Leaching method of battery-grade lithium carbonate
By using hydrogen and argon treatment, potassium fluoride roasting and leaching of C-undecylcalix[4] hydrocarbon resorcinol and valinomycin composite liquid in the preparation of lithium battery grade lithium carbonate, the problem was solved In the existing technology, the problem of insufficient purity and yield of lithium carbonate has been achieved. This method realizes efficient preparation of lithium carbonate, is suitable for lithium battery raw materials, and reduces costs.
Patent Information
- Application Number
- CN202410942129.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
AI Technical Summary
The existing technology is difficult to effectively improve the preparation technology level and purity of battery-grade lithium carbonate, and cannot meet the needs of the lithium battery industry for high purity and high efficiency.
A dimethyl sulfide solution is used which includes lepidolite powder treated at high temperature in a mixed gas of hydrogen and argon, adding potassium fluoride for roasting, and using C-undecylcalix[4] hydrocarbon resorcinol and valinomycin. The leaching method of sulfone complex liquid and carbon dioxide gas removes the hydroxyl groups on the surface of lepidolite, destroys its dense structure, promotes the dissolution of lithium ions, and reduces the content of impurity ions through the complex structure. Finally, high-purity lithium carbonate is obtained through evaporation and crystallization.
It improves the purity and yield of lithium carbonate, is suitable for battery raw materials, reduces raw material costs, and enhances the material supply capacity of the lithium battery industry.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium carbonate preparation, and in particular to a method for leaching battery-grade lithium carbonate. Background Art
[0002] As an upstream product of most other lithium products, lithium carbonate is widely used in glass, ceramics, metallurgy, chemical industry, electronics, medicine, battery and other industries because of its wide range of uses and its outstanding advantages in energy storage equipment. Therefore, the development and utilization of lithium resources to prepare various lithium salt compounds, especially lithium carbonate, the raw material of lithium batteries, is of special significance. With the rapid development of the lithium battery industry, the demand for battery-grade lithium carbonate will increase, the scope of application will continue to expand, and the competition will become increasingly fierce, which will put higher requirements on its preparation technology and purity standards. In order to meet the demand for battery-grade lithium carbonate, improve the level of preparation technology, promote the rational development and utilization of lithium resources, and expand the lithium product market, it is imperative to optimize the preparation of battery-grade lithium carbonate. Summary of the invention
[0003] To this end, the present invention provides a method for leaching battery-grade lithium carbonate, the preparation steps comprising:
[0004] (1) grinding lithium mica into powder, collecting the sieved powder through a 300-mesh sieve, keeping the sieved powder at 600° C. for 2 to 3 hours in a mixed gas atmosphere of hydrogen and argon, cooling to room temperature in an argon atmosphere after the insulation, adding potassium fluoride powder to the powder to form a mixed powder, heating the mixed powder to 420 to 450° C. and roasting for 4 to 5 hours to obtain a roasted powder; preparing a sulfuric acid solution in a reactor, adding the roasted powder to the sulfuric acid solution, and then sealing the reactor, heating to 200 to 220° C. and keeping for 2 to 4 hours, air cooling to room temperature after the insulation, opening the reactor, and performing solid-liquid separation to obtain a leachate and a leach residue;
[0005] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and a dimethyl sulfoxide complex solution of valinomycin, mixing the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and the dimethyl sulfoxide complex solution of valinomycin to form a mixed solution, heating the mixed solution to 85±5° C. in a water bath, stirring at a speed of 100 r / min for more than 30 min, then adding anhydrous sodium carbonate to the mixed solution under stirring, continuing to stir for more than 30 min after the addition is completed, then air cooling to room temperature, separating the solid and the liquid, washing the solid phase with ethanol for more than 3 times, and drying at 60° C. for more than 20 min to obtain crude lithium carbonate;
[0006] (3) adding the crude lithium carbonate into deionized water, stirring evenly to form a suspension, stirring the suspension, introducing carbon dioxide gas into the suspension during stirring to convert the lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, evaporating and crystallizing the clear solution at 80° C. in an evaporating dish to obtain the battery-grade lithium carbonate.
