Inorganic nano-material for cancer sonodynamic therapy and preparation method and application thereof

Through the preparation of titanium-based alkali metal fluoride nanomaterials, the problems of low quantum yield and poor biological safety of inorganic nano-sound sensitizer ROS are solved, and the efficient generation of singlet oxygen under ultrasonic radiation is achieved, which is suitable for sonodynamic therapy of cancer. Demonstrated good sonodynamic performance and biosafety.

CN118754193APending Publication Date: 2024-10-11HUBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410736589.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing inorganic nano-sonosensitizers have low ROS quantum yields under ultrasonic radiation and poor biological safety, which limits the clinical application of sonodynamic therapy.

Method used

Titanium-based alkali metal fluoride inorganic nanomaterials are used and prepared by co-precipitation of titanium-containing precursors with ammonium fluoride and alkali metal hydroxide in high-temperature solvents to form titanium-based alkali metal fluoride nanomaterials with narrow band gaps, which can be used in Under ultrasonic radiation, it combines with intracellular oxygen to generate singlet oxygen to improve sonodynamic performance.

Benefits of technology

The prepared titanium-based alkali metal fluoride nanomaterial has a high ROS quantum yield under ultrasonic radiation, has good biological safety and sonosensitizer properties, is suitable for sonodynamic therapy of cancer, and exhibits excellent sonodynamic properties and good sonodynamic properties. Clinical application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754193A_ABST
    Figure CN118754193A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic biological functional materials, in particular to an inorganic nano material for cancer sonodynamic therapy and a preparation method and application thereof.The preparation method comprises the steps that a titanium-containing precursor and a high-boiling-point solvent are evenly mixed, and a reaction solution is obtained; heating the reaction solution in an inert atmosphere and preserving heat to decompose the precursor to obtain a mixed solution; cooling the obtained mixed solution to room temperature in an inert atmosphere, adding a methanol solution dissolved with ammonium fluoride and alkali metal hydroxide, and removing methanol and water; and continuously heating in an inert atmosphere, keeping the temperature until the reaction is complete, cooling to room temperature, precipitating, separating and washing the product to obtain the titanium-based alkali metal fluoride inorganic nano material. According to the preparation method, conditions are easy to control, repeatability is good, the prepared nanometer material is good in dispersity, uniformity and repeatability, singlet oxygen (1O2) is generated after the nanometer material is combined with oxygen in cells under ultrasonic radiation, and therefore the effect of sonodynamic cancer treatment is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic biological functional materials, and in particular to an inorganic nanomaterial for cancer sonodynamic therapy and a preparation method and application thereof. Background Art

[0002] Cancer, as one of the most serious diseases worldwide, has become the biggest threat to human health. At present, surgery, chemotherapy and radiotherapy are still the first-line treatment methods for tumors in clinical applications, but they have side effects such as drug resistance, severe toxicity to normal tissues and severe metastasis. In recent years, non-invasive treatment methods such as photodynamic therapy (PDT) and photothermal therapy (PTT) based on nanomaterials have used visible light or near-infrared light to excite nanomaterials to produce toxic reactive oxygen species (ROS) or high temperatures, thereby killing tumor cells. [3] , has been approved by the U.S. Food and Drug Administration for clinical trials for the treatment of tumors. However, due to the limited penetration depth of light, photodynamic or photothermal therapy cannot achieve efficient treatment of deep tumors. Therefore, it is of great significance to develop new methods that can effectively treat deep tumors.

[0003] Ultrasound is a mechanical wave that oscillates periodically and has a frequency higher than human hearing. It has become a key technology in medical examinations due to its strong tissue penetration ability. Ultrasound-driven sonodynamic therapy (SDT) uses low-intensity ultrasound to stimulate sonosensitizers to interact with oxygen in tumor tissues, generating hydroxyl radicals (·OH) and superoxide anions (·O 2- ) and singlet oxygen ( 1 O 2 ) and other ROS, which damage organelles and DNA by oxidizing lipids, and induce apoptosis of tumor cells. Compared with PDT and PTT, SDT not only has strong penetration and can non-invasively target lesion tissues and sites in a short time, but also uses low-intensity ultrasound, and long-term treatment will not cause damage to surrounding normal tissues. It is expected to become a new method to replace phototherapy for deep tumors.

