An additive manufacturing method for refractory high-entropy alloys and its application

By using laser deposition and remelting technology to deposit refractory element powders layer by layer, the problem of difficult forming in traditional methods has been solved, and the efficient preparation and performance improvement of large-size refractory high-entropy alloys have been achieved.

CN118751933BActive Publication Date: 2026-11-17HARBIN ENG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410785494.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2026-11-17
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Traditional additive manufacturing technology is difficult to effectively form powders of high-melting-point refractory elements, and traditional alloy powder making processes are complex in terms of composition design and performance control of refractory high-entropy alloys, making the preparation of refractory high-entropy alloys difficult.

Method used

A refractory high-entropy alloy is prepared by using laser deposition combined with laser remelting technology to deposit and remelt a mixture of refractory element powders layer by layer, and then achieving in-situ alloying through a laser directional energy deposition system.

Benefits of technology

This method enables the efficient preparation of large-size refractory high-entropy alloys with good metallurgical bonding, simplifies composition design and performance control, reduces production costs, and improves the strength and plasticity of the alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751933B_ABST
    Figure CN118751933B_ABST
Patent Text Reader

Abstract

The invention discloses an additive manufacturing method for refractory high-entropy alloys and its applications. The manufacturing method involves directly using large-size Nb, Ta, Ti, Hf, and Zr alloys. 2.5 A mixture of five high-melting-point spherical powders of Nb was used to achieve a good metallurgical bond between refractory elements through laser-directed energy deposition combined with laser remelting technology. The atomic percentages of the additively manufactured high-entropy alloy were Nb: 40%, Ta: 25%, Ti: 15%, Hf: 15%, and Zr: 5%. The product prepared by the above method has a completely body-centered cubic structure and has excellent room temperature strength and ductility. This is the first time in China that a large-size additively manufactured refractory high-entropy alloy has been prepared directly using a mixture of Ta-containing spherical powders. It solves the problems of traditional additive manufacturing technology's difficulty in forming high-melting-point powders, and the complexity of performance control and inconvenience of composition design for refractory high-entropy alloys in traditional powder preparation processes. It expands the ideas for additive manufacturing of refractory high-entropy alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an additive manufacturing method and application of refractory high-entropy alloys, and relates to the fields of refractory high-entropy alloys and additive manufacturing technology. Background Technology

[0002] High-entropy alloys are a new type of alloy material composed of five or more elements in equal or near-equal atomic ratios. These alloys exhibit high atomic-scale disorder, existing in a state of random arrangement. In 2010, Senkov et al. [1] Based on the concept of high-entropy alloys, the concept of refractory high-entropy alloys was first proposed and has attracted widespread attention. Refractory high-entropy alloys generally have a stable single-phase structure and exhibit excellent high-temperature performance, corrosion resistance, and creep resistance.

[0003] Refractory high-entropy alloys are mainly composed of refractory metallic elements such as Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W. The vast differences in melting points among these elements pose a significant challenge to their fabrication. Currently, the most common fabrication method is arc melting, which often requires complex performance control to achieve superior microstructure and mechanical properties. [2] However, excessive complexity also presents many inconveniences for the composition design process of refractory high-entropy alloys. [3] In general, the main challenges in preparing refractory high-entropy alloys lie in the complex composition design, diverse preparation processes, and precise performance control. Despite these challenges, researchers continue to strive to find better preparation methods to meet the needs of various applications due to the excellent properties of refractory high-entropy alloys.

[0004] Additive manufacturing technology creates parts by depositing materials layer by layer. For high-entropy alloys, additive manufacturing can directly form complex structural parts with high machining accuracy, fast cooling rate, fine microstructure, and uniform composition. This technology is suitable for forming high-performance complex structural parts, such as aerospace components used under extreme conditions and nuclear reactor fuel pipes. It can also be used to manufacture biomimetic materials for repairing or replacing medical devices. Furthermore, additive manufacturing technology can use elemental powders for in-situ alloying to print finished products, avoiding lengthy development processes. Zhejiang University used refractory element powders for laser deposition, and the printed TiZrHfNb alloy exhibited a room temperature tensile yield strength of ~1034 MPa and a ductility of ~18.5%. [4] .

