Nickel sulfide / cobalt sulfide composite material and preparation method and application thereof
The Ni3S4/Co3S4 composite material is prepared by the semi-liquid phase sintering method, which solves the problem of excessive material size caused by the solid-phase sintering method, achieves high specific capacity and excellent electrochemical performance, and is suitable for supercapacitors.
Patent Information
- Application Number
- CN202410915705.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-11
AI Technical Summary
When the existing solid-phase sintering method is used to prepare nickel-cobalt-based bimetallic sulfide, the material size is larger and densified, which cannot meet the needs of supercapacitors for nanoscale materials and affects the electrochemical performance.
Using the semi-liquid phase sintering method, sodium chloride is added as an additive at low temperature to form a liquid or molten state, breaking the solid-solid phase boundary, accelerating the reaction, and generating a skeleton-like Ni3S4/Co3S4 composite material.
Porous nickel sulfide/cobalt sulfide composite materials with particle diameters of 50-200 nm were successfully prepared, which improved the specific capacity, rate performance and cycle stability of the supercapacitor. The cost is low, the method is simple, and it is suitable for industrial production.
Smart Images

Figure CN118754218A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nano material preparation, and specifically relates to a nickel sulfide / cobalt sulfide composite material and a preparation method and application thereof. Background Art
[0002] With the rapid development of energy devices, the demand for reusable high-power equipment is gradually increasing. Among the existing energy storage devices, the power density provided by supercapacitors is most suitable for high-power applications, but they are all limited by energy density. Transition metal sulfides, especially nickel-cobalt-based bimetallic sulfides, are widely considered to be a way to solve the energy density of supercapacitors because of their excellent electrochemical properties. Nickel-cobalt-based bimetallic sulfides have richer valence state transformations than monometallic sulfides, which can improve electron transfer efficiency and accelerate redox reactions in pseudocapacitors; and compared with monometallic sulfides, bimetallic sulfides have coupled redox reactions and even synergistic effects. Most scientific research believes that the reason for the synergistic effect is that a heterostructure is constructed between the bimetallics. However, not all heterostructures will play a positive role in electrochemical performance. Therefore, it is necessary to design a nickel-cobalt-based bimetallic sulfide heterostructure that is most suitable for supercapacitors.
[0003] At present, researchers have synthesized nickel-cobalt-based bimetallic sulfides through many methods, such as: hydrothermal method (solvothermal method), solid-phase sintering method (high-temperature sulfurization method), microwave-assisted method, electrodeposition method, molten salt method, NaCl-assisted method, ion exchange method, etc. The above methods have their own advantages and disadvantages, but only solid-phase sintering is the most suitable for mass production. Moreover, solid-phase sintering is the most stable way to produce materials with thermodynamic properties. This is because at high temperatures, the solid-phase reactant elements begin to diffuse, the particles are bonded, the voids and grain boundaries gradually decrease, and the grains gradually grow, which makes the crystal structure of the material under solid-phase reaction regular and highly crystalline, making the material have excellent stability. But it is precisely because of the reduction of voids and grain boundaries in the solid-phase reaction that the reactants often present a densified form, making the size of the solid-phase reaction product at the micron level. For example: Chen et al. used nickel powder, cobalt powder and sulfur powder to react at high temperature in a tubular furnace, and finally obtained Ni 0.5 Co 0.5S2. This is a material with extremely stable thermodynamic properties, but the material size distribution is around 3.7-21.4um, which is not suitable for supercapacitors. In addition, in the field of energy storage, many research results have proved that the original performance of the material will change significantly after the size changes from the micron level to the nanometer level. First, the specific surface area of nanomaterials will increase as the size decreases due to surface effects. The ion radius of the electrolyte in the aqueous solution of the supercapacitor is about 0.5nm. Therefore, the presence of mesopores will improve the electrochemical performance from both the double layer and pseudocapacitance. Secondly, nanomaterials are affected by quantum effects, and their original continuous Fermi level will be discretized, which greatly changes the original conductivity. Many studies have shown that the conductivity of bimetallic sulfides will increase after the Fermi level is discretized. In summary, how to obtain smaller materials while maintaining the original advantages of solid-phase sintering is a crucial issue. Summary of the invention
[0004] In order to solve the technical problem that the material is often in the micrometer level due to the growth of grains and the reduction of voids in solid phase sintering, the present invention proposes a nickel sulfide / cobalt sulfide composite material and its preparation method and application. A semi-liquid phase sintering method is proposed to overcome the serious densification problem in solid phase sintering.
[0005] To achieve the above object, the technical solution of the present invention is implemented as follows:
[0006] A method for preparing a nickel sulfide / cobalt sulfide composite material, comprising the following steps:
[0007] (1) nickel acetate tetrahydrate and cobalt acetate tetrahydrate are mixed, distilled water is added, and the mixture is stirred in a constant temperature mixer until it is in a hydrogel state; the mixture is then placed in liquid nitrogen and frozen in a vacuum freeze dryer at -50 to -25°C for 12 to 24 hours to obtain a precursor;
[0008] (2) The precursor prepared in step (1) is fully ground with sodium chloride and sodium thiosulfate pentahydrate to obtain a mixture. Sodium chloride, as an additive, has the advantages of high melting point and stability.
[0009] (3) spreading the mixture obtained in step (2) in a porcelain boat and sintering it in a protective atmosphere to obtain a black block product;
[0010] The environment of the tube furnace allows the material to complete the solid-semi-liquid-solid transformation during sintering.
[0011] (4) The black block product obtained in step (3) is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain a nickel sulfide / cobalt sulfide composite material, recorded as Ni3S4 / Co3S4.
