Multi-effect modification method for mold surface
By spraying a combination of silicon carbide and aluminum oxide particles under compressed gas, the problem that traditional detection methods are difficult to accurately detect the protection effect of non-carburizing or non-nitriding parts is solved, multi-effect modification of the mold surface is achieved, and the mechanical properties are improved. and detection accuracy, extending the service life of the mold.
Patent Information
- Application Number
- CN202410866817.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional detection methods are difficult to accurately detect the protection effect of non-carburized or non-nitrided parts, resulting in some insufficient protection not being detected, and there are hardness differences on the mold surface after shot peening, which affects the reliability of the detection results.
The silicon carbide and alumina particle composition is rapidly sprayed onto the mold surface under the action of compressed gas, and the particles are prepared by the rolling oscillation method to form a mixture with a particle size of 20 to 40 μm. The injection speed is 200 to 500m/S to ensure that the mold surface is smooth and flat. , and detect the hardness through the difference in smoothness to achieve accurate detection.
It improves the mechanical strength, wear resistance, fatigue resistance and corrosion resistance of the mold, cleans up the machining and polishing lines, avoids air entrainment, enhances the detection accuracy of carburizing or nitriding protection effects, and prolongs the use of the mold. life.
Smart Images

Figure CN118752418A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal mold surface treatment, and in particular relates to a multi-effect modification method for a mold surface. Background Art
[0002] Shot peening is a surface strengthening process widely used in factories. There are steel shots, cast iron shots, glass shots, ceramic shots, etc. It is easy to clean the inner and outer surfaces of complex workpieces and the inner walls of pipes, and is not restricted by the site. It can improve the mechanical strength, wear resistance, fatigue resistance and corrosion resistance of parts. When used for surface activation of stainless steel molds before nitriding treatment, the dense passivation film on the surface of stainless steel can be removed to facilitate nitriding treatment; after shot peening, the mold surface is quickly sprayed with high-hardness particles to form uniform tiny pits, and the original lines after polishing or machine tool processing are cleaned up. When the aluminum liquid flows through the mold surface, there is no influence of the lines, and the die-casting production is smoother, avoiding local turbulence of the aluminum liquid due to the influence of the lines, resulting in product defects such as air entrainment; at the same time, after shot peening, the mold surface undergoes local deformation under the impact of high-hardness particles, forming a certain compressive stress, which can improve the fatigue strength of the mold and extend its service life; the original grain size of 20 to 40μm on the mold surface is broken under the impact potential energy of superhard particles to form smaller grains, which play a fine grain strengthening role in the cracking failure of the mold, further greatly improving the service life of the mold; it can also clean the sticky aluminum, rust, oil stains and residual release agent on the surface of the die-casting mold.
[0003] When the mold needs to be partially carburized or nitrided, a preventive agent is usually applied to the non-treated parts for protection. After the carburized or nitrided surface treatment, there is a very obvious hardness difference between the protected and non-protected parts. The traditional detection method is to determine the protection effect by testing the hardness of the non-carburized or non-nitrided parts. This detection method is slow and has limitations. Due to the possibility of random test points, some areas with insufficient protection may not be detected. Summary of the invention
[0004] The purpose of the present invention is to provide a multi-effect modification method for the mold surface in view of the above technical problems, which can improve the mechanical strength, wear resistance, fatigue resistance and corrosion resistance of parts and components, and at the same time be applied to the precise detection of non-carburizing or non-nitriding parts.
[0005] The multi-effect modification method of the mold surface in the technical solution of the present invention comprises rapidly spraying the microparticle composition onto the mold surface under the action of compressed gas.
[0006] Furthermore, the pressure of the compressed air is 0.8-1.0 MPa.
[0007] Furthermore, the speed of the rapid spraying of the microparticle composition is 200-500 m / s.
[0008] Further, the particle composition is a mixture of silicon carbide particles and aluminum oxide particles.
[0009] Furthermore, the mass ratio of silicon carbide particles to aluminum oxide particles in the particle composition is 6-8:2-4; through the appropriate mass ratio of silicon carbide particles to aluminum oxide particles, a good modification treatment effect of the mold surface is ensured, making the treated mold surface smooth and flat.