[0007] Furthermore, in the step (1), in the mixed gas of hydrogen and argon, the mixed volume ratio of hydrogen to argon is hydrogen:argon=5:95.
[0008] Furthermore, in the step (1), the mass ratio of adding potassium fluoride powder to the lepidolite powder to form a mixed powder is lepidolite powder:potassium fluoride powder=30:1-2.
[0009] Furthermore, in the step (1), the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the calcined powder added to the sulfuric acid solution is calcined powder: sulfuric acid solution = 1 g: 4-5 mL.
[0010] Furthermore, in the step (2), in the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution, the concentration of C-undecylcalix[4]hydrocarbon resorcinol is 10-12 mg / mL, and the concentration of valinomycin is 22-26 mg / mL; the volume ratio of the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution is leaching solution: C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution = 10:1-2.
[0011] Furthermore, in the step (2), the amount ratio of anhydrous sodium carbonate added to the mixed solution is mixed solution: anhydrous sodium carbonate = 100 mL: 15 g.
[0012] Furthermore, in the step (3), the mass ratio of the crude lithium carbonate added to the deionized water is crude lithium carbonate: deionized water = 1:30; the carbon dioxide introduction flow rate is 8 to 10 L / min, and the introduction time is more than 2 hours.
[0013] The beneficial effects of the present invention are as follows: the lithium carbonate obtained by treating lithium mica with the method of the present invention has a high purity and is suitable for use as a battery raw material, and the yield of lithium carbonate is high, which can reduce the cost of raw materials. The higher the hydroxyl content on the surface of lithium mica, the more difficult it is for lithium to dissolve; on the contrary, the lower the hydroxyl content of lithium mica, the easier it is for lithium to dissolve. The present invention first treats lithium mica powder at high temperature in a hydrogen environment to remove the hydroxyl groups on the surface of lithium mica, and then adds potassium fluoride before roasting, utilizes the strong electronegativity of fluoride ions, destroys the dense structure of lithium mica during roasting, promotes the dissolution of lithium ions in the subsequent leaching process, and improves the yield of lithium. Subsequently, a dimethyl sulfoxide composite solution of C-undecylcalix[4]hydrocarbon resorcinol and valinomycin is added, and C-undecylcalix[4]hydrocarbon resorcinol and valinomycin are used to form a complex structure with potassium, sodium, magnesium, calcium and other ions, thereby reducing the content of these impurity ions in the crude lithium carbonate, and also reducing the carbide precipitation formed by magnesium, calcium and sodium carbonate. Carbon dioxide gas is then used to convert lithium carbonate into soluble lithium bicarbonate, the mixed magnesium carbonate and calcium carbonate precipitates are filtered out, and the soluble lithium bicarbonate is then evaporated, crystallized and decomposed to form lithium carbonate, thereby obtaining a lithium carbonate product of battery raw material grade. DETAILED DESCRIPTION
[0014] The present invention will be further described below in conjunction with the embodiments.
[0015] Example 1
[0016] A method for leaching battery-grade lithium carbonate, the preparation steps comprising:
[0017] (1) Grinding lithium mica into powder (for the convenience of comparison, each embodiment and comparative example uses the same batch of lithium mica), the powder is passed through a 300-mesh sieve to collect the sieved powder, the sieved powder is kept at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, the mixed gas of hydrogen and argon having a mixing volume ratio of hydrogen to argon of 5:95; after the insulation is completed, the mixture is cooled to room temperature in an argon atmosphere, and then potassium fluoride powder is added to the powder to form a mixed powder, and potassium fluoride powder is added to the lithium mica powder to form a mixed powder. The mass ratio is lepidolite powder: potassium fluoride powder = 30:1; the mixed powder is heated to 420°C and roasted for 4 hours to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3 hours, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0018] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid, mixing the leaching solution with the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid to form a mixed liquid, wherein the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid has a concentration of 10 mg / mL and a concentration of 22 mg / mL of valinomycin; the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid are mixed to form a mixed liquid. The volume ratio of the mixed solution is leaching solution: C-undecyl calix [4] hydrocarbon resorcinol, dimethyl sulfoxide complex solution of valinomycin = 10:1; the mixed solution is heated to 85±5°C in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol 3 times, and dried at 60°C for 20min to obtain crude lithium carbonate;
[0019] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during the stirring process, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the battery-grade lithium carbonate.