[0012] In the above step (1), the molar ratio of nickel acetate tetrahydrate to cobalt acetate tetrahydrate is (1-9): (1-9).
[0013] In the above step (2), the mass ratio of the precursor, sodium thiosulfate pentahydrate and sodium chloride is 0.49:(0.5-1.5):(0.5-1.5).
[0014] The sintering conditions in the above step (3) are: heating rate of 5-10°C / min, sintering temperature of 50-200°C, and time of 30min-12h.
[0015] The semi-liquid phase sintering method proposed in the present invention mainly includes the following three steps: (1) the reaction material should be added with non-reactive additives before sintering and dispersed as much as possible. (2) the reactants need to undergo a preliminary reaction (to produce a liquid phase or a molten state) at a low temperature. (3) the additives must first have sufficient stability and must remain stable in the early dispersion stage, the mid-term preliminary reaction stage, and the final sintering process. Secondly, the additives need to be able to melt or dissociate in the preliminary reaction so as to have a deep contact with the reactants so as to play a filler role in the subsequent sintering. Finally, the additives can be precipitated by washing or other means. In addition to the fact that the reactants can produce a liquid phase (molten state) at a low temperature to achieve the purpose of contact, the addition of the liquid phase also breaks the original solid-solid phase boundary to accelerate the synthesis rate of the reaction. Subsequently, metal salts and thiosulfate are selected as reaction salts, and sodium chloride is selected as additives. In addition to the fact that the reactants can produce a liquid phase (molten state) at a low temperature to achieve the purpose of contact, the addition of the liquid phase also breaks the original solid-solid phase boundary to accelerate the synthesis rate of the reaction. Sodium chloride (additive) can provide mesoporous pores for the material, increase the specific surface area and enrich the active sites. Based on Le Chatelier's principle, the presence of acetate and water will generate acetic acid and hydroxide. Sodium thiosulfate pentahydrate decomposes sulfur element when heated under acidic conditions, and sulfur element will oxidize a part of the metal ions to generate divalent sulfur ions and trivalent metal ions. In this process, the crystalline phases of nickel sulfide and cobalt sulfide are not directly synthesized during the combination of metal ions and sulfur ions, but Ni3S4 / Co3S4 is synthesized in one step. The synthesized Ni3S4 / Co3S4 is assembled with activated carbon electrodes into supercapacitor devices that exhibit high specific capacity and extremely high energy density.
[0016] The nickel sulfide / cobalt sulfide composite material is prepared by the above preparation method.
[0017] The nickel sulfide / cobalt sulfide composite material is in a skeleton-like shape, and the particle diameter is 50-200nm.
[0018] Application of the above nickel sulfide / cobalt sulfide composite material in supercapacitors.
[0019] A supercapacitor comprises a counter electrode, a diaphragm, an electrolyte and a Ni3S4 / Co3S4 electrode. The Ni3S4 / Co3S4 electrode comprises a conductive agent, a binder and the nickel sulfide / cobalt sulfide composite material.
[0020] The assembly steps of the above-mentioned supercapacitor are:
[0021] (1) Preparation of Ni3S4 / Co3S4 electrode: The prepared Ni3S4 / Co3S4, conductive agent and binder were weighed in a mass ratio of 8:1:1 and placed in a 10 mL beaker, and a Ni3S4 / Co3S4 electrode was prepared by slurrying, coating, drying, and tableting.
[0022] (2) Preparation of counter electrode: Activated carbon and binder were weighed in a mass ratio of 9:1 and placed in a 10 mL beaker, and an activated carbon counter electrode was prepared by slurrying, coating, drying, and tableting.
[0023] (3) Assembly of supercapacitor device: The Ni3S4 / Co3S4 electrode, non-woven fabric separator and counter electrode are laminated together and placed in a suitable container. An appropriate amount of KOH aqueous solution is injected as an electrolyte. The container is then sealed with paraffin to obtain a supercapacitor containing Ni3S4 / Co3S4 electrode materials.
[0024] The beneficial effects produced by the present invention are:
[0025] (1) The present invention proposes a method for preparing nickel sulfide / cobalt sulfide composite electrode materials by a semi-liquid phase sintering method, wherein nickel acetate tetrahydrate and cobalt acetate tetrahydrate are used as nickel salt and cobalt salt respectively, water is added and mixed to a hydrogel state, and then placed in liquid nitrogen to freeze to a solid state and freeze-dried to obtain a precursor powder; then the precursor powder is evenly ground with sodium chloride and sodium thiosulfate pentahydrate, and then calcined at high temperature, washed and dried to obtain a Ni3S4 / Co3S4 composite material. The precursor is solid and layered by liquid nitrogen freezing and freeze-drying. In addition to the reactants being able to produce a liquid phase at low temperature to achieve the purpose of contact, the addition of the liquid phase also breaks the original solid-solid phase boundary to accelerate the synthesis rate of the reaction. Subsequently, acetate (nickel acetate tetrahydrate, cobalt acetate tetrahydrate) and thiosulfate are selected as reaction salts, and sodium chloride is used as an additive. In addition to the reactants being able to produce a liquid phase at low temperature to achieve the purpose of contact, the addition of the liquid phase also breaks the original solid-solid phase boundary to accelerate the synthesis rate of the reaction. Sodium chloride (additive) can provide mesoporous pores for the material, increase the specific surface area and enrich the active sites. Based on Le Chatelier's principle, the presence of acetate and water will generate acetic acid and hydroxide. Sodium thiosulfate pentahydrate decomposes sulfur element when heated under acidic conditions, and sulfur element will oxidize a part of the metal ions to generate divalent sulfur ions and trivalent metal ions. In this process, the crystalline phases of nickel sulfide and cobalt sulfide are not directly synthesized during the combination of metal ions and sulfur ions, but Ni3S4 / Co3S4 is synthesized in one step. The directly synthesized Ni3S4 / Co3S4 is assembled with activated carbon electrodes into supercapacitor devices, which show high specific capacity and extremely high energy density.