[0005] In additive manufacturing, the inherently short thermal cycling time limits the flow of molten elements and the formation of microstructures. For high-melting-point refractory elements such as W, Ta, and Nb, complete melting is difficult to guarantee. Higher temperature gradients generate significant residual stress, which can lead to deformation and cracking of parts.

[0006] Laser remelting technology can melt unmelted powder particles by repeatedly scanning the deposited layer, ensuring better metallurgical bonding between refractory elements and eliminating surface and internal defects in parts. Furthermore, remelting allows residual gases in the molten pool to escape to the surface, eliminating internal defects. Researchers are currently attempting to integrate this technology into the additive manufacturing process of refractory high-entropy alloys. Ruhr University Bochum in Germany has for the first time directly alloyed a mixture of refractory element powders in situ using laser deposition combined with laser remelting technology to obtain a NbTaTiHfZr high-entropy alloy. [5] .

[0007] To address the aforementioned problems, this invention proposes a method for preparing refractory high-entropy alloys using laser deposition combined with laser remelting technology. This method utilizes laser deposition combined with laser remelting technology to melt a mixture of high-melting-point refractory element powders (highest melting point Ta: 3017℃), thereby obtaining a refractory high-entropy alloy. Summary of the Invention

[0008] To address the challenges of traditional additive manufacturing techniques in shaping powders of high-melting-point refractory elements, and the complexities and inconveniences in controlling the performance and designing the composition of high-entropy alloys in traditional alloy powder preparation processes, this invention provides an additive manufacturing method and application for refractory high-entropy alloys.

[0009] The specific technical solution of this invention is as follows: an additive manufacturing method for refractory high-entropy alloys, wherein a scanning path file is established in the laser deposition system software, and an industrial robot scans the given path. A mixture of refractory element powders is fed in through a powder feeder, and the mixed powder is deposited onto a TA2 substrate using a fiber laser. The specific preparation process is as follows:

[0010] Step 1: On the TA2 substrate, print 6 layers as the bottom layer using a low power parameter of 1000W;

[0011] Step 2: Starting from the 7th layer, gradually increase the output power, and remelt once after each layer is deposited to ensure that the high melting point element powder is completely melted;

[0012] Step 3: Starting from the 10th layer, print and remelt using a power parameter of 2700W;

[0013] Step 4: Repeat step 10 until the desired height is reached;

[0014] Step 5: After all scanning is completed and the sample has cooled, a single-walled refractory high-entropy alloy sample is obtained.

[0015] Preferably, the elemental composition of the refractory high-entropy alloy is Nb, Ta, Ti, Hf and Zr, and the molar percentage of each element is Nb: 40%, Ta: 25%, Ti: 15%, Hf: 15% and Zr: 5%.

[0016] Preferably, Nb, Ta, Ti, Hf, and Zr with a purity exceeding 99.95% are used. 2.5 Five Nb powders were uniformly mixed in a sealed glass container, then in-situ alloyed using laser-directed energy deposition technology, and layered together to form the final product.

[0017] Preferably, the Nb, Ta, Ti, Hf and Zr 2.5 The particle sizes of the five Nb powders are all 53–150 μm.

[0018] Preferably, the Nb, Ta, Ti, Hf and Zr 2.5 Before printing, the Nb powder was weighed in a molar ratio of 8:5:3:3:1 and then mixed evenly in a sealed glass container.

[0019] Preferably, the uniformly mixed powder is dried in a drying oven at 120°C for 2 hours before printing.

[0020] Preferably, a TA2 substrate of appropriate size and 10mm thickness is selected, and the surface of the substrate is cleaned with alcohol until it is clean, free of oil and dust.

[0021] Preferably, during the deposition process, the sealed deposition chamber is purified with 99.99% pure argon gas throughout the process, with a gas flow rate of 20 L / min. The powder delivery gas is also 99.99% pure argon gas, with a pressure of 0.2–0.3 MPa.

[0022] Preferably, the deposition height of a single layer in the laser deposition process is 0.2 mm, the cladding head is raised by 0.2 mm in each powder feeding process, and the deposition head is not raised in the remelting process.