[0010] Furthermore, the hardness of the silicon carbide particles is greater than Mohs 9.5.
[0011] Furthermore, the hardness of the aluminum oxide particles is greater than Mohs 8.5.
[0012] Furthermore, both silicon carbide particles and aluminum oxide particles are prepared by rolling and oscillating method. The silicon carbide particles and aluminum oxide particles prepared by rolling and oscillating method can ensure their self-sharpening property. When sprayed onto the mold surface, they are impacted and broken into smaller particles, maintaining good cutting ability and producing good modification effect on the surface of the die-casting mold.
[0013] Furthermore, during the rolling oscillation, the rolling pressure is 4-5t, the rotation speed is 20-50rpm / min, the rolling time is 150-200h, the oscillation frequency is 50-100HZ, and the oscillation time is 60-100min.
[0014] Furthermore, the particle diameters of the silicon carbide particles and the aluminum oxide particles are both 20 to 40 μm.
[0015] When a microparticle composition with a smaller particle size impacts a small groove of a workpiece with high kinetic energy, it will not deform the workpiece and can maintain good cutting friction performance, which can produce a greater beneficial effect on the surface of the die-casting mold.
[0016] The present invention also provides the application of the above-mentioned multi-effect modification method in removing machining knife marks and polishing marks on the surface of a mold and detecting the protective effect of a carburized or nitrided mold.
[0017] There will inevitably be lines on the mold surface after polishing or machine processing. When the aluminum liquid flows through the mold surface, local turbulence is easily caused by the knife lines or polishing lines, resulting in undesirable phenomena such as air entrainment. After the mold is modified using the modification method of the present invention, the surface is quickly sprayed with high-hardness particles to form uniform tiny pits, and the original lines are cleaned up, so that there is no influence of the lines on the flow direction of the aluminum liquid, the die-casting production is smoother, the flow of aluminum liquid is effectively improved, and the occurrence of undesirable phenomena such as air entrainment and turbulence is avoided.
[0018] After the mold is treated by the rapid injection of ultra-hard particles in the present invention, different parts of the surface have different resistance to particle impact due to the difference in hardness, and the surface finish of the mold is obviously different. The carburized or nitrided parts have high hardness, strong resistance to particle impact, and the best surface finish; on the contrary, the protected parts have low hardness, poor resistance to particle impact, and rough surface because they are not carburized or nitrided; the hardness detection points can be selected in a targeted manner through the difference in finish to ensure the reliability and accuracy of the test results and avoid missed detection.
[0019] At the same time, the above-mentioned multi-effect modification method can also be used to remove the molten metamorphic layer produced by the mold discharge machining; break up the surface grains to form finer grains, play the role of fine grain strengthening, form a certain compressive stress on the mold surface, improve the fatigue strength of the mold, and effectively extend the service life of the mold; remove the oxide layer on the mold surface, activate the metal, and shorten the time required for nitriding and carburizing.
[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0021] (1) Improving the mechanical strength, wear resistance, fatigue resistance and corrosion resistance of the mold by rapidly spraying the microparticle composition onto the mold surface under the action of compressed gas;
[0022] (2) The silicon carbide particles and alumina particles prepared by the rolling and oscillation method have good self-sharpening properties. When sprayed onto the mold surface, they are crushed into smaller particles by impact, maintaining good cutting ability and ensuring the mold surface modification effect;
[0023] (3) The present invention uses a microparticle composition with a relatively small particle size. When impacting a small groove of a workpiece with high kinetic energy, the workpiece will not be deformed by the impact, and good cutting friction performance can be maintained, thus producing a good modification effect on the surface of the die-casting mold;
[0024] (4) The multi-effect modification method of the present invention can improve the surface texture of the mold and avoid local turbulence when the aluminum liquid flows through the mold surface, resulting in undesirable phenomena such as air entrainment;
[0025] (5) The multi-effect modification method of the present invention has good effects in removing machining marks and polishing marks on the mold surface and detecting the protective effect of carburizing or nitriding molds. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Comparison pictures of the mold surface before and after multi-effect modification in Example 1: (a) after modification, (b) before modification
[0027] Figure 2Comparison pictures of the surface of the mold processed by the machine tool before and after the multi-effect modification in Example 9: (a) picture before modification, (b) microscope picture before modification, (c) picture after modification, (d) microscope picture after modification;
[0028] Figure 3 The pictures of the carburized mold and the surface after multi-effect modification in Example 10 are as follows: (a) before carburization, (b) after carburization, and (c) after modification;
[0029] Figure 4 This is a picture of the mold surface after grinding and polishing in Comparative Example 3. DETAILED DESCRIPTION
[0030] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not used for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0031] The silicon carbide particles in the following examples and comparative examples were purchased from Yongkang Shengjiu Shot Blasting Materials Co., Ltd., and the aluminum oxide particles were purchased from Zhengzhou Shengyang Refractory Materials Technology Co., Ltd.
