Lithium ion battery positive electrode material based on iron tailings and preparation method thereof
Li2FeSiO4 is prepared from iron tailings and combined with lithium hydroxide and carbon layer modification, which solves the problem of low conductivity of lithium-ion battery cathode materials, improves rate performance and electrochemical performance, while reducing preparation costs, and realizing iron tailings resources efficient utilization.
Patent Information
- Application Number
- CN202411032457.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The conductivity of Li2FeSiO4 prepared by the existing technology is low, resulting in low rate characteristics, making it difficult to effectively improve the electrochemical performance of lithium-ion batteries, and the preparation cost is high.
Iron tailings are used as iron and silicon sources, and Li2FeSiO4 is prepared through acid leaching and hydrothermal methods. The iron and silicon elements in the iron tailings are used, combined with lithium hydroxide and carbon layers, for surface modification to improve conductivity and rate performance. .
It achieves high conductivity and good rate performance of lithium-ion battery cathode materials, reduces preparation costs, promotes the comprehensive utilization of iron tailings resources and improves the performance of lithium-ion batteries.
Smart Images

Figure CN118754142A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a lithium ion battery positive electrode material based on iron tailings and a preparation method thereof. Background Art
[0002] The most critical component of lithium-ion batteries is the positive electrode material, and the safety, reliability and service life of lithium-ion batteries are directly related to the properties of the positive electrode material. Therefore, how to improve the safety of lithium-ion batteries has become one of the hot topics in today's scientific research field.
[0003] Orthosilicate material Li2MSiO4, where M = any one of Fe, Mn and Co, as a polyanion positive electrode material for lithium-ion batteries, has attracted extensive attention from scholars at home and abroad due to its high theoretical specific capacity and high energy density. Among them, compared with LiCoO2, LiMn2O4 and LiFePO4 positive electrode materials, Li2FeSiO4 has excellent thermal stability and safety, and the main elements of its preparation raw materials are Si and Fe, which are abundant in reserves, low in price, non-hygroscopic and environmentally friendly, making Li2FeSiO4 able to be used in large-scale power energy storage batteries at a sustainable level, with good market application prospects. Summary of the invention
[0004] In order to solve the problem that the conductivity of Li2FeSiO4 prepared by the above-mentioned prior art is low, resulting in low rate characteristics, and it is difficult to effectively improve the electrochemical performance of lithium-ion batteries if Li2FeSiO4 is directly used as a lithium-ion positive electrode material. The present invention proposes a method that can improve the conductivity of Li2FeSiO4 and reduce the preparation cost, so that Li2FeSiO4 can be used as a lithium-ion battery positive electrode material.
[0005] The present invention provides a lithium-ion battery cathode material based on iron tailings and a preparation method thereof by the following technical solutions:
[0006] The present invention takes into account that the prior art mostly uses pure raw materials as iron source, silicon source and lithium source to prepare Li2FeSiO4 positive electrode material, not only the raw material cost is high, but also the conductivity of the prepared Li2FeSiO4 is low. The present invention takes into account that the comprehensive utilization technology of iron tailings is currently mainly concentrated in building materials, ceramics and refractory materials, although it has been put into practical use, the product added value is not high. In order to solve the comprehensive utilization of iron tailings, the present invention takes into account that the iron tailings are mainly composed of SiO2 and Fe2O3, which are not only rich in a large amount of iron elements, but also contain rich silicon sources. In order to realize the resource utilization of iron tailings, the present invention uses iron tailings as the iron source and silicon source for preparing Li2FeSiO4. However, since there are other elements in the iron tailings, in order to effectively realize the efficient utilization of the iron source and silicon source in the iron tailings, the present invention pre-treats the iron tailings to prepare for extracting the iron source and silicon source in the iron tailings respectively, so as to prepare the positive electrode material of lithium ion batteries based on Li2FeSiO4 using the iron source and silicon source therein. The lithium ion battery positive electrode material of the present invention is specifically prepared by the following steps:
[0007] Step 1, pretreatment of iron tailings: using the iron tailings as the iron source and silicon source, subjecting them to acid leaching in an inorganic acid solution to obtain a mixed inorganic acid solution, and performing solid-liquid separation to obtain filter residue and filtrate.
[0008] It should be noted that in order to separate the iron source and the silicon source in the iron tailings so as to facilitate the subsequent preparation of Li2FeSiO4-based lithium-ion battery positive electrode materials, the present invention takes into account that the silicon source mainly exists in the iron tailings in the form of silicon dioxide, and silicon dioxide is insoluble in water and general inorganic acids, while the iron source in the iron tailings can be dissolved in general inorganic acids. Therefore, in some preferred embodiments of the present invention, the iron tailings are pretreated by acid leaching so that the iron source in the iron tailings can be dissolved in the inorganic acid solution, while silicon dioxide is insoluble in the inorganic acid solution, so that the filter residue and the filtrate can be obtained by solid-liquid separation, wherein the filter residue is a precursor of the silicon source and the filtrate is a precursor of the iron source.
[0009] In order to promote the full contact between the inorganic acid solution and the iron tailings, in some preferred embodiments of the present invention, before immersing the iron tailings in the inorganic acid solution, the iron tailings are first immersed in water to wet the iron tailings with water. And in order to ensure that the amount of water used can fully wet the iron tailings, in other preferred embodiments of the present invention, the ratio of water to iron tailings is 8mL to 12mL:10g.
[0010] In order to ensure that the inorganic acid solution used can fully dissolve the iron source in the iron tailings, in some preferred embodiments of the present invention, since ferrous sulfate has a low solubility and is easy to evaporate and crystallize, the inorganic acid solution used is sulfuric acid. And in order to further ensure that the amount of inorganic acid solution used can fully dissolve the iron source in the iron tailings, in some preferred embodiments of the present invention, the mass concentration of sulfuric acid in the inorganic acid solution is 40% to 50%; the dosage ratio of the inorganic acid solution to the iron tailings is 35mL to 50mL:10g.
[0011] In order to further ensure that the iron source in the iron tailings can be fully dissolved in the inorganic acid solution by acid leaching, in some preferred embodiments of the present invention, the temperature of the acid leaching treatment is 95° C. to 105° C. And in order to further ensure that the iron source in the iron tailings can be fully dissolved in the inorganic acid solution by acid leaching treatment in this temperature range, in some preferred embodiments of the present invention, the temperature of the acid leaching treatment is 2 to 3 hours.
[0012] Step 2: Purification of the iron source in the filtrate:
[0013] The filtrate is subjected to reduction treatment to reduce the iron in the filtrate to Fe 2+ , obtain Fe 2+ Solution; for Fe 2+ The solution is heated to make Fe 2+ The anion crystals provided by the inorganic acid solution are precipitated to obtain Fe 2+ of crystal salt.
[0014] It should be noted that the present invention takes into account Fe 3+ The presence of Fe in the filtrate can easily generate LiFeSiO4, thereby reducing the specific capacity of the sample. 3+ or avoid Fe 2+ Oxidized to Fe 3+ Therefore, the present invention also performs a reduction treatment on the filtrate to ensure that the iron in the filtrate is in the form of Fe 2+ exists in the form of.
