the interaction between algae cells and their secretions and the membrane surface during the filtration process, the flux of high algae water is lower than that of pure water, and it shows a typical two-stage decline trend. First, the filter cake layer formed rapidly by algae cells causes the flux to drop rapidly, and then the extracellular organic matter continues to compress the filter cake layer, causing the flux to drop further. Due to the increased hydrophilicity and electronegativity, such as Fig. 9 (c) The water flux recovery rate of the modified membrane is better than that of the unmodified M0 membrane. The flux recovery rate of the M2 membrane reached 84% after three cycles. The flux recovery rate trend also showed a trend of first increasing and then decreasing. The flux recovery rate change trend is consistent with the membrane hydrophilicity trend. The irreversible fouling of the membrane accounts for Fig. 9(b), the irreversible pollution of the modified membrane was significantly reduced after three cycles, with M0 irreversible pollution of 31% and M2 irreversible pollution of 16%, and the irreversible pollution was reduced by 15%. The effective mitigation of the modified membrane is mainly attributed to the increase in membrane hydrophilicity and electronegativity. The hydration layer formed on the membrane surface reduces the pollution layer formed by the contact between the pollutants and the membrane. The negative charge on the membrane surface increases the repulsion between the pollutants and the membrane surface, improving the membrane's anti-pollution ability. Fig. 9 As can be seen in (d), after backwashing, uneven and significant pollutant deposition forms on the surface of the M0 membrane, while the M2 membrane shows no significant difference. In summary, the anti-pollution ability of the modified membranes is improved in filtering high-algae water solutions. Among them, the M2 membrane shows the best effect in filtering high-algae water and pure water.

[0105] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A PDA@MIL-101 functionalized ultrafiltration membrane, characterized in that: The raw materials for preparing the PDA@MIL-101 functionalized ultrafiltration membrane include PDA@MIL-101 nanomaterials and polyethersulfone.

2. The PDA@MIL-101 functionalized ultrafiltration membrane according to claim 1, characterized in that: The mass ratio of the PDA@MIL-101 nanomaterial to polyethersulfone is (0.1-0.2):

16.

3. The PDA@MIL-101 functionalized ultrafiltration membrane according to claim 1, characterized in that: The structural composition of the PDA@MIL-101 functionalized ultrafiltration membrane includes a bottom layer void structure, a middle layer finger-like pore structure and a top layer sponge-like pore structure.

4. The PDA@MIL-101 functionalized ultrafiltration membrane according to claim 1, characterized in that: The preparation method of the PDA@MIL-101 nanomaterial comprises: mixing a suspension of MIL-101 and dopamine hydrochloride, then adding Tris-HCl buffer, stirring, centrifuging and drying to obtain the PDA@MIL-101 nanomaterial.

5. The PDA@MIL-101 functionalized ultrafiltration membrane according to claim 4, characterized in that: The preparation method of the MIL-101 comprises: mixing a CrCl3·6H2O solution and a terephthalic acid solution, heating the mixture, centrifuging, washing and drying to obtain the MIL-101.

6. The method for preparing the PDA@MIL-101 functionalized ultrafiltration membrane according to any one of claims 1 to 5, characterized in that: The PDA@MIL-101 functionalized ultrafiltration membrane is prepared by using PDA@MIL-101 nanomaterial and polyethersulfone as raw materials through non-solvent induced phase separation.

7. The preparation method according to claim 6, characterized in that: The following steps are involved: Add polyethersulfone to an N-methylpyrrolidone solution of PDA@MIL-101 nanomaterial and polyvinylpyrrolidone, stir evenly, and degas to obtain an ultrafiltration membrane casting liquid; coat the ultrafiltration membrane casting liquid on a substrate, then scrape the membrane, and then soak the substrate in water to obtain the PDA@MIL-101 functionalized ultrafiltration membrane.

8. The preparation method according to claim 7, characterized in that: The mass ratio of the polyethersulfone, PDA@MIL-101 nanomaterial, polyvinyl pyrrolidone and N-methyl pyrrolidone is 16:(0.1-0.2):1:(82.8-82.9).

9. The preparation method according to claim 7, characterized in that: The soaking time is 10 minutes.

10. Use of the PDA@MIL-101 functionalized ultrafiltration membrane according to any one of claims 1 to 5 in treating high algae-containing water.

Citation Information

Patent Citations

  • Method for modifying outer surface of ultrafiltration membrane by microfiltration porous protection layer

    CN108176242A

  • MOF (metal organic framework) modified nanofiltration / reverse osmosis membrane and application thereof

    CN109224861A

  • Preparation method of porous material ultrahigh-loading-capacity mixed matrix membrane

    CN110052182A

  • Pervaporation desalination asymmetric membrane and preparation method thereof

    CN110479102A

  • Preparation method and application of bisphenol A-based molecularly-imprinted high-selectivity nanocomposite on surface of hydrophilic metal organic framework

    CN110813253A

Cited By

  • SPDA modified MIL-101 modified polyether sulfone ultrafiltration membrane as well as preparation method and application thereof

    CN119345906A