Preparation method of 5N high-purity rhenium powder

Through the combined method of vapor deposition and hydrogen reduction, the existing problems of high equipment requirements and incomplete removal of impurities in the preparation of high-purity rhenium powder are solved. The preparation of high-purity rhenium powder is achieved, and the recovery rate of rhenium is increased to more than 85%. , the process is simplified and equipment requirements are reduced.

CN118751931APending Publication Date: 2024-10-11YUNNAN COPPER CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410880197.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing high-purity rhenium powder preparation methods have problems such as high equipment requirements, complex processes, low rhenium recovery rates, and incomplete impurity removal. In particular, the recrystallization method and ion exchange method have high requirements on equipment conditions, and it is difficult to deeply remove tungsten, Molybdenum and other impurities.

Method used

The crude ammonium rhenate is subjected to two-stage multi-temperature zone heat treatment using the vapor deposition method, and the reaction temperature and atmosphere conditions are controlled to realize the chemical reaction and phase change reaction of the ammonium rhenate, and then high-purity rhenium powder of more than 99.999% is obtained through hydrogen reduction. , simplifying the process and reducing equipment requirements.

Benefits of technology

The preparation of high-purity rhenium powder is realized, which solves the problem of incomplete removal of impurities in ammonium rhenate, reduces equipment condition requirements, is simple to operate, and the recovery rate of rhenium reaches more than 85%, and avoids secondary pollution of impurities and rhenium loss.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of 5N high-purity rhenium powder, and belongs to the technical field of high-purity metal purification. According to the method, two-section multi-temperature-zone heat treatment is conducted on crude ammonium rhenate under inert gas and oxygen through a vapor deposition method, the chemical reaction and the phase change reaction of the ammonium rhenate are regulated and controlled by combining regulation and control of the reaction temperature and the atmosphere condition, effective removal of rhenium-containing substances and impurities is achieved, then ammonia water is added for recrystallization, and high-purity ammonium rhenate is obtained. And the rhenium powder with the purity of 99.999% or above is obtained through hydrogen reduction. The method can solve the problem that impurity elements in ammonium rhenate are not thoroughly removed, meanwhile, the requirement for equipment conditions is low, operation is easy, cation exchange resin does not need to be introduced, and secondary pollution of impurities and loss of rhenium are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-purity metal purification, and specifically relates to a method for preparing 5N high-purity rhenium powder. Background Art

[0002] Rhenium is an important strategic rare metal with extremely high melting and boiling points. Rhenium is an important strategic resource for the modern aviation engine industry. Rhenium and its alloys and compounds have special optical, electrical, and magnetic properties and are widely used in electronic communications, aerospace, energy, and life sciences. They are an important supporting material for the development of modern science and technology.

[0003] At present, the main preparation method for producing metal rhenium powder in industry is the ammonium rhenate hydrogen reduction method. The purity of rhenium powder mainly depends on the purity of ammonium rhenate. The purity of commercially available ammonium rhenate is generally 99% to 99.99%, and its impurities mainly include alkali metals (K, Na), alkaline earth metals (Ca), refractory metals (W, Mo) and trace amounts of Cu, Ni, Fe, Si, etc. There are two main commonly used methods for purifying ammonium perrhenate: one is the recrystallization method, in which the ammonium rhenate solution is heated to a supersaturated state and then cooled to room temperature. Most impurities are more difficult to crystallize than ammonium rhenate and are enriched in the crystallization mother liquor, thereby obtaining high-purity ammonium rhenate crystals; however, this method limits the recovery rate of rhenium. At the same time, due to the small difference in the solubility of ammonium tungstate, ammonium molybdate and ammonium rhenate, it is difficult to achieve deep removal of impurity ions such as tungsten and molybdenum by recrystallization. The other is the ion exchange method, in which the impurity ions (K + , Ca 2 + , Fe 3+ Mg 2+ , Cu 2+ 、Ni 2+ 、Al 3+ ), by selecting a suitable cation exchange resin for selective adsorption, the ammonium rhenate is purified, and then high-purity rhenium powder is obtained by hydrogen reduction.