[0015] In order to ensure that the iron in the filtrate can be reduced to Fe 2+ In some preferred embodiments of the present invention, the reducing agent is added to the filtrate and then subjected to heat treatment to allow the reducing agent to fully react with the filtrate to reduce the iron in the filtrate to Fe 2+ , obtain Fe 2+ In some preferred embodiments of the present invention, the reducing agent used is iron powder or machined iron chips. If iron chips are used, they need to be alkali washed and degreased in advance. In order to ensure that the reducing agent used can make the iron in the filtrate all Fe 2+In some preferred embodiments of the present invention, the reducing agent and the filtrate are used in a ratio of 3g:35mL~50mL.
[0016] The present invention is to facilitate the use of the above-mentioned Fe-containing 2+ Fe in solution 2+ As the iron source is used for the subsequent preparation of Li2FeSiO4, the present invention also obtains Fe-containing 2+ The solution was heated to make the Fe 2+ Fe in solution 2+ Together with the anions provided by the inorganic acid, they are crystallized in the form of inorganic salts to obtain pure Fe 2+ In some preferred embodiments of the present invention, when sulfuric acid is used as the inorganic acid solution, the Fe 2+ The solution mainly contains Fe 2+ and sulfuric acid provide sulfate ions. During the heating process, Fe 2+ The sulfate ions provided by sulfuric acid are crystallized in the form of FeSO4 to obtain pure FeSO4.
[0017] In order to ensure that the Fe 2+ Fe in solution 2+ Together with the anions provided by the inorganic acid, they are crystallized in the form of inorganic salts to obtain pure Fe 2+ In some preferred embodiments of the present invention, the temperature of the heating treatment is 45° C. to 55° C. In some preferred embodiments of the present invention, the time of the heating treatment is 1 h to 3 h.
[0018] Step three, purification of silicon source in the filter residue: disperse the filter residue in alkaline solution to obtain a suspension; heat the suspension, cool it to room temperature and filter it to obtain a liquid component; add polyethylene glycol 400 to the liquid component and mix well, adjust the solution pH to 2.5-3.5 and then age it, filter it and dry it to obtain nano-silica.
[0019] It should be noted that the present invention takes into account that although silicon dioxide is insoluble in general inorganic salts, it can be dissolved in alkali solution. Therefore, in some preferred embodiments of the present invention, the filter residue is dispersed in alkali solution so that the silicon dioxide in the filter residue can be dissolved in the alkali solution. In order to ensure that the alkali solution used can fully dissolve the silicon dioxide in the filter residue, in some preferred embodiments of the present invention, the alkali solution is a NaOH solution. And in order to ensure that the concentration of the NaOH solution used can fully and efficiently dissolve the silicon dioxide in the filter residue, in some preferred embodiments of the present invention, the NaOH solution is prepared by mixing NaOH and water in a dosage ratio of 10g:35mL~45mL; and the dosage ratio of NaOH to the filter residue in the NaOH solution is 10:3~7.
[0020] In another preferred embodiment of the present invention, the filter residue is slowly added into the alkali solution and stirred at a rate of 400 r / min to 600 r / min for 5 min to 15 min, so that the filter residue is fully dispersed in the alkali solution.
[0021] In some preferred embodiments of the present invention, the obtained suspension is also subjected to heat treatment to achieve a high leaching rate of silicon dioxide by heating treatment in a polytetrafluoroethylene-lined reactor. In order to ensure that the leaching rate of silicon dioxide can be improved by heating treatment, in some preferred embodiments of the present invention, the heating temperature when the suspension is heated is 230°C to 270°C, and the heating time is 1h to 3h.
[0022] The present invention takes into account that in addition to the filtrate containing the target product, there is also a filter residue in the reaction liquid obtained after the above-mentioned heating reaction. Therefore, the present invention performs solid-liquid separation on the reaction liquid obtained after the heating reaction and then washes it to remove the filter residue and residual alkali solution. In some preferred embodiments of the present invention, a polytetrafluoroethylene filter membrane is used for solid-liquid separation by suction filtration, and water is used for washing.
[0023] In order to obtain white carbon black nanoparticles with good dispersibility and small particle size, in a preferred embodiment of the present invention, polyethylene glycol 400 is used as a dispersant and added to the liquid component obtained above, so as to achieve the dispersion of silicic acid in the subsequent sedimentation process through polyethylene glycol 400. In order to avoid the loss of water during the mixing process of polyethylene glycol 400 and the liquid component, polyethylene glycol 400 is added to the liquid component obtained above and then sealed, and then the mixed solution is stirred to make it fully mixed. Among them, in a preferred embodiment of the present invention, the mass ratio of polyethylene glycol 400 to the filter residue is 0.3-0.7:5.
[0024] In a preferred embodiment of the present invention, the mixture is first stirred at a stirring rate of 400 r / min to 600 r / min until uniformly mixed, for example, for 5 min to 15 min, and then the acid solution is slowly added at a stirring rate of 500 r / min to 700 r / min to adjust the pH of the solution system to 2.5 to 3.5 to achieve the purpose of sedimentation. In a preferred embodiment of the present invention, when adjusting the pH of the solution system, the acid solution used is the same as the inorganic acid solution used for acid leaching to avoid introducing other inorganic anions. After adjusting the pH of the solution system to 2.5 to 3.5, an aging treatment is performed to completely precipitate the silicic acid through the aging treatment. In a preferred embodiment of the present invention, the aging treatment temperature is 50 to 70 ° C and the time is 1 h to 3 h.
[0025] It can be understood that since the aging treatment is carried out in a solution environment, the obtained nano-silica is also present in the solution environment. In order to facilitate the use of nano-silica as a silicon source for the subsequent preparation of Li2FeSiO4, the present invention also performs solid-liquid separation on the reaction solution obtained after the aging treatment, such as suction filtration, and the obtained solid component is dried to obtain nano-silica. Among them, in some preferred embodiments of the present invention, the drying is carried out by vacuum drying treatment, and the drying temperature is 70°C to 90°C, and the time is 8h to 12h.
[0026] Step 4: Preparation of Li2FeSiO4: 2+ Li2FeSiO4 was prepared by a hydrothermal method using crystalline salt as the iron source, nano-white carbon black as the silicon source, lithium hydroxide as the lithium source, and water as the solvent.
[0027] It should be noted that, in order to ensure that the Li2FeSiO4 with small particle size, butterfly shape, uniform particle size distribution and high purity can be obtained through hydrothermal reaction, in some preferred embodiments of the present invention, the following steps are specifically implemented: lithium hydroxide and nano-white carbon black are mixed in water to obtain a first mixed solution; 2+ The crystalline salt is dispersed in an ethylene glycol aqueous solution to obtain a second mixed solution; under an Ar gas atmosphere, the first mixed solution is dropped into the second mixed solution and mixed to obtain a third mixed solution; the third mixed solution is subjected to a hydrothermal reaction and then solid-liquid separation to obtain a solid component; and the solid component is dried to obtain Li2FeSiO4.