[0004] The sonosensitizers currently used for SDT include organic small molecule sonosensitizers and inorganic sonosensitizers. Organic sonosensitizers represented by porphyrin and its derivatives have been widely studied because of their high ROS quantum yield. However, their poor water stability, potential phototoxicity, chemical instability and poor tumor accumulation have hindered their further application in clinical practice. Inorganic sonosensitizers represented by titanium dioxide are favored by researchers because of their lower phototoxicity and better chemical stability. However, commercial TiO 2 The band gap of nanoparticles is wide, and the electrons and holes generated after ultrasonic radiation are easy to recombine quickly, and the ROS quantum yield is not high, which restricts its sonodynamic performance. 2It is non-degradable in the body, and its long-term biosafety is also a concern.

[0005] In summary, in order to solve the problems of low ROS quantum yield and poor biosafety of current inorganic nanosonosensitizers, it is still necessary to develop inorganic nanosonosensitizers with good biocompatibility and high sonodynamic performance to promote the clinical application of SDT. Summary of the invention

[0006] One of the purposes of the present invention is to provide a method for preparing an inorganic nanomaterial for cancer sonodynamic therapy. The conditions of the synthesis method are easy to control and the repeatability is good. The prepared nanomaterial has good dispersibility, uniformity and repeatability. After combining with oxygen in cells under ultrasonic radiation, singlet oxygen ( 1 O 2 )Thereby achieving the effect of sonodynamic therapy for cancer.

[0007] The second object of the present invention is to provide an inorganic nanomaterial for cancer sonodynamic therapy, which has sonosensitizer properties and can generate singlet oxygen ( 1 O 2 ) to achieve the effect of sonodynamic therapy for cancer.

[0008] The third object of the present invention is to provide an application of inorganic nanomaterials for cancer sonodynamic therapy.

[0009] The solution adopted by the present invention to achieve one of the purposes is: a method for preparing an inorganic nanomaterial for cancer sonodynamic therapy, comprising the following steps:

[0010] S1, mixing the titanium-containing precursor and the high boiling point solvent uniformly to obtain a reaction solution;

[0011] S2, heating and keeping the reaction solution warm under an inert atmosphere to decompose the precursor in the reaction solution to obtain a mixed solution;

[0012] S3, cooling the obtained mixed solution to room temperature under an inert atmosphere, adding a methanol solution containing ammonium fluoride and an alkali metal hydroxide, and then removing methanol and water;

[0013] S4. Continue heating and keeping warm under an inert atmosphere until the reaction is complete, then cool to room temperature, precipitate, separate, and wash the product to obtain the titanium-based alkali metal fluoride inorganic nanomaterial.

[0014] Preferably, in step S1, the titanium-containing precursor is selected from one or more of titanium acetylacetonate, titanyl sulfate, titanium chloride, and butyl titanate.

[0015] Preferably, in step S1, the high boiling point solvent is selected from one or more of oleic acid, oleylamine and octadecene.

[0016] Preferably, in step S2, the reaction solution is heated to 120-160° C. under the protection of an inert gas, and the temperature is kept until the precursor in the reaction solution is decomposed.

[0017] Preferably, in step S3, the molar ratio of ammonium fluoride to alkali metal hydroxide is 1:1-5.

[0018] Preferably, in step S3, the operation of removing methanol and water is: heating the reaction system to 120-160° C. under the protection of an inert gas, and keeping the temperature to remove methanol and water.

[0019] Preferably, in step S4, the temperature is heated to 260-320° C. and kept warm until the reaction is completed.

[0020] Preferably, in step S4, the solvent used to precipitate the titanium-based alkali metal fluoride inorganic nanomaterial is selected from one or more of ethanol, methanol and water.

[0021] The solution adopted by the present invention to achieve the second purpose is: an inorganic nanomaterial for cancer sonodynamic therapy is prepared by the preparation method.

[0022] The solution adopted by the present invention to achieve the third purpose is: the application of the titanium-based alkali metal fluoride inorganic nanomaterial in cancer sonodynamic therapy.

[0023] The present invention has the following advantages and beneficial effects:

[0024] 1. The preparation method of the present invention has easy controllable conditions and good repeatability. The prepared nanomaterials have good dispersibility, uniformity and repeatability. Singlet oxygen ( 1 O 2 ) thereby achieving the effect of sonodynamic therapy for cancer. The nanomaterial prepared by the preparation method of the present invention exhibits excellent sonodynamic performance and has good application prospects in sonodynamic therapy for cancer.