[0026] (2) During the sintering process of the present invention, crystal water will precipitate from the metal salt and thiosulfate. This will also cause the sintering to enter the second stage (semi-liquid phase stage). At the beginning of the semi-liquid phase stage, 0.5mmol of metal salt and 1mmol of thiosulfate will first precipitate 7mmol of water. As the temperature rises, 7mmol of water will melt all the thiosulfate, metal salt and sodium chloride. The addition of liquid not only breaks the original solid-solid interface and greatly accelerates the reaction process, but also allows sodium chloride to be fully dissolved in the two salts, which provides the necessary conditions for the emergence of mesopores in the later stage. Thiosulfate can only decompose sulfide ions and sulfur element under acidic conditions. Therefore, the present invention uses acetate as the metal salt to generate an acidic environment. The emergence of the acidic environment represents that the semi-liquid phase has entered the second step of the reaction. At this stage, the acidic environment will gradually decompose thiosulfate. Specifically, in an acidic environment, sodium thiosulfate pentahydrate will decompose sulfur element, and sulfur element will oxidize a part of the metal ions to generate sulfide ions and trivalent metal ions. Adding liquid phase to solid phase sintering can greatly accelerate the sintering reaction. After the semi-liquid phase environment ends, the decomposition reaction of thiosulfate is basically over. The reaction enters the third sintering state. In this process, the additives begin to play a role, and the fully integrated sodium chloride will be in full contact with the sulfide grains. NC82 SEM characterization was carried out under the conditions of sintering at 150℃ for 2h, 6h, and 12h. By comparing with and without additives, it can be clearly observed that the material containing sodium chloride will present a smaller size and rich mesopores. The Ni3S4 / Co3S4 composite material prepared by semi-liquid phase sintering is porous granular with a particle diameter of 50-200nm.
[0027] (3) The asymmetric supercapacitor device assembled from the nickel sulfide / cobalt sulfide composite material prepared by the present invention has high specific capacity, excellent rate performance and outstanding cycle stability. -1 At a current density of 1.5 %, the device has a specific capacity of up to 650 F g -1 , at 5Ag -1 The capacity retention rate after 9,000 cycles at a current density of about 89.6% and the coulombic efficiency of about 95%. In addition, the preparation cost of the composite material is low, the method is simple, environmentally friendly, and efficient, making it easier to scale up industrially to solve practical application problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 It is a schematic diagram of preparing a skeleton-like Ni3S4 / Co3S4 composite material by the semi-liquid phase sintering method of the present invention.
[0030] Figure 2 SEM images of precursors prepared by different freeze-drying methods; (ab) are refrigerator freeze-drying, and (cd) are nitrogen freeze-drying.
[0031] Figure 3 (a) is the XRD pattern of thiosulfate before and after sintering at 150°C for 2h; (b) is the pH value of the reaction product after dissolving in deionized water; (c) is the in-situ video of the reactants in the semi-liquid reaction; (d) is the XRD pattern when sintered at 70-150°C for 2min without washing; (e) is the XRD pattern when sintered at 150°C for 12h without introducing NaCl and without washing; (f) is the XRD pattern after sintering at 150°C, 350°C and 550°C for 2h and washing.
[0032] Figure 4 These are parallel experiments of acetic acid and sodium thiosulfate, where (a) is a photograph of the formation of elemental sulfur observed after sintering at 150°C for 30 min; (bd) are photographs of the formation of elemental sulfur in parallel experiments of acetic acid and sodium thiosulfate.
[0033] Figure 5 These are the SEM and TEM images of NC82 prepared in Example 1 of the present invention, wherein: (ac) FESEM images of NC82 at different magnifications; (dg) element distribution diagrams of NC82; (h) TEM image of NC82; (i) HRTEM image of NC82; and (j) corresponding selected area diffraction patterns.
[0034] Figure 6 These are FESEM images of the composite materials prepared in Comparative Example 1, Example 2 and Example 3 of the present invention, wherein (ac) are FESEM images of NC010; (df) are FESEM images of NC19; and (gi) are FESEM images of NC28.
[0035] Figure 7 These are FESEM images of the nickel sulfide / cobalt sulfide composite materials prepared in Examples 4-6 of the present invention, wherein: (ac) FESEM images of NC37; (df)) FESEM images of NC46; and (gi) FESEM image of NC55.
[0036] Figure 8 These are FESEM images of the nickel sulfide / cobalt sulfide composite materials prepared in Examples 7-9 of the present invention, wherein: (ac) FESEM images of NC64; (df)) FESEM images of NC73; and (gi) FESEM image of NC91.
[0037] Fig. 9 These are FESEM images of the material prepared in Comparative Example 2, where (ac) are FESEM images of NC100 at different magnifications.
[0038] Fig.10 These are FESEM images of nickel sulfide / cobalt sulfide composite materials prepared in Examples 1, 10, 11 and Comparative Examples 3-5.
[0039] Fig.11 Electrochemical properties of different electrode materials, including: (a) CV curve of NC100 at different scan rates; (b) CV curve of NC55 at different scan rates; (c) CV curve of NC82 at different scan rates; (d) discharge time diagram of the three materials at different current densities; (e) discharge time diagram of NC82 at different current densities; (f) specific capacity diagram of NC55, NC82 and NC100 at different current densities at 0.5V, 2mol KOH.