[0028] It should be noted that the present invention takes into account the uniformity of the components of the final product. In some preferred embodiments of the present invention, lithium hydroxide is first dispersed in water to form a lithium hydroxide solution; then nano-silica is added to ensure that the lithium hydroxide and the nano-silica are fully mixed to form lithium silicate, and then mixed with the Fe 2+ The crystallization salts are mixed to achieve lithium silicate and Fe 2+ Evenly mixed to facilitate the subsequent formation of Li2FeSiO4. In order to ensure that nano-white carbon black and lithium hydroxide fully form lithium silicate, in some preferred embodiments of the present invention, the amount ratio of lithium hydroxide, nano-white carbon black and water is 1.2g-1.5g:0.72g:12.8mL.
[0029] In some preferred embodiments of the present invention, the dispersion is carried out by stirring, and the stirring rate is 200r / min to 400r / min, and the stirring is carried out until the lithium hydroxide is completely dissolved. In order to ensure that the nano-white carbon black can be fully dispersed in the lithium hydroxide solution, in some preferred embodiments of the present invention, the dispersion is carried out by heating and stirring, and the stirring temperature is 35°C to 45°C, the stirring rate is 200r / min to 400r / min, and the stirring is carried out until the white carbon black is completely dissolved, so as to ensure that lithium silicate is fully formed and there is no residual solid phase white carbon black.
[0030] In order to ensure that the Fe 2+ The crystal salt can be evenly dispersed in the ethylene glycol aqueous solution. In some preferred embodiments of the present invention, the dispersion is carried out by stirring, and the stirring temperature is 35°C to 45°C, the stirring rate is 200r / min to 400r / min, and the stirring time is 10min to 30min. In order to ensure that the ethylene glycol aqueous solution can fully disperse the Fe 2+ In some preferred embodiments of the present invention, the crystalline salt contains Fe 2+ The usage ratio of the crystalline salt to the ethylene glycol aqueous solution is 2.5 g:11.3 mL-15.3 mL, and the ethylene glycol aqueous solution is prepared by mixing water and ethylene glycol in a volume ratio of 3.8:7.5-8.0.
[0031] In some preferred embodiments of the present invention, the first mixed liquid and the second mixed liquid are mixed in an Ar atmosphere to avoid air entering during the stirring process and causing Fe 2+ Oxidized.
[0032] In order to ensure that the third mixed solution can form Li2FeSiO4 during the hydrothermal reaction, in some preferred embodiments of the present invention, Fe 2+ The molar ratio of the crystalline salt, nano-white carbon black and lithium hydroxide is 1:1:3. In order to ensure that Li2FeSiO4 can be fully formed through the hydrothermal reaction, in some preferred embodiments of the present invention, the temperature of the hydrothermal reaction is 180°C to 260°C and the time is 6h to 36h.
[0033] The present invention takes into account that the above hydrothermal reaction is carried out in a solution environment, so the present invention also performs solid-liquid separation treatment on it to obtain a solid component. In some preferred embodiments of the present invention, solid-liquid separation is preferably performed by centrifugation, first by transferring the reaction solution into a centrifuge tube, adding distilled water for stirring, and then centrifuging at a rate of 4000r / min to 6000r / min for 2min to 5min; after pouring out the supernatant, add anhydrous ethanol for stirring, and then centrifuge at a rate of 4000r / min to 6000r / min for 2min to 5min, and continue to repeat this operation twice to obtain a clean solid component. In order to remove the solvent that may remain on the surface of the solid component, in some preferred embodiments of the present invention, vacuum drying is used for drying, and the drying temperature is 70℃ to 90℃, and the drying time is 8h to 12h.
[0034] In some preferred embodiments of the present invention, the present invention also uses Li2FeSiO4 as a matrix, and a carbon layer is coated on its surface to modify the surface of Li2FeSiO4. The carbon layer has a higher conductivity and can be used as a conductive medium, thereby improving the conductivity of Li2FeSiO4. However, the present invention takes into account that the introduction of carbon elements will lead to a decrease in its specific capacity. Therefore, in order to ensure that the electrochemical performance of Li2FeSiO4 can be improved while improving the conductivity of Li2FeSiO4, in some preferred embodiments of the present invention, the carbon layer is coated on the surface of Li2FeSiO4 through the following steps:
[0035] Sucrose and Li2FeSiO4 are mixed in water to obtain a fourth mixed solution, which is then subjected to a hydrothermal reaction at 180°C to 220°C, solid-liquid separation, washing, and drying to obtain a precursor. The precursor is sintered in an argon atmosphere to coat the surface of Li2FeSiO4 with carbon to obtain Li2FeSiO4 / C.
[0036] It should be noted that the present invention takes into account the low cost of sucrose, so in some preferred embodiments of the present invention, sucrose is used as a carbon source to achieve carbon composite of Li2FeSiO4 while reducing the preparation cost. In order to ensure that sucrose and Li2FeSiO4 can be fully mixed in water, in some preferred embodiments of the present invention, sucrose is first dispersed in water by stirring to obtain a sucrose solution; then Li2FeSiO4 is uniformly dispersed in the sucrose solution by ultrasound. In some preferred embodiments of the present invention, the frequency of ultrasound is 40KHz, the ultrasonic power is set to 150-200W, and the ultrasonic time is 5min-15min.
[0037] In order to ensure that sucrose and Li2FeSiO4 can fully react in the hydrothermal reaction process in water to obtain a precursor, in some preferred embodiments of the present invention, the mass ratio of Li2FeSiO4 to sucrose is 1:0.1 to 4. In some preferred embodiments of the present invention, the amount ratio of sucrose to water is 0.5g:35mL to 45mL.
[0038] In order to ensure that the sucrose in the fourth mixed liquid can fully contact with Li2FeSiO4 and be fully carbonized through the hydrothermal reaction, in some preferred embodiments of the present invention, the temperature of the hydrothermal reaction of the fourth mixed liquid in a polytetrafluoroethylene-lined reactor is 180°C to 220°C, and the time is 6h to 18h.
[0039] In order to obtain a solid precursor, in some preferred embodiments of the present invention, the reaction liquid of the hydrothermal reaction is preferably separated into solid and liquid by centrifugation, and the centrifugal rate is 5000r / min, and the centrifugal time is 5 to 15min. Then, the obtained solid component is washed three times with water and anhydrous ethanol respectively to remove impurities and then dried to remove excess solvent. In some preferred embodiments of the present invention, the drying is carried out by vacuum drying treatment, and the drying temperature is 70°C to 90°C, and the drying time is 8h to 12h.
[0040] Considering that the crystallinity of the precursor obtained above is low, the present invention also performs a sintering treatment on the precursor, so that the Li2FeSiO4 and carbon in the precursor are completely crystallized during the sintering treatment process, and a composite material composed of Li2FeSiO4 and a carbon layer with a better crystallization effect is obtained. In some preferred embodiments of the present invention, the sintering treatment temperature is 500°C to 600°C, and the sintering time is 1h to 3h.