[0025] 2. The titanium-based alkali metal fluoride inorganic nanomaterial provided by the present invention has sonosensitizer properties. Due to the narrow band gap, electron holes are easily separated under ultrasonic radiation; at the same time, the abundant oxygen vacancies can act as electron traps to prevent the recombination of electrons and holes, and the ROS quantum yield is higher. Therefore, the titanium-based alkali metal fluoride inorganic nanomaterial of the present invention can be used as an inorganic nanomaterial with sonosensitivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 for Na 3 TiF 6 X-ray diffraction patterns of NPs;

[0027] Figure 2 for Na 3 TiF 6 X-ray photoelectron spectroscopy of NPs;

[0028] Figure 3 Preparation of Na for Titanium Acetylacetonate 3 TiF 6 Transmission electron microscopy images of NPs at different resolutions;

[0029] Figure 4 Preparation of Na for titanium tetrachloride 3 TiF 6 Transmission electron microscopy images of NPs at different resolutions;

[0030] Figure 5 Preparation of Na2TiO4 3 TiF 6 Transmission electron microscopy images of NPs at different resolutions;

[0031] Figure 6 Preparation of Na for titanyl sulfate 3 TiF 6 Transmission electron microscopy images of NPs at different resolutions;

[0032] Figure 7 for Na 3 TiF 6 ESR oxygen vacancy map of NPs and comparison with commercial titanium dioxide;

[0033] Figure 8 for Na 3 TiF 6 Electrochemical impedance spectroscopy of NPs and comparison with commercial titanium dioxide;

[0034] Fig. 9 for Na 3 TiF 6 Ultrasonic response current diagram of NPs and comparison with commercial titanium dioxide;

[0035] Fig.10 for Na 3 TiF 6 The rate diagram of NPs oxidizing 1,3-diphenylisobenzofuran (DPBF) probe under ultrasound, and compared with pure water and commercial titanium dioxide;

[0036] Fig.11 for Na 3 TiF 6 NPs generate ROS in tumor cells under ultrasound. DETAILED DESCRIPTION

[0037] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0038] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.

[0040] According to a typical implementation of an embodiment of the present invention, a method for preparing a titanium-based alkali metal fluoride inorganic nanomaterial is provided, which uses a titanium-containing precursor, ammonium fluoride and an alkali metal hydroxide as raw materials, and utilizes a high-temperature solvent co-precipitation method to obtain a titanium-based alkali metal fluoride inorganic nanomaterial.

[0041] The method comprises:

[0042] Step S1, using a titanium-containing precursor and adding a high boiling point solvent to obtain a reaction solution;

[0043] In the step S1,

[0044] The titanium-containing precursor is selected from one or more of titanium acetylacetonate, titanyl sulfate, titanium chloride, and butyl titanate;

[0045] The high boiling point solvent is selected from one or more of oleic acid, oleylamine, and octadecene. Preferably, the high boiling point solvent is a mixed solvent of oleic acid and octadecene. Preferably, the volume ratio of oleic acid to octadecene is 1:(0.5-3).

[0046] Step S2, heating and keeping the reaction solution warm to decompose the precursor in the reaction solution to obtain a mixed solution;

[0047] In the step S2,

[0048] The reaction solution is heated to 120-160° C. under the protection of an inert gas, kept at this temperature for 30-90 minutes, and then naturally cooled to room temperature.

[0049] Step S3, adding a methanol solution containing ammonium fluoride and alkali metal hydroxide to the mixed solution obtained above, and heating and keeping warm to remove methanol and water;

[0050] In the step S3,

[0051] The molar ratio of ammonium fluoride to alkali metal hydroxide is 1:(1-5); under the protection of inert gas, the mixture is heated to 50-70°C and kept warm for 15-30 minutes to remove methanol, and the mixture is heated to 90-120°C and kept warm for 10-30 minutes to remove water.

[0052] Step S4, continue heating and keeping warm, cool to room temperature, precipitate, separate, and wash to obtain the titanium-based alkali metal fluoride inorganic nanomaterial.

[0053] In the step S4,

[0054] Continue heating to 260-320° C. under the protection of inert gas and keep the temperature for 30-60 minutes before naturally cooling to room temperature. The solvent used to precipitate the titanium-based alkali metal fluoride inorganic nanomaterial is selected from one or more of ethanol, methanol and water.