[0040] Fig.12 Electrochemical performance of asymmetric supercapacitors, including (a) CV test of NC82 / / AC at different scan rates; (b) discharge time of NC82 / / AC at different current densities; (c) constant current charge and discharge test of different supercapacitors at different current densities; (d) Ragon diagram; (e) 5Ag -1 Long cycle test under . DETAILED DESCRIPTION
[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0044] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0045] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.997 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0046] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0047] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC82.
[0048] Figure 1 This is a schematic diagram of the preparation of porous granular nickel sulfide / cobalt sulfide composite materials by a semi-liquid phase sintering method, which mainly includes two steps: 1. Pre-preparation of metal raw materials; 2. Sintering. In order to avoid the situation where metal ions are too aggregated and do not react with sulfide ions, it was chosen to first disperse them. Specifically, nickel acetate and cobalt acetate were first prepared into aqueous solutions, and then dispersed by stirring at 80°C. Then liquid nitrogen and refrigerator freezing were used respectively. The difference between liquid nitrogen cooling and refrigerator cooling was observed by scanning electron microscopy. It is not difficult to see that both methods make the metal salts appear in solid lamellar form. Liquid nitrogen cooling is more likely to form larger flakes than refrigerator cooling. This is mainly because more crystalline water is preserved after freeze-drying with liquid nitrogen ( Figure 2 ). The obtained precursor (powdered product) was then fully ground with sodium thiosulfate pentahydrate and sodium chloride into powder. The powder was then poured into a porcelain boat for sintering. In order to explore the specific reaction process, the materials in the porcelain boat were observed at different time temperatures and time periods. It is not difficult to see that the color of the material changes from white to green and finally to black as the temperature rises. This is mainly because the crystal water in the metal salt and thiosulfate is precipitated. This will also cause the sintering to enter the second stage (semi-liquid phase stage). At the beginning of the semi-liquid phase, 0.5mmol metal salt and 1mmol thiosulfate will first precipitate 7mmol water. 7mmol water will melt all thiosulfate, metal salt and sodium chloride as the temperature rises. This is mainly because acetate and sodium chloride are not soluble enough at room temperature, but their solubility will increase with the increase of temperature. The addition of liquid not only breaks the original solid-solid interface and greatly accelerates the reaction process, but also allows sodium chloride to be fully dissolved in the two salts, which provides the necessary conditions for the appearance of mesopores in the later stage.
[0049] In order to verify the hypothesis based on Le Chatelier's principle, thiosulfate was sintered at 150℃ for 2h. XRD showed that thiosulfate was sintered at 150℃ for 2h only to separate crystal water without any reaction ( Figure 3a). This verifies that thiosulfate usually decomposes into sulfide ions or sulfur under acidic or high temperature conditions. According to Le Chatelier's principle, if the conditions of a reversible reaction are changed, the chemical equilibrium is destroyed and moves in the direction of weakening this change. Because acetate cannot be completely hydrolyzed in water, in theory, some acetic acid and hydroxide will be generated. In order to verify this, the following experiments were conducted. First, after the sintering is completed, there is often an acetic acid smell at the outlet of the tube furnace. But this does not fully prove the presence of acetic acid. Then, it is raised to 120℃ at a rate of 5℃ / min and maintained for 5min, and taken out directly without cooling after the end. The material in the porcelain boat can be clearly felt to be similar to a gel-like liquid by scraping it with a medicine spoon, but the granularity is obvious. The material scratched on the medicine spoon will solidify in just a few seconds and complete the transition from semi-liquid phase to solid. At the same time, the material becomes extremely hard. The drops of liquid and green traces at the bottom of the porcelain boat will also quickly turn into solids. Then 10mL of deionized water is added to the porcelain boat, and the pH value is found to be around 4-5 by acid-base titration ( Figure 3 b) This is mainly because the acetate is not completely hydrolyzed during hydrolysis to generate acetic acid. After the sample is taken out, the acetic acid is exposed to air, and part of the acetic acid volatilizes, producing an acetic acid smell. The volatilized acetic acid causes the material to solidify. The final material solidification phenomenon and pH value also prove this point.