[0041] In the process of exploring the surface modification of Li2FeSiO4 to improve its conductivity, the present invention found that the particle size of Li2FeSiO4 can affect its ion conductivity. Li2FeSiO4 with a fine particle size can effectively reduce the transmission path of lithium ions in the electrode, increase the contact area with the electrolyte, and make the positive electrode material Li2FeSiO4 have better rate performance. Therefore, the present invention attempts to control the particle size of Li2FeSiO4 while modifying the surface of Li2FeSiO4.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The present invention mainly aims at the utilization of iron tailings resources, takes iron tailings as the main raw material, makes full use of the iron and silicon elements in the iron tailings, and provides a new method for preparing lithium iron silicate / carbon composite lithium ion battery positive electrode material. The method is suitable for actual production and has important significance for the comprehensive development and utilization of iron tailings, environmental protection, and the development of the preparation technology of high-performance lithium ion battery positive electrode materials.
[0044] The present invention uses high-silicon iron tailings as the main raw materials, prepares FeSO4 and SiO2 precursors, and obtains Li2FeSiO4 and Li2FeSiO4 / C lithium-ion battery positive electrode materials by solvent thermal, effectively utilizing a variety of valuable elements in the iron tailings, and providing a new economical and efficient path for the comprehensive utilization of iron tailings resources and increasing the added value of products. The lithium-ion battery positive electrode material based on iron tailings prepared by the present invention has good cycle stability and good rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is the XRD pattern of silicon dioxide, Figure 1 In the figure, Figure a is the XRD spectrum of commercially available analytical pure SiO2 chemical reagent, and Figure b is the XRD spectrum of white carbon black prepared in Example 1.
[0046] Figure 2 is a scanning electron microscope image of the white carbon black prepared in Example 1, Figure 2 In the figure, Figure a is a scanning electron microscope image at a 10 μm scale, and Figure b is a scanning electron microscope image at a 2 μm scale.
[0047] Figure 3 This is the thermogravimetric-differential thermal analysis curve of the white carbon black prepared in Example 1.
[0048] Figure 4 The XRD spectra of Example 1 and Comparative Examples 4 to 7 are shown.
[0049] Figure 5 These are the XRD spectra of Example 1, and Example 6-Example 8.
[0050] Figure 6 The following are the XRD spectra of Example 1 and Example 2-Example 5.
[0051] Figure 7 is the scanning electron microscope image of Example 1, Figure 7 In the figure, Figure a is a scanning electron microscope image of Example 1 at a scale of 2 μm, and Figure b is a scanning electron microscope image of Example 1 at a scale of 1 μm.
[0052] Figure 8 The scanning electron microscope images of Example 11 and Comparative Examples 1 to 3 are shown in FIG. Figure 8 In the figure, Figure a is a scanning electron microscope image of comparative example 2 at a 2 μm scale, and Figure b is a scanning electron microscope image of comparative example 2 at a 10 μm scale; Figure c is a scanning electron microscope image of comparative example 3 at a 2 μm scale, and Figure d is a scanning electron microscope image of comparative example 3 at a 10 μm scale; Figure e is a scanning electron microscope image of embodiment 11 at a 2 μm scale, and Figure f is a scanning electron microscope image of embodiment 11 at a 10 μm scale; Figure g is a scanning electron microscope image of comparative example 1 at a 2 μm scale, and Figure h is a scanning electron microscope image of comparative example 1 at a 10 μm scale.
[0053] Fig. 9 These are the XRD spectra of Example 1, and Example 9 to Example 14.
[0054] Fig.10 The XRD spectra of Example 11 and Comparative Examples 1 to 3 are shown.
[0055] Fig.11 The charge and discharge curves of Examples 9 to 13 at a current density of 0.1C; Fig.11 In the figure, Figure a is a charge and discharge curve diagram of Example 9, Figure b is a charge and discharge curve diagram of Example 10, Figure c is a charge and discharge curve diagram of Example 11, Figure d is a charge and discharge curve diagram of Example 12, and Figure e is a charge and discharge curve diagram of Example 13.
[0056] Fig.12 The specific capacity and coulombic efficiency of Examples 9 to 13 after 100 cycles at a current density of 0.1C are shown in FIG. Fig.12 , Figure a is a graph showing the change of specific capacity and coulombic efficiency of Example 9, Figure b is a graph showing the change of specific capacity and coulombic efficiency of Example 10, Figure c is a graph showing the change of specific capacity and coulombic efficiency of Example 11, Figure d is a graph showing the change of specific capacity and coulombic efficiency of Example 12, and Figure e is a graph showing the change of specific capacity and coulombic efficiency of Example 13.
[0057] Fig.13 The charge and discharge curves of Example 1, Example 11, Comparative Examples 1 to 3 and Comparative Example 8 at a current density of 0.1C; Fig.13 In the figure, Figure a is the charge and discharge curve of Example 1; Figure b is the charge and discharge curve of Comparative Example 8; Figure c is the charge and discharge curve of Comparative Example 2; Figure d is the charge and discharge curve of Comparative Example 3; Figure e is the charge and discharge curve of Example 11; and Figure f is the charge and discharge curve of Comparative Example 1.
[0058] Fig.14 The cycle performance curves of Example 1, Example 11, Comparative Examples 1 to 3 and Comparative Example 8 at a current density of 0.1C are shown; Fig.14In the figure, Figure a is the cycle performance curve of Example 1; Figure b is the cycle performance curve of Comparative Example 8; Figure c is the cycle performance curve of Comparative Example 2; Figure d is the cycle performance curve of Comparative Example 3; Figure e is the cycle performance curve of Example 11; and Figure f is the cycle performance curve of Comparative Example 1.
[0059] Fig.15 The figure shows the rate performance curves of Example 1, Example 11, Comparative Examples 1 to 3 and Comparative Example 8 at different current densities. Fig.15 In the figure, Figure a is the rate performance curve of Example 1; Figure b is the rate performance curve of Comparative Example 8; Figure c is the rate performance curve of Comparative Example 2; Figure d is the rate performance curve of Comparative Example 3; Figure e is the rate performance curve of Example 11; and Figure f is the rate performance curve of Comparative Example 1. DETAILED DESCRIPTION
[0060] The technical solutions in the embodiments of the present invention are described clearly and completely below. It should be noted that the raw materials used in the following embodiments of the present invention are all directly purchased commercial reagents. Among them, the pure iron powder, Super-P, electrolyte, diaphragm Celgard-2500 and lithium metal sheet used are all purchased from Kelude Experimental Equipment Technology Co., Ltd.
[0061] Example 1
[0062] This embodiment provides a lithium ion battery positive electrode material based on iron tailings, and the positive electrode material is prepared by the following steps:
[0063] 1) Take 10 g of iron tailings, add 10 mL of distilled water and mix well, then add 40 mL of sulfuric acid and mix well, then heat in an oil bath at 100 °C for 2.5 h to obtain a mixed inorganic acid solution, filter and obtain a residue and a filtrate.
[0064] 2) Add 3 g of iron powder and 20 mL of distilled water to the filtrate, and then heat in a water bath at 50° C. for 2 h to obtain a FeSO4 solution. Under an argon atmosphere, heat the FeSO4 solution in a water bath at 80° C. for 3 h to obtain FeSO4.