[0020] Example 2
[0021] A method for leaching battery-grade lithium carbonate, the preparation steps comprising:
[0022] (1) Grinding lepidolite to powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen to argon is 5:95; cooling to room temperature in an argon atmosphere after the insulation, and then adding potassium fluoride powder to the powder to form a mixed powder, wherein the mass ratio of the mixed powder to form a mixed powder is lepidolite powder: potassium fluoride. powder = 30:1; the mixed powder is heated to 420°C and roasted for 4h to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3h, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0023] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid, mixing the leaching solution with the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid to form a mixed liquid, wherein the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid has a concentration of 11 mg / mL and a concentration of 24 mg / mL of valinomycin; the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid are mixed to form a mixed liquid. The volume ratio of the mixed solution is leaching solution: C-undecyl calix [4] hydrocarbon resorcinol, dimethyl sulfoxide complex solution of valinomycin = 10:1; the mixed solution is heated to 85±5°C in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol 3 times, and dried at 60°C for 20min to obtain crude lithium carbonate;
[0024] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during the stirring process, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the battery-grade lithium carbonate.
[0025] Example 3
[0026] A method for leaching battery-grade lithium carbonate, the preparation steps comprising:
[0027] (1) Grinding lepidolite to powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen to argon is 5:95; cooling to room temperature in an argon atmosphere after the insulation, and then adding potassium fluoride powder to the powder to form a mixed powder, wherein the mass ratio of the mixed powder to form a mixed powder is lepidolite powder: potassium fluoride. powder = 30:2; the mixed powder is heated to 420°C and roasted for 4h to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3h, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0028] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid, mixing the leaching solution with the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid to form a mixed liquid, wherein the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid has a concentration of 11 mg / mL and a concentration of 24 mg / mL of valinomycin; the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid are mixed to form a mixed liquid. The volume ratio of the mixed solution is leaching solution: C-undecyl calix [4] hydrocarbon resorcinol, dimethyl sulfoxide complex solution of valinomycin = 10:2; the mixed solution is heated to 85±5°C in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol 3 times, and dried at 60°C for 20min to obtain crude lithium carbonate;
[0029] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during the stirring process, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the battery-grade lithium carbonate.
[0030] Example 4
[0031] A method for leaching battery-grade lithium carbonate, the preparation steps comprising:
[0032] (1) Grinding lepidolite to powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen to argon is 5:95; cooling to room temperature in an argon atmosphere after the insulation, and then adding potassium fluoride powder to the powder to form a mixed powder, wherein the mass ratio of the mixed powder to form a mixed powder is lepidolite powder: potassium fluoride. powder = 30:2; the mixed powder is heated to 420°C and roasted for 4h to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3h, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0033] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid, mixing the leaching solution with the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid to form a mixed liquid, wherein the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid has a concentration of 12 mg / mL and a concentration of 26 mg / mL of valinomycin; the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid are mixed to form a mixed liquid. The volume ratio of the mixed solution is leaching solution: C-undecyl calix [4] hydrocarbon resorcinol, dimethyl sulfoxide complex solution of valinomycin = 10:2; the mixed solution is heated to 85±5°C in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol 3 times, and dried at 60°C for 20min to obtain crude lithium carbonate;
[0034] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during the stirring process, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the battery-grade lithium carbonate.