[0055] According to another typical implementation of the embodiments of the present invention, there is provided a titanium-based alkali metal fluoride inorganic nanomaterial obtained by the method.

[0056] According to another typical implementation of the embodiments of the present invention, there is provided application of the titanium-based alkali metal fluoride inorganic nanomaterial in cancer sonodynamic therapy.

[0057] The synthetic method is easy to control and has good reproducibility. The prepared nanomaterials have good dispersion, uniformity and reproducibility. They combine with oxygen in cells under ultrasonic radiation to produce singlet oxygen ( 1 O 2 ), thereby achieving the effect of sonodynamic therapy for cancer. The nanomaterial has good biosafety due to its low cytotoxicity and biotoxicity, making the inorganic nanomaterial of the present invention have good application prospects in sonodynamic therapy for cancer.

[0058] The following is a detailed description of a method for preparing a fluorescent nanomaterial of the present application in combination with embodiments, comparative examples and experimental data.

[0059] Example 1

[0060] A method for preparing an inorganic nanomaterial for cancer sonodynamic therapy comprises the following steps:

[0061] (1) At room temperature, add 146 μL of titanium acetylacetonate, 5 mL of oleic acid, and 10 mL of octadecene into a 100 mL three-necked flask;

[0062] (2) The solution was heated to 100°C and vacuumed to remove oxygen and water. 2 Under protection, the solution was heated to 130 °C and stirred for 60 min;

[0063] (3) After cooling to room temperature, 2 mL of methanol solution containing 72 mg of NaOH and 5 mL of methanol solution containing 66.7 mg of NH 4 F methanol solution; heating the solution to 70°C to remove methanol; continuing to heat the solution to 100°C, and vacuuming to remove oxygen and water;

[0064] (4)N 2 Under protection, the solution was heated to 280°C and stirred rapidly for 1 hour. After the reaction was completed, ethanol was added for precipitation and centrifuged at 10000 rpm for 10 minutes to separate Na 3 TiF 6 NPs, namely titanium-based alkali metal fluoride inorganic nanomaterials.

[0065] Example 2

[0066] A method for preparing an inorganic nanomaterial for cancer sonodynamic therapy comprises the following steps:

[0067] (1) At room temperature, add 33 μL of titanium tetrachloride, 5 mL of oleic acid, and 15 mL of octadecene into a 100 mL three-necked flask;

[0068] (2) The solution was heated to 100°C and vacuumed to remove oxygen and water. 2 Under protection, the solution was heated to 140 °C and stirred for 60 min;

[0069] (3) After cooling to room temperature, 2 mL of methanol solution containing 72 mg of NaOH and 5 mL of methanol solution containing 74 mg of NH 4 F methanol solution; heating the solution to 70°C to remove methanol; continuing to heat the solution to 100°C, and vacuuming to remove oxygen and water;

[0070] (4)N 2 Under protection, the solution was heated to 300°C and stirred rapidly for 1 hour. After the reaction was completed, ethanol was added for precipitation and centrifuged at 10000 rpm for 10 minutes to separate Na 3 TiF 6 NPs, namely titanium-based alkali metal fluoride inorganic nanomaterials.

[0071] Example 3

[0072] A method for preparing an inorganic nanomaterial for cancer sonodynamic therapy comprises the following steps:

[0073] (1) At room temperature, add 102 μL of butyl titanate, 5 mL of oleic acid, and 5 mL of octadecene into a 100 mL three-necked flask;

[0074] (2) The solution was heated to 100°C and vacuumed to remove oxygen and water.2 Under protection, the solution was heated to 150°C and stirred for 40 min;

[0075] (3) After cooling to room temperature, 2 mL of methanol solution containing 72 mg of NaOH and 5 mL of methanol solution containing 111 mg of NH 4 F methanol solution; heating the solution to 70°C to remove methanol; continuing to heat the solution to 100°C, and vacuuming to remove oxygen and water;

[0076] (4)N 2 Under protection, the solution was heated to 320°C and stirred rapidly for 30 minutes. After the reaction was completed, methanol was added for precipitation and centrifuged at 10000 rpm for 10 minutes to separate Na 3 TiF 6 NPs, namely titanium-based alkali metal fluoride inorganic nanomaterials.