[0065] 3) Mix 10.00g NaOH and 40mL distilled water at a rate of 500r / min to obtain a NaOH solution. Add 5.00g of the above-mentioned filter residue to the NaOH solution, stir at a rate of 500r / min for 10min to obtain a suspension. Transfer the suspension to the lining of the reactor, keep it at 250℃ for 2h, cool it to room temperature, filter it with a polytetrafluoroethylene filter membrane, add 10mL distilled water to rinse it again, and obtain a liquid component. Add 0.50g of polyethylene glycol 400 to the liquid component, seal it with plastic wrap, stir it at a rate of 500r / min for 10min in a 70℃ water bath, then adjust the solution system to pH 3 by slowly dripping sulfuric acid solution at a rate of 600r / min while stirring, and then age it at 50-70℃ for 2h. Filter it with suction, and vacuum dry the solid component at 80℃ for 10h to obtain nano-white carbon black.
[0066] 4) Mix 1.2g of lithium hydroxide and 12.8mL of deionized water at a rate of 300r / min to obtain a lithium hydroxide solution. Add 0.72g of nano-white carbon black to the above lithium hydroxide solution, stir at 300r / min at 40°C until dissolved, and obtain a first mixed solution, marked as L1. After mixing 3.8mL of deionized water and 7.5mL of ethylene glycol, add 2.5g of the above FeSO4, stir at 300r / min at 40°C for 20min, and obtain a second mixed solution, marked as L2. While continuously passing Ar gas, drop L1 into L2 and mix to obtain a third mixed solution. Quickly transfer the third mixed solution to the lining of the reactor, hydrothermally react at 240°C for 24h to obtain a reaction solution. The reaction solution was transferred into a centrifuge tube, distilled water was added for stirring, and the mixture was centrifuged at 5000 r / min for 3 min. The upper layer of liquid was removed and poured out, anhydrous ethanol was added for stirring, and the mixture was centrifuged at 5000 r / min for 3 min again. This operation was repeated twice. After centrifugation, the mixture was placed in a vacuum drying oven at 80°C for 12 h to obtain Li2FeSiO4.
[0067] Example 2
[0068] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction temperature of the third mixed liquid is 180°C.
[0069] Example 3
[0070] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction temperature of the third mixed liquid is 200°C.
[0071] Example 4
[0072] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction temperature of the third mixed liquid is 220°C.
[0073] Example 5
[0074] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction temperature of the third mixed liquid is 260°C.
[0075] Example 6
[0076] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction time of the third mixed solution is 6 hours.
[0077] Example 7
[0078] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction time of the third mixed solution is 12 hours.
[0079] Example 8
[0080] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this embodiment and embodiment 1 is only that: in this embodiment, the hydrothermal reaction time of the third mixed solution is 36 hours.
[0081] Example 9
[0082] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and this embodiment is different from Embodiment 1 only in that:
[0083] In this embodiment, sucrose is subjected to hydrothermal reaction and sintering treatment in sequence, and a carbon layer is coated on the surface of Li2FeSiO4, that is, the following two steps are further performed on the basis of Example 1:
[0084] 5) 0.05 g of sucrose was added to 40 mL of distilled water and stirred to dissolve to obtain a sucrose solution. 0.5 g of Li2FeSiO4 from Example 1 was added to the sucrose solution and ultrasonically dissolved for 10 min, followed by hydrothermal reaction at 200° C. for 12 h, centrifuged and washed, and dried at 80° C. for 12 h to obtain a precursor.
[0085] 6) The precursor was heated to 550° C. at a heating rate of 10° C. / min, sintered at 550° C. for 2 h in an Ar atmosphere, and naturally cooled to room temperature to obtain a positive electrode material for a lithium-ion battery.
[0086] In this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:0.1.
[0087] Example 10
[0088] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this embodiment and Example 9 is that in this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:0.5.
[0089] Embodiment 11
[0090] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this embodiment and Embodiment 9 is that in this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:1.
[0091] Example 12
[0092] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this embodiment and Embodiment 9 is that in this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:2.
[0093] Example 13
[0094] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this embodiment and Example 9 is that in this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:3.
[0095] Embodiment 14
[0096] This embodiment provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this embodiment and Example 9 is that in this embodiment, the mass ratio of Li2FeSiO4 to sucrose is 1:4.
[0097] Comparative Example 1
[0098] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and in this comparative example, steps 1) to 3) are the same as those in Example 11, so they are not described again, please refer to Example 11. The only difference from Example 11 is:
[0099] 4) Mix 1.2g lithium hydroxide and 12.8mL deionized water at a rate of 300r / min to obtain a lithium hydroxide solution. Add 0.72g nano-white carbon black to the above lithium hydroxide solution, stir magnetically at 300r / min at 40°C until dissolved, and obtain a mixed solution, marked as L3. Mix 3.8mL deionized water and 7.5mL ethylene glycol, then add 0.5g sucrose and stir until completely dissolved; then add 2.5g FeSO4 prepared in step 2 above, stir magnetically at 500r / min at 40°C for 20min, and obtain a mixed solution, marked as L4. While continuously passing Ar gas, drop L3 into L4, mix well, quickly transfer the mixed solution to the lining of the reactor, put it into a blast constant temperature drying oven, react at 240°C for 24h, and obtain a reaction solution. The reaction solution was transferred into a centrifuge tube, distilled water was added for stirring, and the mixture was centrifuged at 5000 r / min for 3 min. The upper layer of liquid was removed and poured out, anhydrous ethanol was added for stirring, and the mixture was centrifuged at 5000 r / min for 3 min again. This operation was repeated twice. After centrifugation, the centrifuge tube was placed in a vacuum drying oven and dried at 80°C for 12 h to obtain carbon-coated Li2FeSiO4, i.e., the precursor.
[0100] 5) The precursor was heated to 550°C at a heating rate of 10°C / min, sintered at 550°C for 2h in an Ar atmosphere, and naturally cooled to room temperature to obtain Li2FeSiO4 / C.
[0101] That is, the difference between this comparative example and Example 11 is only that:
[0102] In this comparative example, sucrose is added during the preparation of Li2FeSiO4 to form carbon during the hydrothermal and calcination processes, that is, sucrose, lithium hydroxide, white carbon black and FeSO4 are prepared as a precursor by a hydrothermal method, and then calcined to obtain Li2FeSiO4 / C.
[0103] Comparative Example 2
[0104] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this comparative example and Example 11 is that this comparative example does not undergo calcination treatment.
[0105] Comparative Example 3
[0106] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the only difference between this comparative example and comparative example 1 is that this comparative example does not undergo calcination treatment.
[0107] Comparative Example 4
[0108] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this comparative example and Example 1 is only that the amount of LiOH used in this comparative example is 18.76 mmol, i.e., 0.8 g.
[0109] Comparative Example 5
[0110] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this comparative example and Example 1 is only that the amount of LiOH used in this comparative example is twice that of 18.76 mmol, that is, 1.6 g.
[0111] Comparative Example 6
[0112] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this comparative example and Example 1 is only that:
[0113] The amount of LiOH used in this comparative example is 2.5 times of 18.76 mmol, i.e. 2.0 g.
[0114] Comparative Example 7
[0115] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this comparative example and Example 1 is only that:
[0116] The amount of LiOH used in this comparative example is 4 times of 18.76 mmol, i.e. 3.2 g.