[0032] The silicon carbide particles and alumina particles purchased above are processed to a particle size of 20-40 μm by a rolling and oscillation method. In the rolling and oscillation method, the rolling pressure is 4.5t, the rotation speed is 30rpm / min, the rolling time is 150-200h, the oscillation frequency is 80HZ, and the oscillation time is 60-100min.
[0033] Example 1
[0034] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spraying speed of 300 m / s under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 30 μm; the mold surface before and after modification is as follows Figure 1 As shown, the surface of the modified mold is obviously clean and smooth.
[0035] Example 2
[0036] The multi-effect modification method of the mold surface in this embodiment includes spraying a particulate composition onto the surface of the die-casting mold at a spray speed of 350 m / S under the action of compressed gas, wherein the particulate composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 7:3, the particle size of the silicon carbide particles is 25 μm, and the particle size of the aluminum oxide particles is 35 μm.
[0037] Example 3
[0038] The multi-effect modification method of the mold surface in this embodiment includes spraying a particulate composition onto the surface of the die-casting mold at a spray speed of 400 m / S under the action of compressed gas, wherein the particulate composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 8:2, the particle size of the silicon carbide particles is 35 μm, and the particle size of the aluminum oxide particles is 40 μm.
[0039] Example 4
[0040] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spray speed of 300 m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 5:5, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 30 μm.
[0041] Example 5
[0042] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spray speed of 300 m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 4:6, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 30 μm.
[0043] Example 6
[0044] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spray speed of 300 m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 15 μm.
[0045] Example 7
[0046] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spray speed of 300 m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 45 μm.
[0047] Example 8
[0048] The multi-effect modification method of the mold surface in this embodiment includes spraying a particle composition onto the surface of the die-casting mold at a spray speed of 300 m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 45 μm, and the silicon carbide particles and the aluminum oxide particles are obtained by ball milling.
[0049] Example 9
[0050] The multi-effect modification method of the mold surface of this embodiment includes spraying a particle composition onto the mold surface processed by a machine tool at a spraying speed of 300 m / s under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 30 μm; the mold surface before and after modification is as follows Figure 2 (b) and Figure 2 As shown in (c), the surface of the modified mold is obviously clean and smooth without any lines.
[0051] Example 10
[0052] The multi-effect modification method of the mold surface of this embodiment includes spraying a particle composition onto the mold surface after carburization treatment at a spraying speed of 300m / S under the action of compressed gas, wherein the particle composition is a mixture of silicon carbide particles and aluminum oxide particles in a mass ratio of 6:4, and the particle sizes of the silicon carbide particles and the aluminum oxide particles are both 30μm; Figure 3 As shown in (b), after carburizing, part of the protective part falls off, causing the protected part to be carburized and have higher hardness and better finish. The protected part has low hardness, poor impact resistance and poor finish. The difference in finish can be used to quickly determine the abnormal part, such as Figure 3 (c) as shown.
[0053] Comparative Example 1
[0054] The multi-effect modification method of the mold surface of the comparative example includes spraying aluminum oxide particles onto the surface of the die-casting mold at a spraying speed of 300 m / S under the action of compressed gas, and the particle size of the aluminum oxide particles is 30 μm.