[0035] Comparative Example 1
[0036] A comparative method for leaching lithium carbonate comprises the following steps:
[0037] (1) grinding lithium mica into powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen and argon in the mixed gas of hydrogen and argon is hydrogen:argon=5:95; cooling to room temperature in an argon atmosphere after the insulation, and then heating to 420° C. and roasting for 4 h to obtain a roasted powder; preparing a sulfuric acid solution in a reactor, adding the roasted powder to the sulfuric acid solution, wherein the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder to the sulfuric acid solution is roasted powder:sulfuric acid solution=1 g:5 mL; then sealing the reactor, heating to 200° C. and keeping the temperature for 3 h, air cooling to room temperature after the insulation, opening the reactor, and performing solid-liquid separation to obtain a leachate and a leach residue;
[0038] (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid, mixing the leaching solution with the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid to form a mixed liquid, wherein the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid has a concentration of 11 mg / mL and a concentration of 24 mg / mL of valinomycin; the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite liquid are mixed to form a mixed liquid. The volume ratio of the mixed solution is leaching solution: C-undecyl calix [4] hydrocarbon resorcinol, dimethyl sulfoxide complex solution of valinomycin = 10:1; the mixed solution is heated to 85±5°C in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol 3 times, and dried at 60°C for 20min to obtain crude lithium carbonate;
[0039] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during stirring, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the lithium carbonate described in this comparative example.
[0040] Comparative Example 2
[0041] A comparative method for leaching lithium carbonate comprises the following steps:
[0042] (1) Grinding lepidolite to powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen to argon is 5:95; cooling to room temperature in an argon atmosphere after the insulation, and then adding potassium fluoride powder to the powder to form a mixed powder, wherein the mass ratio of the mixed powder to form a mixed powder is lepidolite powder: potassium fluoride. powder = 30:1; the mixed powder is heated to 420°C and roasted for 4h to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3h, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0043] (2) preparing a dimethyl sulfoxide solution of C-undecylcalix[4]hydrocarbon resorcinol, mixing the leaching solution and the dimethyl sulfoxide solution of C-undecylcalix[4]hydrocarbon resorcinol to form a mixed solution, wherein the concentration of C-undecylcalix[4]hydrocarbon resorcinol in the dimethyl sulfoxide solution of C-undecylcalix[4]hydrocarbon resorcinol is 11 mg / mL; and the volume ratio of the leaching solution to the dimethyl sulfoxide solution of C-undecylcalix[4]hydrocarbon resorcinol is 1:1. ] hydrocarbon resorcinol dimethyl sulfoxide liquid = 10:1; the mixed solution is heated to 85±5℃ in a water bath and stirred at a speed of 100r / min for 30min, and then anhydrous sodium carbonate is added to the mixed solution under stirring, and the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100mL: 15g; after the addition is completed, stirring is continued for 30min, and then air-cooled to room temperature, solid-liquid separation, the solid phase is washed with ethanol 3 times, and dried at 60℃ for 20min to obtain crude lithium carbonate;
[0044] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during stirring, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the lithium carbonate described in this comparative example.