[0077] Example 4

[0078] A method for preparing an inorganic nanomaterial for cancer sonodynamic therapy comprises the following steps:

[0079] (1) At room temperature, add 48 mg of titanyl sulfate, 5 mL of oleic acid, and 10 mL of octadecene into a 100 mL three-necked flask;

[0080] (2) The solution was heated to 100°C and vacuumed to remove oxygen and water. 2 Under protection, the solution was heated to 160°C and stirred for 30 min;

[0081] (3) After cooling to room temperature, 2 mL of methanol solution containing 72 mg of NaOH and 5 mL of methanol solution containing 66.7 mg of NH 4 F methanol solution; heating the solution to 70°C to remove methanol; continuing to heat the solution to 100°C, and vacuuming to remove oxygen and water;

[0082] (4)N 2 Under protection, the solution was heated to 320°C and stirred rapidly for 1 hour. After the reaction was completed, pure water was added to settle and centrifuged at 10000 rpm for 10 minutes to separate Na 3 TiF 6 NPs, namely titanium-based alkali metal fluoride inorganic nanomaterials.

[0083] Experimental Example 1

[0084] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6NPs were analyzed by X-ray diffraction. The specific test steps are: take 200μL of sample solution with a concentration of 5mg / mL and drop it on a glass slide, and then perform X-ray diffraction test after the sample is dried. The image is as follows Figure 1 As shown in the figure, it can be seen that the nanomaterial has good crystallinity, and its diffraction peak position and relative intensity are similar to those of Na 3 TiF 6 The PDF standard card (JCPDS No.26-1491) is consistent and belongs to the orthorhombic system.

[0085] Experimental Example 2

[0086] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were analyzed by X-ray photoelectron spectroscopy. The specific test steps are: take 2mL of sample solution with a concentration of 5mg / mL in an EP tube, and after the sample is vacuum dried, perform X-ray photoelectron spectroscopy test. The image is as follows Figure 2 As shown in the figure, it can be seen that the nanomaterial contains three elements: Na, Ti, and F, and the narrow spectrum of Ti 2p orbitals conforms to the titanium fluoride spectrum.

[0087] Experimental Example 3

[0088] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were photographed under a transmission electron microscope. The specific test steps are: take 10 μL of a sample solution with a concentration of 0.05 mg / mL and drop it on a copper grid. After the sample is dried, perform a morphology test. Figure 3 As shown in the figure, it can be seen that the nanomaterial has an obvious spherical structure, uniform size and good dispersion, and its particle size is about 5nm.

[0089] Experimental Example 4

[0090] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were photographed under a transmission electron microscope. The specific test steps are: take 10 μL of a sample solution with a concentration of 0.05 mg / mL and drop it on a copper grid. After the sample is dried, perform a morphology test. Figure 4 As shown in the figure, it can be seen that the nanomaterial has an obvious spherical structure, uniform size and good dispersion, and its particle size is about 30nm.

[0091] Experimental Example 5

[0092] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF6 NPs were photographed under a transmission electron microscope. The specific test steps are: take 10 μL of a sample solution with a concentration of 0.05 mg / mL and drop it on a copper grid. After the sample is dried, perform a morphology test. Figure 5 As shown in the figure, it can be seen that the nanomaterial has an obvious spherical structure, uniform size and good dispersion, and its particle size is about 15nm.

[0093] Experimental Example 6

[0094] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were photographed under a transmission electron microscope. The specific test steps are: take 10 μL of a sample solution with a concentration of 0.05 mg / mL and drop it on a copper grid. After the sample is dried, perform a morphology test. Figure 6 As shown in the figure, it can be seen that the nanomaterial has an obvious spherical structure, uniform size and good dispersion, and its particle size is about 10nm.

[0095] Experimental Example 7

[0096] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were subjected to ESR oxygen vacancies determination. The specific test steps were as follows: 20 mg of vacuum-dried Na 3 TiF 6 ESR oxygen vacancy test of NPs powders and comparison with commercial TiO 2 For comparison. Figure 7 As shown in the figure, it can be seen that Na 3 TiF 6 NPs than commercial TiO 2 With more oxygen vacancies, abundant oxygen vacancies can act as electron traps to prevent the recombination of electrons and holes.