[0050] The emergence of an acidic environment means that the semi-liquid phase enters the second step of the reaction. In this reaction, the semi-liquid phase formed by water and acetic acid plays an important role. Figure 3 It is not difficult to see in c that the entire reaction system is very rapid. The system begins to hydrolyze at 90°C. Acetate produces acetic acid and hydroxide from hydrolysis. Two minutes later, the temperature reaches 110°C, and a distinct green color appears. This color is mainly due to the generated hydroxide. At this time, acetic acid appears along with hydroxide. The appearance from green to black is almost synchronous. This means that the three of acetic acid, sodium thiosulfate reaction and hydroxide appear at the same time. At this time, the system has reached the second equilibrium point. Because sodium thiosulfate will decompose into sulfur, sulfide ions and sodium sulfate when pH is less than 4.2. Among them, S decomposed from sodium thiosulfate 2- It generally exists in the form of hydrogen sulfide. However, due to the presence of nickel hydroxide, before hydrogen sulfide is generated, the decomposed hydrogen ions will coordinate with the hydroxide ions of nickel hydroxide to re-form water. 2- and M 2+ (M stands for "Ni orCo") to form a sulfide without a crystalline phase. The separated sulfur will combine with a part of M 2+ Oxidation-reduction reaction occurs to form M 3+ and S 2- . M 2+ 、M 3+ Will and S 2-React together to form M3S4. When M3S4 is formed, it reaches the third equilibrium point. At this time, the system will return to the first step to regenerate acetic acid and hydroxide. This is also the reason why there is no sulfur adhesion on the tin foil after wrapping it tightly with high-temperature tape. Therefore, a parallel experiment with acetic acid and sodium thiosulfate was conducted ( Figure 4 ). The light yellow substance floating on the surface of the beaker indicates the presence of sulfur. The light white substance at the bottom of the beaker indicates the presence of sodium acetate. However, the formed M3S4 does not directly produce a crystalline phase. On the contrary, after reaching the third equilibrium point, the phases in the entire system began to gradually decompose until the water disappeared. In order to verify the dynamic equilibrium of these three points. We tested its XRD under the conditions of sintering at 70-150℃ for 2min. The XRD results clearly show that the peaks of acetate and thiosulfate gradually weakened. And no crystalline phase appeared after 130℃ ( Figure 3 d). In order to prove that the sodium thiosulfate and acetate in the material were not completely decomposed, XRD was tested after sintering at 150℃ for 12h without washing. Figure 3 e). XRD results confirmed the speculation about sodium thiosulfate. Considering the presence of acetate, sodium thiosulfate will decompose sulfur and sodium sulfite at 310℃, and the two may re-coordinate under high temperature pyrolysis to form a new crystalline phase. Sintered at 150℃, 350℃ and 550℃ for 2h, and then washed and tested XRD ( Figure 3 f). XRD results show that the material will have a composite phase of M3S4 and MS at 350℃, and will turn back into M3S4 and residual MS at 550℃. This proves that our guess is correct. The existence of the semi-liquid phase plays an important role in the whole reaction process. While breaking the original solid-solid interface, it also plays an important role in the formation of dynamic equilibrium.
[0051] After the semi-liquid phase environment ends, the decomposition reaction of thiosulfate is basically over. The reaction officially enters the third sintering state. In this process, additives begin to play a role. The fully integrated sodium chloride will be in full contact with the sulfide grains. NC82 SEM characterization under the conditions of sintering at 150℃ for 2h, 6h, and 12h. By comparing with and without additives, it can be clearly observed that the material containing sodium chloride will have a smaller size and abundant mesopores.
[0052] Figure 5 a is the FESEM image of NC82 at 10um size. Figure 5 b and Figure 5 c shows that Figure 5 a is composed of a skeleton-like framework. Figure 5It is not difficult to see in b that the pores in the skeleton are large and small. This is because the NaCl added during the reaction does not participate in the reaction. Due to the stability of NaCl itself and its friction agent properties, the grains that should have been bonded and grown during the sintering process are blocked by the dispersed NaCl. However, since NaCl cannot be dispersed at the nanometer level in the gaps of each reactant, the resulting particles are of different sizes. Figure 5 As shown in c, the particle size of Ni3S4 / Co3S4 is 50-200nm. These particles of different sizes can just bring about pores of different sizes. This makes it easier for the electrolyte to contact the material through these pores, increasing the reactive sites. Figure 5 From the element distribution diagram of (dg), it can be seen that the three elements Ni, Co, and S are evenly distributed in the material, which just illustrates the necessity of precursor preparation. Because nickel acetate and cobalt acetate are difficult to be ground and dispersed without using a ball mill. After synthesizing the precursor, nickel acetate and cobalt acetate are hydrolyzed by heating in water, and the subsequent stirring can make the nickel and cobalt well dispersed. It is not difficult to find from the ternary phase diagram of water that rapid freezing using liquid nitrogen can retain more water during the vacuum freeze-drying process than putting it in a refrigerator for braking. These water can provide the necessary liquid phase in the subsequent reaction environment. The TEM image also further illustrates that the material itself is a skeleton-like stacking formation, which is consistent with the SEM image ( Figure 5 h). The depth of the color indicates that the material has different contents at that point. The TEM image shows that the material has a variety of pores, which exposes a large number of active sites and contributes to the excellent performance of this composite material. The high-resolution TEM (HRTEM) image of NC82 shows clear light and dark lattice fringes in different directions, with clear lattice distortion interfaces between them ( Figure 5 i). The crystal plane with a spacing value of 0.272nm can be assigned to the (2 2 2) crystal plane of Ni3S4; the crystal plane of 0.272nm can be pointed to the (2 2 2) crystal plane of Co3S4. In addition, the close adhesion between Ni3S4 and Co3S4 forms a cross interface (red area), and the interfacial synergy is expected to directly enhance the electrochemical behavior. This also provides direct evidence for the heterostructure of Ni3S4@Co3S4. The intersection interface between the red line and the black line is due to the lattice distortion caused by the distortion and rearrangement of the corresponding crystal planes during the sintering process. This also provides strong evidence for the emergence of heterostructures. The structure, crystal phase and crystal defect characteristics of the material were analyzed by electron diffraction. Selected area electron diffraction (SAED) image ( Figure 5j) The clear and bright diffraction rings with lattice characteristics can be attributed to the (1 1 1), (2 2 0), (2 2 2), (4 00), (4 2 2), (2 2 0) and (4 4 0) crystal planes of Ni3S4. However, Co3S4, due to its weak crystallinity, showed diffraction spots in SAED, but a few diffraction spots still formed a quasi-crystalline ring. Therefore, according to the diffraction distance, they were attributed to the (2 22) and (4 2 2) crystal planes of Co3S4 respectively. This also proves the existence of (2 2 2) of Co3S4 and Ni3S4 that appeared in TEM.