[0045] Comparative Example 3
[0046] A comparative method for leaching lithium carbonate comprises the following steps:
[0047] (1) Grinding lepidolite to powder, collecting the sieved powder through a 300-mesh sieve, and keeping the sieved powder at 600° C. for 2 h in a mixed gas atmosphere of hydrogen and argon, wherein the mixed volume ratio of hydrogen to argon is 5:95; cooling to room temperature in an argon atmosphere after the insulation, and then adding potassium fluoride powder to the powder to form a mixed powder, wherein the mass ratio of the mixed powder to form a mixed powder is lepidolite powder: potassium fluoride. powder = 30:1; the mixed powder is heated to 420°C and roasted for 4h to obtain roasted powder; a sulfuric acid solution is prepared in a reactor, and the roasted powder is added to the sulfuric acid solution, the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the roasted powder added to the sulfuric acid solution is roasted powder: sulfuric acid solution = 1g: 5mL; then the reactor is sealed, heated to 200°C and kept warm for 3h, and after the end of the heat preservation, it is air-cooled to room temperature, the reactor is opened, and the solid-liquid separation is performed to obtain the leachate and the leach residue;
[0048] (2) preparing a dimethyl sulfoxide solution of valinomycin, mixing the leaching solution and the dimethyl sulfoxide solution of valinomycin to form a mixed solution, wherein the concentration of valinomycin in the dimethyl sulfoxide solution of valinomycin is 24 mg / mL; the mixed volume ratio of the leaching solution and the dimethyl sulfoxide solution of valinomycin is leaching solution: dimethyl sulfoxide solution of valinomycin = 10:1; heating the mixed solution to 85±5° C. in a water bath, stirring at a speed of 100 r / min for 30 min, and then adding anhydrous sodium carbonate to the mixed solution under stirring, wherein the amount ratio of anhydrous sodium carbonate added to the mixed solution is to the mixed solution: anhydrous sodium carbonate = 100 mL: 15 g; stirring is continued for 30 min after the addition is completed, and then air-cooling is performed to room temperature, solid-liquid separation is performed, the solid phase is washed with ethanol three times, and dried at 60° C. for 20 min to obtain crude lithium carbonate;
[0049] (3) adding the crude lithium carbonate to deionized water and stirring evenly to form a suspension, wherein the mass ratio of the crude lithium carbonate to the deionized water is crude lithium carbonate: deionized water = 1:30; stirring the suspension, and introducing carbon dioxide gas into the suspension during stirring, wherein the carbon dioxide introduction flow rate is 8 L / min and the introduction time is 2 h; converting lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, and evaporating and crystallizing the clear solution in an evaporating dish at 80° C. to obtain the lithium carbonate described in this comparative example.
[0050] Example 5
[0051] The purity and yield of lithium carbonate obtained by the methods described in the above embodiments and comparative examples were tested. The yield is the ratio of the actual yield of lithium carbonate to the theoretical yield of lithium carbonate. The results are shown in Table 1.
[0052] As shown in Table 1, the lithium carbonate obtained by treating lithium mica with the method of the present invention has a high purity and is suitable for use as a battery raw material. The yield of lithium carbonate is high, which can reduce the cost of raw materials. The higher the hydroxyl content on the surface of lithium mica, the more difficult it is for lithium to dissolve; on the contrary, the lower the hydroxyl content of lithium mica, the easier it is for lithium to dissolve. The present invention first treats lithium mica powder at high temperature in a hydrogen environment to remove the hydroxyl groups on the surface of lithium mica, and then adds potassium fluoride before roasting, using the strong electronegativity of fluoride ions to destroy the dense structure of lithium mica during roasting, promote the dissolution of lithium ions in the subsequent leaching process, and improve the yield of lithium. Subsequently, a dimethyl sulfoxide composite solution of C-undecylcalix[4]hydrocarbon resorcinol and valinomycin is added, and C-undecylcalix[4]hydrocarbon resorcinol and valinomycin are used to form a complex structure with potassium, sodium, magnesium, calcium and other ions, thereby reducing the content of these impurity ions in the crude lithium carbonate, and also reducing the carbide precipitation formed by magnesium, calcium and sodium carbonate. Carbon dioxide gas is then used to convert lithium carbonate into soluble lithium bicarbonate, the mixed magnesium carbonate and calcium carbonate precipitates are filtered out, and the soluble lithium bicarbonate is then evaporated, crystallized and decomposed to form lithium carbonate, thereby obtaining a lithium carbonate product of battery raw material grade.