[0055] Comparative Example 2
[0056] The multi-effect modification method of the mold surface of the comparative example includes spraying silicon carbide particles onto the surface of the die-casting mold at a spraying speed of 300 m / S under the action of compressed gas, and the particle size of the silicon carbide particles is 30 μm.
[0057] Comparative Example 3
[0058] This comparative example is to grind and polish the surface of the die casting mold. Figure 3 As shown, there are still obvious textures.
[0059] After the die-casting mold surfaces of Examples 1-3 were modified by multiple effects, the mechanical strength, wear resistance, fatigue resistance and corrosion resistance of the molds were significantly improved; the microparticle composition used in Example 4 contained too much silicon carbide particles and too little aluminum oxide particles, which would cause the microparticle composition to have too much spraying effect on the workpiece surface, resulting in more small sharp corners and other uneven places, which is not conducive to the implementation of subsequent other surface treatments; the microparticle composition used in Example 5 contained too little silicon carbide particles and too much aluminum oxide particles, which deteriorated the grinding and cutting ability of the workpiece surface and increased the surface roughness of the workpiece; the microparticle composition used in Example 6 had a smaller particle size and a lower weight, and was very easy to present an umbrella-shaped distribution under high-speed airflow. The particles are scattered and cannot cover narrow gaps, and the kinetic energy generated is small, the force on the workpiece surface is too small, and the modification effect is poor. The particle size of the particle composition used in Example 7 is large, and the kinetic energy generated is also large, which can easily cause the shape of the workpiece to deform, and some plate-like products may even warp and deform. In Example 8, silicon carbide particles and aluminum oxide particles are obtained by ball milling, and the surface is relatively smooth and flat, the cutting ability is poor, and the surface modification effect is poor. In Comparative Example 1, only aluminum oxide particles are used to modify the mold surface, and Comparative Example 2 only silicon carbide particles are used to modify the mold surface. The impact ability on the mold surface is obviously poor, and the surface roughness and activation effect of the workpiece after treatment are also poor.
[0060] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. A multi-effect modification method for a mold surface, characterized in that: It involves rapidly spraying a particulate composition onto a mold surface under the action of compressed gas.
2. The multi-effect modification method according to claim 1, characterized in that: The pressure of compressed air is 0.8~1.0MPa.
3. The multi-effect modification method according to claim 1, characterized in that: The speed of the quick spraying of the microparticle composition is 200 to 500 m / s.
4. The multi-effect modification method according to claim 1, characterized in that: The particle composition is a mixture of silicon carbide particles and aluminum oxide particles.
5. The multi-effect modification method according to claim 4, characterized in that: The mass ratio of silicon carbide particles to aluminum oxide particles in the particle composition is 6-8:2-4.
6. The multi-effect modification method according to claim 4 or 5, characterized in that: The hardness of silicon carbide particles is greater than Mohs 9.
5.
7. The multi-effect modification method according to claim 4 or 5, characterized in that: The hardness of the aluminum oxide particles is greater than 8.5 on the Mohs scale.
8. The multi-effect modification method according to claim 4, characterized in that: Silicon carbide particles and aluminum oxide particles are both prepared by rolling and oscillation method.
9. The multi-effect modification method according to claim 8, characterized in that: During rolling oscillation, the rolling pressure is 4-5t, the rotation speed is 20-50rpm / min, the rolling time is 150-200h, the oscillation frequency is 50-100HZ, and the oscillation time is 60-100min.
10. The multi-effect modification method according to claim 4, characterized in that: The particle sizes of the silicon carbide fine particles and the aluminum oxide fine particles are both 20 to 40 μm.
Citation Information
Patent Citations
Method for producing diamond micro-powder by using vibration ball mill
CN102989560A
Aluminum pressure casting die surface coating processing process and coated aluminum pressure casting die
CN108893707A
Production method for precise elastic abrasive particles
CN110861236A
Shot peening strengthening method for surface of die-casting die
CN116463483A
Method of and apparatus for grit blast damage free score initiation
US4427142A