[0053] Example 2
[0054] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0055] (1) Pour 0.2 mmol of nickel acetate tetrahydrate and 1.8 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0056] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0057] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0058] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC19.
[0059] Example 3
[0060] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0061] (1) Pour 0.4 mmol of nickel acetate tetrahydrate and 1.6 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0062] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0063] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0064] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then the product was dried to obtain Ni3S4 / Co3S4, denoted as NC28.
[0065] Example 4
[0066] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0067] (1) Pour 0.6 mmol of nickel acetate tetrahydrate and 1.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0068] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0069] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0070] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC37.
[0071] Example 5
[0072] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0073] (1) Pour 0.8 mmol of nickel acetate tetrahydrate and 1.2 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0074] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0075] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0076] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC46.
[0077] Example 6
[0078] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0079] (1) Pour 1.0 mmol of nickel acetate tetrahydrate and 1.0 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0080] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0081] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0082] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC55.
[0083] Example 7
[0084] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0085] (1) Pour 1.2 mmol of nickel acetate tetrahydrate and 0.8 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0086] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0087] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0088] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC64.
[0089] Example 8
[0090] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0091] (1) Pour 1.4 mmol of nickel acetate tetrahydrate and 0.6 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0092] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0093] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0094] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC73.
[0095] Example 9
[0096] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0097] (1) Pour 1.8 mmol of nickel acetate tetrahydrate and 0.2 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0098] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0099] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0100] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4 / Co3S4, denoted as NC91.
[0101] Example 10
[0102] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0103] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0104] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.993 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0105] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 2 h to obtain a black block product;
[0106] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0107] Embodiment 11
[0108] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0109] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0110] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0111] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 6 h to obtain a black block product;
[0112] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0113] Example 12
[0114] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0115] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −25° C. for 24 h to obtain a precursor;
[0116] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.500 g of sodium thiosulfate pentahydrate and 0.500 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0117] (3) Place the porcelain boat in a tube furnace, raise the temperature to 50°C at 5°C / min, and sinter for 12 h to obtain a black block product;
[0118] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0119] Example 13
[0120] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0121] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 10 h to obtain a precursor;
[0122] (2) 0.49 g of the precursor prepared in step (1) was mixed with 1.5 g of sodium thiosulfate pentahydrate and 1.5 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0123] (3) placing the porcelain boat in a tube furnace, heating to 200°C at 7°C / min, and sintering for 30 min to obtain a black block product;
[0124] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0125] Comparative Example 1
[0126] The preparation method of the Co3S4 material of this comparative example comprises the following steps:
[0127] (1) Pour 2 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0128] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0129] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0130] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then the product was dried to obtain Co3S4, denoted as NC010.
[0131] Comparative Example 2
[0132] The preparation method of the Ni3S4 material of this comparative example comprises the following steps:
[0133] (1) Pour 2 mmol of nickel acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0134] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate and 0.996 g of sodium chloride, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0135] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0136] (4) The black block product was dispersed in deionized water, washed by centrifugation multiple times with deionized water and ethanol, and then dried to obtain Ni3S4, denoted as NC100.
[0137] Comparative Example 3
[0138] The preparation method of a Ni3S4 / Co3S4 composite material without NaCl additive in this comparative example is different from that in Example 1 in that there is no NaCl additive, and the steps are as follows:
[0139] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0140] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0141] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0142] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 2 h to obtain a black block product;
[0143] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0144] Comparative Example 4
[0145] The preparation method of a Ni3S4 / Co3S4 composite material without NaCl additive in this comparative example is different from that in Example 1 in that there is no NaCl additive, and the steps are as follows:
[0146] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0147] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0148] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0149] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 6 h to obtain a black block product;
[0150] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0151] Comparative Example 5
[0152] The preparation method of a Ni3S4 / Co3S4 composite material without NaCl additive in this comparative example is different from that in Example 1 in that there is no NaCl additive, and the steps are as follows:
[0153] The preparation method of the nickel sulfide / cobalt sulfide composite material of this embodiment comprises the following steps:
[0154] (1) Pour 1.6 mmol of nickel acetate tetrahydrate and 0.4 mmol of cobalt acetate tetrahydrate into 10 mL of water, and stir at 400 r / min at 80° C. in a constant temperature mixer until the mixture is in a hydrogel state; freeze the mixture with liquid nitrogen, and dry the mixture in a vacuum freeze dryer at −50° C. for 12 h to obtain a precursor;
[0155] (2) 0.49 g of the precursor prepared in step (1) was mixed with 0.993 g of sodium thiosulfate pentahydrate, and then ground into powder using a mortar and pestle and placed in a porcelain boat;
[0156] (3) Place the porcelain boat in a tube furnace, raise the temperature to 150°C at a rate of 10°C / min, and sinter for 12 h to obtain a black block product;
[0157] (4) The black block product is dispersed in deionized water, centrifuged and washed multiple times with deionized water and ethanol, and then the product is dried to obtain Ni3S4 / Co3S4.
[0158] Figure 6 The FESEM images of the composite materials prepared in Comparative Example 1, Example 2 and Example 3. It can be seen from the figure that when the material is only metal cobalt, the morphology of the material prepared in Comparative Example 1 is formed by the accumulation of small particles ( Figure 6 ac). It can be seen from the figure that when the ratio of nickel to cobalt is 1:9, a skeleton-like structure gradually appears in the morphology of the material prepared in Example 2, but there are more particles ( Figure 6 df). When the ratio of nickel to cobalt in the material is 2:8, the pores in the skeleton morphology of the material prepared in Example 3 begin to gradually increase ( Figure 6 gi).