[0117] Comparative Example 8
[0118] This comparative example provides a lithium-ion battery positive electrode material based on iron tailings, and the difference between this comparative example and Example 1 is only that:
[0119] In this comparative example, the Li2FeSiO4 obtained in Example 1 was further subjected to hydrothermal reaction in water at 240°C for 24 hours to obtain Li2FeSiO4 that had undergone a secondary hydrothermal reaction.
[0120] Experimental Section
[0121] (I) Structural analysis of white carbon black
[0122] 1) X-ray diffraction test
[0123] In order to verify that white carbon black is an amorphous structure, the present invention conducted X-ray diffraction tests on the white carbon black prepared in Example 1 and the commercially available analytically pure SiO2 chemical reagent, and the test results are as follows: Figure 1 shown.
[0124] Figure 1 is the XRD pattern of silicon dioxide, Figure 1In the figure, Figure a is the XRD spectrum of the commercially available analytical pure SiO2 chemical reagent, and Figure b is the XRD spectrum of the white carbon black prepared in Example 1. It can be seen that the XRD spectrum of pure SiO2 and the white carbon black prepared in Example 1 is inconsistent. There is no sharp crystal diffraction peak in the XRD spectrum of the white carbon black prepared in Example 1, and only one amorphous diffraction peak appears in the low diffraction angle region of about 25°, and no other crystalline phase is contained, indicating that the white carbon black prepared in Example 1 is an amorphous non-crystalline structure. Although white carbon black and silicon dioxide are both materials composed of silicon dioxide, there are some significant differences in their structure, properties and applications.
[0125] 2) Scanning electron microscopy analysis
[0126] The present invention takes the white carbon black prepared in Example 1 as an example, and performs a scanning electron microscope test on it, and the test results are as follows: Figure 2 shown. Figure 2 is a scanning electron microscope image of the white carbon black prepared in Example 1, Figure 2 In the figure, Figure a is a scanning electron microscope image of the white carbon black prepared in Example 1 at a scale of 10 μm, and Figure b is a scanning electron microscope image of the white carbon black prepared in Example 1 at a scale of 2 μm.
[0127] Depend on Figure 2 As can be seen from Figure a in the figure, the overall shape of the white carbon black prepared in Example 1 is irregular block, and the primary particles are obviously agglomerated. Figure 2 As can be seen from Figure b, the silica particles are approximately spherical, with a particle size of less than 1 μm. Some particles are aggregated, and the microstructure of some secondary particles is a flocculent and network-like quasi-particle structure.
[0128] 3) Thermogravimetric-differential thermal analysis
[0129] The present invention takes the white carbon black prepared in Example 1 as an example, and performs thermogravimetric-differential thermal analysis on it, and the test range is from 25°C to 800°C, the heating rate is 15°C per minute, and a nitrogen-oxygen mixed atmosphere is used to determine the crystal water content of the white carbon black by thermogravimetric-differential thermal analysis. And the test results are as follows Figure 3 shown.
[0130] Figure 3 The thermogravimetric-differential thermal analysis curve of the white carbon black prepared in Example 1 shows that the weight loss of the white carbon black prepared in Example 1 is mainly divided into two stages. The weight loss rate of the white carbon black in the first stage at 0°C to 260°C is 16.70%, and the main loss is the attached water; the weight loss rate in the second stage at 260°C to 800°C is 22.44%, and the main loss is the crystallization water; and after 720°C, the weight loss of the white carbon black becomes slow, so the crystallization water content of the white carbon black is 22.44%.
[0131] (II) Analysis of factors affecting the structure of Li2FeSiO4
[0132] 1) Effect of LiOH dosage on prepared Li2FeSiO4
[0133] The present invention takes Li2FeSiO4 prepared in Example 1 and Comparative Examples 4 to 7 as examples, and performs XRD tests on them respectively, and the test results are as follows: Figure 4 shown.
[0134] Depend on Figure 4 It can be seen that by comparing the diffraction peaks in the standard Li2FeSiO4 card PDF#01-080-7252, when the amount of LiOH is too much or too little, the phase of its XRD spectrum changes, which is not conducive to obtaining pure phase Li2FeSiO4. Therefore, the present invention preferably contains Fe 2+ The mass ratio of the crystalline salt, nano-white carbon black and lithium hydroxide is 2.5g:0.72:1.2.
[0135] 2) Effect of hydrothermal reaction temperature on the preparation of Li2FeSiO4
[0136] The present invention takes Li2FeSiO4 prepared in Example 1 and Example 2-Example 5 as examples, and performs XRD tests on them respectively, and the test results are as follows Figure 5 shown.
[0137] Depend on Figure 5 It can be seen that by comparing with the diffraction peaks in the standard Li2FeSiO4 card PDF#01-080-7252, the diffraction peaks of the standard Li2FeSiO4 can be observed in the XRD spectrum of Li2FeSiO4 obtained at a hydrothermal reaction temperature of 180°C to 260°C, indicating that Li2FeSiO4 can be obtained at a hydrothermal reaction temperature of 180°C to 260°C. However, in the XRD spectrum of Li2FeSiO4 obtained at a hydrothermal reaction temperature of 180°C to 220°C, obvious miscellaneous peaks also appear, so the present invention preferably sets the hydrothermal reaction temperature to 220°C to 260°C. The most preferred temperature is 240°C.
[0138] 3) Effect of hydrothermal reaction time on the preparation of Li2FeSiO4
[0139] The present invention takes Example 1 and Example 6-Example 8 as examples, and performs XRD tests on them respectively, and the test results are as follows Figure 6 shown.
[0140] Depend on Figure 6It can be seen that by comparing with the diffraction peaks in the standard Li2FeSiO4 card PDF#01-080-7252, the diffraction peaks of the standard Li2FeSiO4 can be observed in the XRD spectra of Li2FeSiO4 obtained in Example 1 and Example 6-Example 8, indicating that Li2FeSiO4 can be obtained at a hydrothermal reaction time of 6h to 36h. However, in the XRD spectrum of Li2FeSiO4 obtained at a hydrothermal reaction time of 6h, obvious miscellaneous peaks also appear, so the present invention preferably sets the hydrothermal reaction temperature to 12h to 36h. The most preferred temperature is 24h.
[0141] 4) Scanning electron microscopy analysis
[0142] The present invention takes Li2FeSiO4 prepared in Example 1 as an example, and performs scanning electron microscope tests on it, and the test results are as follows: Figure 7 shown. Figure 7 is the scanning electron microscope image of Example 1, Figure 7 In the figure, Figure a is a scanning electron microscope image of Li2FeSiO4 prepared in Example 1 at a scale of 2 μm, and Figure b is a scanning electron microscope image of Li2FeSiO4 prepared in Example 1 at a scale of 1 μm.
[0143] Depend on Figure 7 It can be seen that the particles of Example 1 are spherical and have a relatively uniform particle size distribution.