[0004] Patent application CN107052357A discloses a method for preparing high-purity rhenium powder. The method mainly includes the steps of: ammonium rhenate purification - centrifugal atomization - primary reduction - secondary reduction. The purity of ammonium rhenate is raised to more than 99.99% by using equipment such as a spray drying tower and a centrifugal atomizer, and then rhenium powder is obtained by two hydrogen reductions. The method has a short process flow, and can directly purify ammonium rhenate in a spray drying tower, and can prepare rhenium powder of more than 99.995%. However, the method has high requirements for equipment and large investment, which is not conducive to its popularization and use.

[0005] Patent application CN115026297B discloses a high-purity rhenium powder and its preparation process. The process uses ion exchange resin to prepare a high-concentration high-purity perrhenic acid solution through concentration, and then sprays the prepared ammonium rhenate solution into a hydrogen reduction reactor to prepare high-purity rhenium powder. The process is short and has a high recovery rate of metal rhenium powder, but this method has problems such as high requirements for equipment and process control.

[0006] Patent application CN114653940B discloses a method for purifying high-purity rhenium by a two-step hydrogen-vacuum sintering method. The method includes four steps: pressing, pre-sintering, high-temperature sintering, and post-treatment. First, high-purity rhenium powder is pressed, then pre-sintered in a hydrogen atmosphere, and then sintered at high temperature in a vacuum atmosphere. Finally, the sintering furnace is cooled and vacuuming is stopped to obtain purified high-purity rhenium. However, this process has high requirements on equipment. Summary of the invention

[0007] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing 5N high-purity rhenium powder.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing 5N high-purity rhenium powder comprises the following steps:

[0010] (1) using a vapor deposition method, the crude ammonium rhenate is placed in an inert atmosphere for heating and insulation, then placed in an oxygen atmosphere for heating and insulation, and naturally cooled to room temperature to obtain a rhenium-containing vapor deposit on the tube wall of a vapor deposition device;

[0011] (2) dissolving the rhenium-containing vapor deposit in water, and then adding ammonia water to obtain ammonium perrhenate;

[0012] (3) Ammonium perrhenate is heated and reduced in a hydrogen atmosphere to obtain high-purity rhenium powder.

[0013] As a preferred embodiment of the present invention, the purity of the crude ammonium rhenate is ≤99%.

[0014] As a preferred embodiment of the present invention, the heating and heat preservation time in the inert atmosphere is 4-6 hours, the temperature is 200-300° C., and the flow rate of the inert gas is 75-85 mL / min.

[0015] The inert atmosphere is nitrogen.

[0016] As a preferred embodiment of the present invention, the heating and heat preservation time in the oxygen atmosphere is 3-6 hours, the temperature is 220-300° C., and the flow rate of oxygen is 80-150 mL / min.

[0017] More preferably, the flow rate of the oxygen is 100-120 mL / min.

[0018] As a preferred embodiment of the present invention, in the step (2), ammonia water is added to filter the precipitate, and the filter residue is ammonium perrhenate. Ammonia water is further added to the filtrate and then filtered, and the filter residues are combined to obtain ammonium perrhenate.

[0019] As a preferred embodiment of the present invention, the temperature of the heating reduction is 650-800°C and the time is 1-2h.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention adopts a vapor deposition method to perform a two-stage multi-temperature zone heat treatment on crude ammonium rhenate, and combines the control of reaction temperature and atmosphere conditions to control the chemical reaction and phase change reaction of ammonium rhenate, thereby achieving effective removal of rhenium-containing substances and impurities, and then obtains high-purity ammonium rhenate by concentration and recrystallization, and obtains rhenium powder with a purity of more than 99.999% through hydrogen reduction.

[0022] (2) The method of the present invention can solve the problem of incomplete removal of impurity elements in ammonium rhenate. At the same time, it has low requirements on equipment conditions and is simple to operate. It does not require the introduction of cation exchange resin, thus avoiding secondary contamination of impurities and loss of rhenium. The recovery rate of rhenium in the present invention is more than 85%. DETAILED DESCRIPTION

[0023] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0024] The ammonium rhenate used in this embodiment and the comparative example has a purity of 99%, and its impurities mainly include alkali metals (K, Na), alkaline earth metals (Ca), refractory metals (W, Mo) and trace amounts of Cu, Ni, Fe, Si, etc.