[0023] The present invention also provides a second aspect: a product obtained by the additive manufacturing method of any of the above-described refractory high-entropy alloys.

[0024] Advantages and beneficial effects of the present invention:

[0025] The additive manufacturing technology for refractory high-entropy alloys provided by this invention is the first in China to directly use a mixture of Ta-containing spherical powders to prepare large-size additive manufacturing high-entropy alloys. It solves the problems of traditional additive manufacturing technology's difficulty in forming high-melting-point Ta powder, and the complexity of traditional powder preparation processes in controlling the performance of refractory high-entropy alloys and the inconvenience of composition design.

[0026] By employing laser-directed energy deposition combined with laser remelting technology, a good metallurgical bond was achieved in a mixture of Ta-containing spherical powders, enabling the preparation of large-sized refractory high-entropy alloy samples. This method offers advantages such as simple processing, short production cycle, and low production cost. The prepared refractory high-entropy alloy exhibits good strength and plasticity at room temperature, expanding the possibilities for additive manufacturing of refractory high-entropy alloys. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the preparation method of the present invention;

[0028] Figure 2 This is a photograph of a sample of the additive manufacturing of the refractory high-entropy alloy described in this invention.

[0029] Figure 3 This is an optical microscope image of the refractory high-entropy alloy described in this invention;

[0030] Figure 4 Here is a SEM image of the refractory high-entropy alloy described in this invention;

[0031] Figure 5 This is a tensile stress-strain curve of the refractory high-entropy alloy described in this invention at room temperature. Detailed Implementation

[0032] Combined with appendix Figures 1-5 The additive manufacturing method for the refractory high-entropy alloy of the present invention will be further described in detail below.

[0033] The additive manufacturing method for the refractory high-entropy alloy uses Nb, Ta, Ti, Hf, and Zr with a purity exceeding 99.95%. 2.5 Five types of Nb powder, with particle sizes ranging from 53 to 150 μm, were directly printed by stacking the powder materials layer by layer using a laser-directed energy deposition system.

[0034] The Nb, Ta, Ti, Hf and Zr mentioned 2.5 Before printing, Nb powder was weighed in a molar ratio of 8:5:3:3:1 and mixed thoroughly in a sealed glass container. The mixture was then dried in a 120°C oven for 2 hours prior to printing.

[0035] The laser-directed energy deposition system is equipped with a fiber laser (1080nm wavelength, 12000W maximum output power), an industrial robot, a powder feeder, and a cladding head, with a spot diameter of 1.3mm and a gun distance of 20mm.

[0036] SEM analysis was performed using an APREO S LOVAC high-resolution scanning electron microscope.

[0037] The room temperature tensile test was conducted using a 5-ton electronic universal testing machine. The gauge length of the tensile specimen was 5 × 2 × 1.5 mm. 3 At least three specimens were measured at a strain rate of 0.001 / s to obtain the final engineering stress-strain curve.

[0038] In the additive manufacturing method described above, a TA2 substrate of appropriate size and 10mm thickness is selected, and the surface of the substrate is cleaned with alcohol until it is clean, free of oil and dust.

[0039] The additive manufacturing method described herein involves establishing a scanning path file in the system software, scanning the given path using an industrial robot, simultaneously feeding mixed powder into the system using the powder feeder, and depositing the powder onto the TA2 substrate using a fiber laser.

[0040] The specific preparation process is as follows:

[0041] Step 1: On the TA2 substrate, print 6 layers as the bottom layer using a low power parameter of 1000W.

[0042] Step 2: Starting from layer 7, gradually increase the output power. After each layer is deposited, reduce the scanning speed and remelt once with the same power to ensure that the high-melting-point element powder is completely melted.

[0043] Step 3: Starting from the 10th layer, print and remelt using a power parameter of 2700W.

[0044] Step 4: Repeat step 10 until the desired height is reached.

[0045] Step 5: After all scanning is completed and the sample has cooled, a single-walled refractory high-entropy alloy sample is obtained. Specific laser deposition parameters are shown in Table 1.