[0144] (II) Analysis of factors affecting the structure of Li2FeSiO4 / C
[0145] 1) Effect of carbon layer formation on Li2FeSiO4 / C
[0146] The present invention respectively carried out scanning electron microscope test on Example 11 and Comparative Examples 1-3, and the test results are as follows Figure 8 shown. Figure 8 In the figure, Figure a is a scanning electron microscope image of comparative example 2 at a 2 μm scale, and Figure b is a scanning electron microscope image of comparative example 2 at a 10 μm scale; Figure c is a scanning electron microscope image of comparative example 3 at a 2 μm scale, and Figure d is a scanning electron microscope image of comparative example 3 at a 10 μm scale; Figure e is a scanning electron microscope image of embodiment 11 at a 2 μm scale, and Figure f is a scanning electron microscope image of embodiment 11 at a 10 μm scale; Figure g is a scanning electron microscope image of comparative example 1 at a 2 μm scale, and Figure h is a scanning electron microscope image of comparative example 1 at a 10 μm scale.
[0147] By comparison Figure 8 It can be seen from the various figures that the morphology and particle size of Li2FeSiO4 / C have not changed significantly, so changing the order of adding sucrose and whether or not to calcine has little effect on the morphology of the product.
[0148] 2) Effect of sucrose dosage on the morphology of Li2FeSiO4 / C
[0149] The present invention has carried out XRD test on embodiment 1 and embodiment 9-embodiment 14 respectively, and the test results are as follows Fig. 9 shown.
[0150] Depend on Fig. 9 It can be seen that with the increase of sucrose concentration, the diffraction peak of Li2FeSiO4 at 28° gradually disappears. Since the diffraction peak of Li2FeSiO4 / C sample shows amorphous characteristics, the coated carbon obtained after sucrose carbonization is amorphous.
[0151] 3) Effects of sucrose addition sequence and sintering treatment on the phase structure of Li2FeSiO4 / C
[0152] The present invention respectively carried out XRD test on Example 11 and Comparative Examples 1-3, and the test results are as follows Fig.10 shown.
[0153] Depend on Fig.10 It can be seen that a sharp diffraction peak can be observed in the XRD spectrum of Comparative Example 2, but the diffraction peak of Comparative Example 1 does not match the Li2FeSiO4 standard PDF card. At this time, the phase composition is mainly LiFeSi2O6, indicating that part of the divalent iron is oxidized during the calcination process. While Example 11 and Comparative Example 3 show the characteristics of amorphous diffraction peaks. This shows that adding sucrose first is not conducive to obtaining amorphous Li2FeSiO4 / C.
[0154] (IV) Electrochemical performance test
[0155] The electrochemical performance test uses a half-cell, with a metal lithium sheet as the counter electrode, a Celgard 2500 separator, and an electrolyte of 1.0 mol / L LiPF6 of a mixture of ethylene carbonate and diethyl carbonate, wherein the volume ratio of ethylene carbonate to diethyl carbonate is 1:1, the binder is polyvinylidene fluoride, and the conductive agent is Super-P. The slurry is prepared according to the mass ratio of active material: Super-P: PVDF = 8:1:1. By assembling button cells, the prepared Li2FeSiO4 / C powder is used as the positive electrode, and the lithium sheet is used as the counter electrode to assemble a half-cell. The electrochemical properties of the prepared different powder materials are analyzed by testing the charge and discharge curves, rate performance, and cycle performance. The CT-4008T battery test system produced by Shenzhen Xinwei Electronics Co., Ltd. is used to simulate the half-cell for electrochemical performance testing, which can intuitively evaluate the electrochemical performance of the Li2FeSiO4 / C material; the voltage range is set to 1.5V~4.6V, and the current density is set to 0.05A·g -1 ~1A·g -1.
[0156] 1) Effect of sucrose dosage on charge and discharge performance of Li2FeSiO4 / C
[0157] The present invention has carried out the charge and discharge performance test on embodiment 9-embodiment 13 respectively, and the test results are as follows Fig.11 shown. Fig.11 The charge and discharge curves of Examples 9 to 13 at a current density of 0.1C.
[0158] Fig.11 In the figure, a is the charge and discharge curve of Example 9, b is the charge and discharge curve of Example 10, c is the charge and discharge curve of Example 11, d is the charge and discharge curve of Example 12, and e is the charge and discharge curve of Example 13. Among them, 0.1C is 33.2mA·g -1 .
[0159] Depend on Fig.11 It can be seen that when the current density is 0.1C, the first discharge specific capacity of Examples 9 to 13 is 125 mAh·g -1 、194mAh·g -1 、171mAh·g -1 、90mAh·g -1 and 43mAh·g -1 After 10 charge and discharge cycles, the specific capacity is 67 mAh g -1 、194mAh·g -1 、101mAh·g -1 、150mAh·g -1 、80mAh·g -1 and 25mAh g -1 The initial discharge capacity of Example 10 was relatively high, but after 10 cycles, the capacity gradually decayed to 101 mAh·g -1 The specific capacity of Example 11 after 10 cycles is the largest, which is 151 mAh g -1 .
[0160] 2) Effect of sucrose dosage on the cycling performance of Li2FeSiO4 / C
[0161] The present invention respectively carried out cycle performance tests on Examples 9 to 13, that is, the specific capacity and coulombic efficiency changes after 100 cycles at a current density of 0.1C were tested, and the test results are as follows: Fig.12 shown. Fig.12, Figure a is a graph showing the change of specific capacity and coulombic efficiency of Example 9, Figure b is a graph showing the change of specific capacity and coulombic efficiency of Example 10, Figure c is a graph showing the change of specific capacity and coulombic efficiency of Example 11, Figure d is a graph showing the change of specific capacity and coulombic efficiency of Example 12, and Figure e is a graph showing the change of specific capacity and coulombic efficiency of Example 13.
[0162] Depend on Fig.12 It can be seen that when the current density is 0.1C, the specific capacity of Examples 9 to 13 is maintained at 46 mAh·g after 100 charge and discharge cycles. -1 、90mAh·g -1 、150mAh·g -1 , 42mAh·g -1 and 10mAh·g -1 After 100 charge-discharge cycles, the specific capacity of Example 11 is the largest, and the charge-discharge efficiency is close to 100%. The specific capacity of Example 11 gradually increases during the first 50 cycles, and then slowly decreases, which may be due to the activation of Li2FeSiO4 during the charge-discharge process.
[0163] 3) Effects of sucrose addition order and sintering treatment on the charge-discharge performance of Li2FeSiO4 / C
[0164] The present invention tests the charge and discharge performance of Example 1, Example 11, Comparative Examples 1 to 3 and Comparative Example 8 at a current density of 0.1C, and the test results are as follows: Fig.13 shown. Fig.13 In the figure, Figure a is the charge and discharge curve of Example 1; Figure b is the charge and discharge curve of Comparative Example 8; Figure c is the charge and discharge curve of Comparative Example 2; Figure d is the charge and discharge curve of Comparative Example 3; Figure e is the charge and discharge curve of Example 11; and Figure f is the charge and discharge curve of Comparative Example 1.