[0053] Table 1
[0054] Experimental Group Lithium carbonate purity Lithium carbonate yield Example 1 99.64% 76.52% Example 2 99.81% 77.08% Example 3 99.77% 77.11% Example 4 99.72% 77.03% Comparative Example 1 98.69% 66.85% Comparative Example 2 91.80% 72.34% Comparative Example 3 92.15% 74.67%
[0055] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for leaching battery-grade lithium carbonate, It is characterized in that The preparation steps include: (1) grinding lithium mica into powder, collecting the sieved powder through a 300-mesh sieve, keeping the sieved powder at 600° C. for 2 to 3 hours in a mixed gas atmosphere of hydrogen and argon, cooling to room temperature in an argon atmosphere after the insulation, adding potassium fluoride powder to the powder to form a mixed powder, heating the mixed powder to 420 to 450° C. and roasting for 4 to 5 hours to obtain a roasted powder; preparing a sulfuric acid solution in a reactor, adding the roasted powder to the sulfuric acid solution, and then sealing the reactor, heating to 200 to 220° C. and keeping for 2 to 4 hours, air cooling to room temperature after the insulation, opening the reactor, and performing solid-liquid separation to obtain a leachate and a leach residue; (2) preparing a C-undecylcalix[4]hydrocarbon resorcinol and a dimethyl sulfoxide complex solution of valinomycin, mixing the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and the dimethyl sulfoxide complex solution of valinomycin to form a mixed solution, heating the mixed solution to 85±5° C. in a water bath, stirring at a speed of 100 r / min for more than 30 min, then adding anhydrous sodium carbonate to the mixed solution under stirring, continuing to stir for more than 30 min after the addition is completed, then air cooling to room temperature, separating the solid and the liquid, washing the solid phase with ethanol for more than 3 times, and drying at 60° C. for more than 20 min to obtain crude lithium carbonate; (3) adding the crude lithium carbonate into deionized water, stirring evenly to form a suspension, stirring the suspension, introducing carbon dioxide gas into the suspension during stirring to convert the lithium carbonate into soluble lithium bicarbonate, precipitating residual magnesium and calcium in the crude lithium carbonate, and then filtering to obtain a clear solution, evaporating and crystallizing the clear solution at 80° C. in an evaporating dish to obtain the battery-grade lithium carbonate.
2. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (1), in the mixed gas of hydrogen and argon, the mixed volume ratio of hydrogen to argon is hydrogen:argon=5:
95.
3. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (1), potassium fluoride powder is added to the lepidolite powder to form a mixed powder in a mass ratio of lepidolite powder:potassium fluoride powder=30:1-2.
4. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (1), the mass percentage of the solute in the sulfuric acid solution is 15%, and the amount ratio of the calcined powder added to the sulfuric acid solution is calcined powder: sulfuric acid solution = 1g: 4-5mL.
5. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (2), in the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution, the concentration of C-undecylcalix[4]hydrocarbon resorcinol is 10-12 mg / mL, and the concentration of valinomycin is 22-26 mg / mL; the volume ratio of the leaching solution and the C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution is leaching solution: C-undecylcalix[4]hydrocarbon resorcinol and valinomycin dimethyl sulfoxide composite solution = 10:1-2.
6. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (2), the amount of anhydrous sodium carbonate added to the mixed solution is mixed solution: anhydrous sodium carbonate = 100 mL: 15 g.
7. A method for leaching battery-grade lithium carbonate according to claim 1, It is characterized in that In the step (3), the mass ratio of the crude lithium carbonate added to the deionized water is crude lithium carbonate: deionized water = 1:30; the carbon dioxide introduction flow rate is 8 to 10 L / min, and the introduction time is more than 2 hours.
Citation Information
Cited By
High-stability lithium ion battery electrolyte and preparation method thereof
CN119381569A
Anti-scaling method and device for long-period operation of MVR (mechanical vapor recompression) evaporator for concentrating high-carbonate lithium solution
CN120423745A
A long-period operation scale prevention method and device for MVR evaporator for concentrating high-carbonate lithium liquid
CN120423745B