[0046] Table 1. Laser Deposition Parameters:

[0047]

[0048] During the deposition process, the sealed deposition chamber is continuously protected by 99.99% pure argon gas at a flow rate of 20 L / min. The powder delivery gas is also 99.99% pure argon gas at a pressure of 0.2–0.3 MPa.

[0049] The laser deposition process described above has a single-layer deposition height of 0.2 mm, and the cladding head is raised by 0.2 mm during each powder feeding process, while the deposition head is not raised during the remelting process.

[0050] The prepared refractory high-entropy alloy has a molar percentage of Nb: 40%, Ta: 25%, Ti: 15%, Hf: 15%, and Zr: 5%, and is composed entirely of body-centered cubic phase.

[0051] The prepared refractory high-entropy alloy has a room temperature tensile yield strength of approximately 786.6 MPa, a tensile strength of 818.6 MPa, and an elongation after fracture of 14.1%.

Claims

1. An additive manufacturing method for a refractory high-entropy alloy, comprising: establishing a scanning path file in laser deposition system software; having an industrial robot scan a given path; feeding a mixture of refractory element powders via a powder feeder; and depositing the mixed powder onto a TA2 substrate using a fiber laser, characterized in that: The specific preparation process is as follows: Step 1: On the TA2 substrate, print 6 layers as the bottom layer using a low power parameter of 1000W; Step 2: Starting from the 7th layer, gradually increase the output power, and remelt once after each layer is deposited to ensure that the high melting point element powder is completely melted; Step 3: Starting from the 10th layer, print and remelt using a power parameter of 2700W; Step 4: Repeat step 10 until the desired height is reached; Step 5: After all scanning is completed and the sample has cooled, a single-walled refractory high-entropy alloy sample is obtained. The elemental composition of the refractory high-entropy alloy is Nb, Ta, Ti, Hf and Zr, with the molar percentage of each element being Nb: 40%, Ta: 25%, Ti: 15%, Hf: 15% and Zr: 5%.

2. The additive manufacturing method for a refractory high-entropy alloy according to claim 1, characterized in that: It uses Nb, Ta, Ti, Hf, and Zr with a purity exceeding 99.95%. 2.5 Five types of Nb powder were used as raw materials. They were uniformly mixed in a sealed glass container and then in-situ alloyed using laser-directed energy deposition technology, and then stacked layer by layer to form the final product.

3. The additive manufacturing method for a refractory high-entropy alloy according to claim 2, characterized in that: The Nb, Ta, Ti, Hf and Zr mentioned 2.5 The particle sizes of the five Nb powders are all 53–150 μm.

4. The additive manufacturing method for a refractory high-entropy alloy according to claim 2, characterized in that: The Nb, Ta, Ti, Hf and Zr mentioned 2.5 Before printing, the Nb powder was weighed in a molar ratio of 8:5:3:3:1 and then mixed evenly in a sealed glass container.

5. The additive manufacturing method for a refractory high-entropy alloy according to claim 4, characterized in that: The uniformly mixed powder was dried in a 120°C oven for 2 hours before printing.

6. The additive manufacturing method for a refractory high-entropy alloy according to claim 1, characterized in that: Select a 10mm thick TA2 substrate and clean the surface of the substrate with alcohol until it is clean, free of oil and dust.

7. The additive manufacturing method for a refractory high-entropy alloy according to claim 1, 2, 3 or 4, characterized in that: During the deposition process, the sealed deposition chamber is protected by 99.99% pure argon gas at a flow rate of 20 L / min. The powder delivery gas is also 99.99% pure argon gas at a pressure of 0.2–0.3 MPa.

8. The additive manufacturing method for a refractory high-entropy alloy according to claim 7, characterized in that: In the laser deposition process, the single-layer deposition height is 0.2 mm. The deposition head is raised by 0.2 mm during each powder feeding process, and the deposition head is not raised during the remelting process.

9. A single-walled sample of a refractory high-entropy alloy prepared by the additive manufacturing method of any one of claims 1 to 8.

Citation Information

Patent Citations

  • Microalloyed Ti-Zr-Hf-V-Nb-Ta refractory high-entropy alloy and preparation method thereof

    CN108220742A

  • Method for preparing TiAl alloy structural member by selective laser melting

    CN109202080A