[0025] Example 1

[0026] A method for preparing 5N high-purity rhenium powder comprises the following steps:

[0027] (1) Take 20 g of crude ammonium rhenate and spread it evenly in a clean quartz boat, and then put the quartz boat into a clean quartz tube. High-purity nitrogen (nitrogen flow rate is 75 mL / min) is introduced into the quartz tube for protection and sealing. The crude ammonium rhenate is pretreated, and the treatment temperature is gradually increased from room temperature to 200°C. The treatment is sealed in a nitrogen atmosphere for 4 hours, and finally it is allowed to stand and cool to room temperature to obtain rhenium oxide.

[0028] (2) The rhenium oxide is evenly spread in a clean porcelain boat, and the porcelain boat is placed in a clean quartz tube. Oxygen is first introduced into the quartz tube, and then the rhenium oxide is oxidized and sublimated. During this process, the oxygen gas rate in the quartz tube is 100 mL / min, and the treatment is carried out at 250°C for 4 hours. Finally, the oxygen supply is stopped, and the boat is sealed and allowed to cool to room temperature. The rhenium-containing vapor phase deposit generated by the reaction is on the inner wall of the clean high-temperature resistant container, and the remaining solid phase material in the boat is impurities.

[0029] (3) Rinium-containing vapor deposits deposited on the inner wall of a clean quartz tube are rinsed with ultrapure water and sufficient ammonia water is added to obtain an ammonium perrhenate solution. Ammonium perrhenate undergoes chemical precipitation, and the filter residue is ammonium perrhenate after filtration. Ammonia water is continuously added to the filtrate and then filtered. The filter residues are combined and dried to obtain high-purity ammonium perrhenate.

[0030] (4) Ammonium perrhenate is placed in a high-purity zirconium oxide boat and hydrogen reduced at 650°C for 1.2 hours to obtain high-purity rhenium powder with a purity of up to 99.99959011%.

[0031] Example 2

[0032] The only difference between the method for preparing 5N high-purity rhenium powder in this embodiment and that in embodiment 1 is that:

[0033] In the step (1), the treatment temperature is gradually increased from room temperature to 230°C.

[0034] The purity of the obtained high-purity rhenium powder is 99.999141%.

[0035] Example 3

[0036] The only difference between the method for preparing 5N high-purity rhenium powder in this embodiment and that in embodiment 1 is that:

[0037] In the step (1), the treatment temperature is gradually increased from room temperature to 260°C; in the step (2), the temperature of the oxidative sublimation treatment is 400°C.

[0038] The purity of the obtained high-purity rhenium powder is 99.999719%.

[0039] Example 4

[0040] The only difference between the method for preparing 5N high-purity rhenium powder in this embodiment and that in embodiment 1 is that:

[0041] In the step (1), the treatment temperature is gradually increased from room temperature to 300°C.

[0042] The purity of the obtained high-purity rhenium powder is 99.999748%.

[0043] Example 5

[0044] A method for preparing 5N high-purity rhenium powder comprises the following steps:

[0045] (1) Take 20 g of crude ammonium rhenate and spread it evenly in a clean quartz boat, and then put the quartz boat into a clean quartz tube. High-purity nitrogen (nitrogen flow rate is 85 mL / min) is passed into the quartz tube for protection and sealing. The crude ammonium rhenate is pretreated, and the treatment temperature is gradually increased from room temperature to 200°C. The treatment is sealed in a nitrogen atmosphere for 6 hours, and finally it is allowed to stand and cool to room temperature to obtain rhenium oxide.

[0046] (2) The rhenium oxide is evenly spread in a clean porcelain boat, and the porcelain boat is placed in a clean quartz tube. Oxygen is first introduced into the quartz tube, and then the rhenium oxide is oxidized and sublimated. During this process, the oxygen gas rate in the quartz tube is 80 mL / min, and the treatment is carried out at 300°C for 6 hours. Finally, the oxygen supply is stopped, and the boat is sealed and allowed to cool to room temperature. The rhenium-containing vapor deposit generated by the reaction is on the inner wall of the clean high-temperature resistant container, and the remaining solid phase material in the boat is impurities.

[0047] (3) Rinium-containing vapor deposits deposited on the inner wall of a clean quartz tube are rinsed with ultrapure water and sufficient ammonia water is added to obtain an ammonium perrhenate solution. Ammonium perrhenate undergoes chemical precipitation, and the filter residue is ammonium perrhenate after filtration. Ammonia water is continuously added to the filtrate and then filtered. The filter residues are combined and dried to obtain high-purity ammonium perrhenate.