[0159] Figure 7 This is a FESEM image of the nickel sulfide / cobalt sulfide composite material prepared in Example 4-6. It can be seen from the figure that when the ratio of nickel to cobalt in the material is 3:7, the spherical shape in the skeleton morphology of the material prepared in Example 4 begins to gradually become larger ( Figure 7ac). When the ratio of nickel to cobalt in the material is 4:6, the skeleton morphology of the material prepared in Example 5 begins to gradually become uniform ( Figure 7 df). When the ratio of nickel to cobalt is 5:5, the pores of the skeleton-like morphology of the material prepared in Example 6 begin to gradually increase and the particles gradually become smaller ( Figure 7 gi).
[0160] Figure 8 The FESEM images of the nickel sulfide / cobalt sulfide composite materials prepared in Examples 7-9. It can be seen from the figure that when the ratio of nickel to cobalt in the material is 6:4, the skeleton in the skeleton-like morphology of the material prepared in Example 7 begins to gradually become larger ( Figure 8 ac). When the ratio of nickel to cobalt in the material is 7:3, the skeleton-like morphology of the material prepared in Example 8 begins to gradually become uniform and a skeleton-like shape appears ( Figure 8 df). When the ratio of nickel to cobalt in the material is 9:1, the skeleton-like morphology of the material prepared in Example 9 begins to squeeze the pores, and the pores begin to gradually decrease ( Figure 8 gi).
[0161] Fig. 9 The FESEM image of the material prepared in Comparative Example 2 shows that when the material is Ni3S4, the morphology of the material prepared in Comparative Example 2 is more agglomerated, and NaCl only increases the pores, but cannot form a skeleton-like structure ( Fig. 9 ac).
[0162] Fig.10 The FESEM images of the nickel sulfide / cobalt sulfide composite materials prepared in Examples 1, 10, 11 and Comparative Examples 3-5 are shown in the figure. As can be seen from the figure, the addition of sodium chloride not only makes the material size smaller, but also makes NC82 have more porous skeleton structure. It also makes the material morphology more uniform, and no agglomeration occurs under long-term sintering.
[0163] Test Case
[0164] 1. Electrochemical properties of electrode materials
[0165] The materials prepared in Examples 1, 6 and Comparative Example 2 were weighed with a conductive agent and a binder at a mass ratio of 8:1:1 and placed in a 10 mL beaker, and Ni3S4 / Co3S4 electrodes and Ni3S4 electrodes were prepared by pulping, coating, drying, and tableting. Then, a three-electrode system test was used, and the specific test process was as follows:
[0166] Test of the three-electrode system of electrode materials: The coated Ni3S4 / Co3S4 electrode and Ni3S4 electrode are used as working electrodes, the metal platinum sheet is used as the counter electrode, and Hg / HgO is used as the reference electrode. They are placed in a 2mol KOH aqueous solution. GCD test is performed on the blue electric test system. The test conditions are 0-0.5V, and the interval is 60s after each charge and discharge. When the current density exceeds 1A, -1 After that, an additional 0.5Ag -1 Discharge test; Cyclic voltammetry was tested in Chi660E, and the test conditions were 0-0.7V.
[0167] Fig.11 is the electrochemical properties of different electrode materials. Fig.11 As shown in Figure ac, cyclic voltammetry (CV) tests were performed on the three materials at different scan rates. Obvious redox peaks can be seen in the three figures, indicating that all three materials have pseudocapacitive properties. The CV curves show that NC82 has obvious pseudocapacitive behavior. The obvious redox peaks are mainly attributed to However, NC100 changes from 30mV s -1 The oxidation peak gradually disappeared and began to be distorted. This was mainly attributed to the slow cation reaction rate of Ni3S4 at high scan rates. This also means that NC100 does not have good tolerance in high-density current. However, the anode trace of NC55 gradually increased with the increase of scan rate. At 2 mV s -1 The highest reached 0.58mA, which is mainly attributed to the poor crystallinity of Co3S4 in NC55. In the case of a large amount of Co doping, nickel and cobalt did not form an effective heterostructure, and KOH aqueous solution caused them to quickly decompose and accumulate in the diffusion layer. The larger the electrode potential energy level, the more serious the accumulation of nickel and cobalt in the diffusion, which greatly affected the electrochemical performance of NC55. Because too many ions are piled in the diffusion layer and cannot be re-embedded, this will also lead to a significant decline in electrochemistry. The symmetrical redox peaks of NC82 illustrate the redox characteristics. From 2mV s -1 To 50mV s -1 The good overlap rate of the CV curves indicates its tolerance under high current, which also proves that NC82 forms the best heterostructure. Fig.11 d is the discharge time of the three materials at different current densities. -1 NC82 has the longest discharge time (1378s). -1 NC82 also has the longest discharge time (82s), but NC100 has the shortest discharge time (16s). This is completely consistent with the characteristics shown in the CV test. Fig.11e is the discharge time diagram of NC82 at different current densities. The heterogeneous structure of NC82 enables it to exhibit excellent electrochemical performance at different current densities. -1 The discharge times under are 1378, 585, 261, 82, 38, 23 and 7s respectively. Fig.11 f is the specific capacity diagram of NC55, NC82 and NC100 at different current densities under 2 mol KOH. It can be seen that NC82 and NC55 far exceed NC100 in the three-electrode system. -1 The discharge specific capacities under these conditions reached 1374, 1223, 1118, 923, 712, 459 and 290 F g -1 .