[0097] Experimental Example 8

[0098] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were subjected to electrochemical impedance spectroscopy. The specific test steps were as follows: 3 TiF 6 NPs powder was dissolved in a mixed solution of ethanol, naphthol and water, 100 μL of the mixed solution was dropped on the nickel foam, and then the electrochemical impedance spectroscopy test was performed after vacuum drying. Figure 8 As shown in the figure, it can be seen that Na 3 TiF 6 NPs have better performance than commercial TiO2 Smaller semicircle diameter indicates Na 3 TiF 6 NPs have lower impedance for charge transfer and higher charge separation.

[0099] Experimental Example 9

[0100] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 NPs were tested for ultrasonic response current spectrum. The specific test steps were as follows: 3 TiF 6 NPs powder was dissolved in a mixed solution of ethanol, naphthol and water, 100 μL of the mixed solution was dropped on the nickel foam, and then vacuum dried and the ultrasonic response current spectrum was tested. Fig. 9 As shown in the figure, Na 3 TiF 6 NPs have better performance than commercial TiO 2 The larger ultrasound response current indicates that Na 3 TiF 6 The electron-hole pairs of NPs are easier to separate under ultrasonic conditions and the separation efficiency is higher.

[0101] Experimental Example 10

[0102] The titanium-based alkali metal fluoride inorganic nanomaterial Na 3 TiF 6 The rate of DPBF probe oxidation under ultrasound was determined for the NPs and compared with commercial TiO 2 Compared with water. Fig.10 As shown in the figure, it can be seen that at the same concentration, Na 3 TiF 6 NPs have better performance than commercial TiO 2 Faster DPBF probe oxidation rate; in the same time, Na 3 TiF 6 The NPs group was able to produce more than commercial TiO 2 More ROS causes the UV absorption of the DPBF probe to decrease further.

[0103] Experimental Example 11

[0104] The titanium-based alkali metal fluoride inorganic nanomaterial Na containing Example 1 3 TiF 6 Mouse breast cancer 4T1 cells were cultured in 1640 culture medium containing NPs (50 μg / mL) and in 5% CO 2After incubation in a 37°C incubator for 12 h, ROS probe (DCFH-DA) (50 μM) was added for ultrasonic stimulation. Fluorescence imaging was performed after rinsing three times with PBS buffer solution. The experiment was divided into an experimental group and a blank control group. Fig.11 As can be seen from the cell imaging pictures, Na 3 TiF 6 NPs can generate ROS in tumor cells under ultrasound stimulation.

[0105] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0106] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0107] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A method for preparing an inorganic nanomaterial for cancer sonodynamic therapy, characterized in that: The following steps are involved: S1, mixing the titanium-containing precursor and the high boiling point solvent uniformly to obtain a reaction solution; S2, heating and keeping the reaction solution warm under an inert atmosphere to decompose the precursor in the reaction solution to obtain a mixed solution; S3, cooling the obtained mixed solution to room temperature under an inert atmosphere, adding a methanol solution containing ammonium fluoride and an alkali metal hydroxide, and then removing methanol and water; S4. Continue heating and keeping warm under an inert atmosphere until the reaction is complete, then cool to room temperature, precipitate, separate, and wash the product to obtain the titanium-based alkali metal fluoride inorganic nanomaterial.

2. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In the step S1, the titanium-containing precursor is selected from one or more of titanium acetylacetonate, titanyl sulfate, titanium chloride, and butyl titanate.

3. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In the step S1, the high boiling point solvent is selected from one or more of oleic acid, oleylamine, and octadecene.

4. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In the step S2, the reaction solution is heated to 120-160° C. under the protection of an inert gas, and the temperature is kept until the precursor in the reaction solution is decomposed.

5. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In step S3, the molar ratio of ammonium fluoride to alkali metal hydroxide is 1:1-5.

6. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In step S3, the operation of removing methanol and water is: heating the reaction system to 120-160° C. under the protection of inert gas, and keeping the temperature to remove methanol and water.

7. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In the step S4, the temperature is heated to 260-320° C. and kept warm until the reaction is completed.

8. The method for preparing inorganic nanomaterials for cancer sonodynamic therapy according to claim 1, characterized in that: In the step S4, the solvent used to precipitate the titanium-based alkali metal fluoride inorganic nanomaterial is selected from one or more of ethanol, methanol and water.

9. An inorganic nanomaterial for sonodynamic cancer therapy, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. Use of the titanium-based alkali metal fluoride inorganic nanomaterial as claimed in claim 9 in cancer sonodynamic therapy.