[0048] (4) Ammonium perrhenate is placed in a high-purity zirconium oxide boat and hydrogen reduced at 800°C for 1 hour to obtain high-purity rhenium powder with a purity of up to 99.999012%.

[0049] Example 6

[0050] A method for preparing 5N high-purity rhenium powder comprises the following steps:

[0051] (1) Take 20 g of crude ammonium rhenate and spread it evenly in a clean quartz boat, and then put the quartz boat into a clean quartz tube. High-purity nitrogen (nitrogen flow rate is 85 mL / min) is passed into the quartz tube for protection and sealing. The crude ammonium rhenate is pretreated, and the treatment temperature is gradually increased from room temperature to 200°C. The treatment is sealed in a nitrogen atmosphere for 4 hours, and finally it is allowed to stand and cool to room temperature to obtain rhenium oxide.

[0052] (2) The rhenium oxide is evenly spread in a clean porcelain boat, and the porcelain boat is placed in a clean quartz tube. Oxygen is first introduced into the quartz tube, and then the rhenium oxide is oxidized and sublimated. During this process, the oxygen gas rate in the quartz tube is 150 mL / min, and the treatment is carried out at 220°C for 3 hours. Finally, the oxygen supply is stopped, and the boat is sealed and allowed to cool to room temperature. The rhenium-containing vapor phase deposit generated by the reaction is on the inner wall of the clean high-temperature resistant container, and the remaining solid phase material in the boat is impurities.

[0053] (3) Rinium-containing vapor deposits deposited on the inner wall of a clean quartz tube are rinsed with ultrapure water and sufficient ammonia water is added to obtain an ammonium perrhenate solution. Ammonium perrhenate undergoes chemical precipitation, and the filter residue is ammonium perrhenate after filtration. Ammonia water is continuously added to the filtrate and then filtered. The filter residues are combined and dried to obtain high-purity ammonium perrhenate.

[0054] (4) Ammonium perrhenate is placed in a high-purity zirconium oxide boat and hydrogen reduced at 700°C for 2 hours to obtain high-purity rhenium powder with a purity of up to 99.999113%.

[0055] Comparative Example 1

[0056] The only difference between the method for preparing a high-purity rhenium powder in this comparative example and the method for preparing a 5N high-purity rhenium powder in Example 1 is that the crude ammonium rhenate is directly oxidized and sublimated in oxygen without being pretreated under nitrogen conditions.

[0057] The purity of the high-purity rhenium powder obtained can reach 99.997748%.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing 5N high-purity rhenium powder, characterized in that: The steps include: (1) using a vapor deposition method, the crude ammonium rhenate is placed in an inert atmosphere for heating and insulation, then placed in an oxygen atmosphere for heating and insulation, and naturally cooled to room temperature to obtain a rhenium-containing vapor deposit on the tube wall of a vapor deposition device; (2) dissolving the rhenium-containing vapor deposit in water, and then adding ammonia water to obtain ammonium perrhenate; (3) Ammonium perrhenate is heated and reduced in a hydrogen atmosphere to obtain high-purity rhenium powder.

2. The method for preparing the 5N high-purity rhenium powder according to claim 1, characterized in that: The purity of the crude ammonium rhenate is ≤99%.

3. The method for preparing 5N high-purity rhenium powder according to claim 1, characterized in that: The heating and heat preservation time in the inert atmosphere is 4-6 hours, the temperature is 200-300° C., and the flow rate of the inert gas is 75-85 mL / min.

4. The method for preparing 5N high-purity rhenium powder according to claim 1, characterized in that: The heating and heat preservation time in the oxygen atmosphere is 3-6 hours, the temperature is 220-300° C., and the flow rate of oxygen is 80-150 mL / min.

5. The method for preparing 5N high-purity rhenium powder according to claim 1, characterized in that: The flow rate of the oxygen is 100-120 mL / min.

6. The method for preparing 5N high-purity rhenium powder according to claim 1, characterized in that: In the step (2), ammonia water is added to filter the precipitate, and the filter residue is ammonium perrhenate. Ammonia water is further added to the filtrate and then filtered, and the filter residues are combined to obtain ammonium perrhenate.

7. The method for preparing 5N high-purity rhenium powder according to claim 1, characterized in that: The temperature of the heating reduction is 650-800° C. and the time is 1-2 hours.

Citation Information

Cited By

  • Preparation method of rhenium trioxide and rhenium dioxide

    CN121292525A