[0165] And by Fig.13 It can be seen that the specific capacity of Comparative Example 8 obtained after the secondary solvent thermal treatment is reduced, indicating that the secondary solvent thermal treatment is not conducive to improving the electrochemical properties of the LFS matrix. The specific capacities of Example 1, Example 11, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 8 are 175 mAh·g -1 、80mAh·g -1 、171mAh·g -1 、49mAh·g -1 、115mAh·g -1 and 95mAh·g -1 Among them, the first discharge specific capacity of Example 1 is the largest. After 10 cycles, the specific capacity gradually decays to 115 mAh g -1After 10 charge-discharge cycles, the specific capacity of Example 11 can still be maintained at 150 mAh g -1 , and has good cycle stability. This shows that coating the carbon layer helps to improve the specific capacity and cycle stability of the material.
[0166] 4) Effects of sucrose addition sequence and sintering treatment on the cycling performance of Li2FeSiO4 / C
[0167] The present invention respectively performs cycle performance tests on Example 1, Example 11, Comparative Examples 1 to 3 and Comparative Example 8 at a current density of 0.1C, and the test results are as follows: Fig.14 shown. Fig.14 In the figure, Figure a is the cycle performance curve of Example 1; Figure b is the cycle performance curve of Comparative Example 8; Figure c is the cycle performance curve of Comparative Example 2; Figure d is the cycle performance curve of Comparative Example 3; Figure e is the cycle performance curve of Example 11; and Figure f is the cycle performance curve of Comparative Example 1.
[0168] Depend on Fig.14 It can be seen that the specific capacities of Example 1, Example 11, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 8 after 100 charge and discharge cycles are 116 mAh·g -1 , 41mAh·g -1 、150mAh·g -1 、70mAh·g -1 、125mAh·g -1 and 78mAh g -1 , the charge and discharge efficiency is close to 100%. The results show that after 10 charge and discharge cycles, the specific capacity of different samples tends to be stable, among which the specific capacity of comparative example 1 gradually increases during the first 50 cycles, and then slowly decreases; the specific capacity of Example 1 and Example 11 gradually increases during the initial charge and discharge, which may be due to the activation of Li2FeSiO4 during the charge and discharge process. This shows that compared with the Li2FeSiO4 / C composite material with sucrose added first and carbonized by secondary calcination, the Li2FeSiO4 / C composite material with sucrose added later and carbonized by secondary calcination shows better cycle stability, maintains a higher specific capacity after 100 charge and discharge cycles, and has better cycle stability.
[0169] 5) Effects of sucrose addition order and sintering treatment on the rate performance of Li2FeSiO4 / C
[0170] The present invention takes Example 1, Example 11, Comparative Examples 1 to Comparative Examples 3 and Comparative Examples 8 as examples, and performs cycle performance tests at current densities of 0.01C, 0.05C, 0.1C, 1C and 2C, respectively, and the test results are as follows: Fig.15 As shown. Among them, 1C is 332mA·g-1 . Fig.15 In the figure, Figure a is the rate performance curve of Example 1; Figure b is the rate performance curve of Comparative Example 8; Figure c is the rate performance curve of Comparative Example 2; Figure d is the rate performance curve of Comparative Example 3; Figure e is the rate performance curve of Example 11; and Figure f is the rate performance curve of Comparative Example 1.
[0171] Depend on Fig.15 It can be seen that at a current density of 1C, the specific capacities of Example 1, Example 11, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 8 are respectively maintained at 83 mAh·g -1 , 19mAh·g -1 、82mAh·g -1 , 20mAh·g -1 、80mAh·g -1 and 35mAh·g -1 When the current density returns to 0.01C, the specific capacity is consistent with the initial charge and discharge capacity, indicating that the structural stability is good. The results show that the rate performance of comparative example 8 after secondary solvent heat treatment is significantly lower; Fig.15 As shown in Figure d and Figure f, the specific capacity of Comparative Example 3 and Comparative Example 1 prepared by adding sucrose first is low at a current density of 2C, while the specific capacity of Comparative Example 2 and Example 11 samples prepared by adding sucrose later can be maintained at 40 mAh·g at a high current density of 2C. -1 , with better rate performance. This shows that adding sucrose later is more conducive to improving the rate performance of the material.
[0172] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a positive electrode material for a lithium-ion battery based on iron tailings, characterized in that: The following steps are involved: The iron tailings are subjected to acid leaching treatment in an inorganic acid solution, so that the iron in the iron tailings is dissolved in the inorganic acid solution, and the solid and liquid are separated to obtain a filter residue and a filtrate; The filtrate is subjected to reduction treatment to reduce the iron in the filtrate to Fe 2+ , obtain Fe 2+ solution; heating the iron-containing solution to make Fe 2+ The anion crystals provided by the inorganic acid solution are precipitated to obtain Fe 2+ of crystal salt; dispersing the filter residue in an alkali solution to obtain a suspension; The suspension is subjected to a heating treatment to separate the solid from the liquid to obtain a liquid component; Adding polyethylene glycol 400 to the liquid component and mixing evenly, adjusting the pH value of the solution to 2.5-3.5, aging, filtering and drying to obtain nano-white carbon black; The Fe 2+ The crystalline salt is used as the iron source, the nano-white carbon black is used as the silicon source, lithium hydroxide is used as the lithium source, and water is used as the solvent to prepare Li2FeSiO4 by a hydrothermal method; Using Li2FeSiO4 as the positive electrode material for lithium-ion batteries, or The composite material obtained by taking the Li2FeSiO4 as a matrix and coating the surface of the matrix with a carbon layer is used as a positive electrode material for a lithium ion battery.
2. The preparation method according to claim 1, characterized in that The composite material is prepared by the following steps: Using sucrose as a carbon source, mixing it with the Li2FeSiO4 in water to obtain a fourth mixed solution; subjecting the fourth mixed solution to a hydrothermal reaction at 180° C. to 220° C., performing solid-liquid separation, washing, and drying to obtain a precursor; The precursor is sintered in an argon atmosphere so that carbon is coated on the surface of Li2FeSiO4 to obtain a positive electrode material for a lithium ion battery.
3. The preparation method according to claim 2, characterized in that: The mass ratio of Li2FeSiO4 to sucrose is 1:0.1-4; The sintering temperature is 500°C to 600°C.
4. The preparation method according to claim 1, characterized in that: The Fe 2+ The molar ratio of the crystalline salt, nano-white carbon black and lithium hydroxide is 1:1:3-4.
5. The preparation method according to claim 1, characterized in that: When Li2FeSiO4 is prepared by the hydrothermal method, the temperature of the hydrothermal reaction is 220℃~260℃.
6. The preparation method according to claim 1, characterized in that: The inorganic acid is sulfuric acid; The temperature of the acid leaching treatment is 95°C to 105°C.
7. The preparation method according to claim 1, characterized in that: The reducing agent is iron powder; When the iron-containing solution is subjected to a heating treatment, the heating treatment temperature is 45°C to 55°C.
8. The preparation method according to claim 1, characterized in that: The alkali solution is NaOH solution; The heating temperature when the suspension is subjected to heat treatment is 230°C to 270°C.
9. The preparation method according to claim 1, characterized in that: The mass ratio of the polyethylene glycol 400 to the filter residue is 0.3-0.7:
5.
10. A positive electrode material for a lithium ion battery prepared by the preparation method according to any one of claims 1 to 9.