[0168] 2. Electrochemical performance of supercapacitors
[0169] A method for assembling a supercapacitor device comprising a framework-like Ni3S4 / Co3S4 electrode material, comprising the following steps:
[0170] (1) Preparation of porous granular Ni3S4 / Co3S4 electrode: The nickel sulfide / cobalt sulfide composite material (Ni3S4 / Co3S4, NC82) prepared in Example 1, a conductive agent and a binder in a mass ratio of 8:1:1 were weighed and placed in a 10 mL beaker, and a skeleton-like Ni3S4 / Co3S4 electrode was obtained by slurrying, coating, drying, and pressing.
[0171] (2) Preparation of counter electrode: Conductive carbon material and binder were weighed in a mass ratio of 8:2 and placed in a 10 mL beaker. An activated carbon counter electrode was prepared by slurrying, coating, drying, and pressing.
[0172] (3) Assembly of supercapacitor device: The skeleton-like Ni3S4 / Co3S4 electrode, non-woven fabric separator and counter electrode are laminated together and placed in a suitable container. An appropriate amount of KOH aqueous solution is injected as an electrolyte. The container is then sealed with paraffin to obtain a supercapacitor device, denoted as NC82 / / AC.
[0173] The nickel sulfide / cobalt sulfide composite electrode material (Ni3S4 / Co3S4, NC55) prepared in Example 6 and the nickel sulfide electrode material (Ni3S4, NC100) prepared in Comparative Example 2 were assembled into corresponding supercapacitor devices NC55 / / AC and NC100 / / AC according to the above-mentioned assembly method.
[0174] The electrochemical test of the asymmetric supercapacitor assembled above was carried out as follows: the assembled supercapacitor device was subjected to GCD test on the Blue Electric test system. The test conditions were 0-1.6V, with a 60s interval after each charge and discharge. -1 After that, an additional 0.5Ag -1 Discharge test; Cyclic voltammetry and AC impedance method were tested in Chi660E, and the test conditions were 0-1.8V.
[0175] Fig.12 The electrochemical performance results of the assembled devices Ni3S4 / Co3S4 / / AC or Ni3S4 / / AC. Fig.12 a is the CV curve of the supercapacitor device assembled in Example 1. In the cyclic voltammetry test graph, the obvious redox peaks once again prove the above results. Fig.12 b is the discharge time of the supercapacitor device assembled in Example 1 at 0.5Ag -1 The discharge time reached 1978s. The specific capacitance of different supercapacitor devices was calculated according to the formula ( Fig.12 c). In the constant current charge and discharge test diagram of capacitors assembled with NC82, NC55 and NC100 as electrode materials, NC82 / / AC at 0.5, 1, 2, 3, 5, 8 and 15Ag -1 The specific capacitances under the conditions are 650, 511, 453, 420, 377, 321, and 244 F g -1 NC82 / / AC has a specific capacitance of 0.5Ag -1 It is 1.5 times higher than NC100 / / AC. Especially at high current 15Ag -1 This indicates that the heterojunction structure of Ni3S4 / Co3S4 synthesized under multiphase transformation can not only improve the electrochemical performance, but also greatly improve its charge and discharge capacity under large current. Therefore, the heterojunction and OSO brought by sintering can ensure that the material can be used at 5A g -1 After 9000 cycles of testing, it can maintain 89.6% of its initial capacitance and the Coulomb efficiency is about 95% ( Fig.12 e). Then the Ragone diagram of energy-power density was calculated by the formula ( Fig.12 d), the assembled NC82 / / AC can be 234.3W kg -1 Power density reaches 197Wh kg -1 The energy density is 6104.9W kg -1 Maintain 37.3Wh kg -1 energy density.
[0176] In summary, the present invention proposes a new sintering method for the field of nanomaterials. This method overcomes the problem of severe densification during the sintering process leading to excessive material size. It is safe, simple, fast, easy to operate, and suitable for industrial scale-up.
[0177] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a nickel sulfide / cobalt sulfide composite material, characterized in that: Here are the steps: (1) nickel acetate tetrahydrate, cobalt acetate tetrahydrate and water are mixed, stirred until a hydrogel state is formed, and then frozen to a solid state and freeze-dried to obtain a precursor; (2) mixing and grinding the precursor obtained in step (1) with sodium thiosulfate pentahydrate and sodium chloride, and sintering the mixture in a protective atmosphere to obtain a black block product; (3) The black block product obtained in step (2) is washed and dried to obtain a nickel sulfide / cobalt sulfide composite material.
2. The method for preparing the nickel sulfide / cobalt sulfide composite material according to claim 1, characterized in that: In the step (1), the molar ratio of nickel acetate tetrahydrate to cobalt acetate tetrahydrate is (1-9): (1-9).
3. The method for preparing the nickel sulfide / cobalt sulfide composite material according to claim 2, characterized in that: The freeze drying temperature in step (1) is -50 to -25 o C, time is 10-24 h.
4. The method for preparing the nickel sulfide / cobalt sulfide composite material according to claim 3, characterized in that: In the step (2), the mass ratio of the precursor, sodium thiosulfate pentahydrate and sodium chloride is 0.49: (0.5-1.5): (0.5-1.5).
5. The method for preparing the nickel sulfide / cobalt sulfide composite material according to claim 4, characterized in that: The sintering conditions in step (2) are: a heating rate of 5-10 o C / min, sintering temperature is 50-200 o C, time is 30min-12h.
6. The method for preparing the nickel sulfide / cobalt sulfide composite material according to claim 5, characterized in that: The washing in step (3) refers to multiple centrifugal washings with deionized water and ethanol.
7. A nickel sulfide / cobalt sulfide composite material prepared by the preparation method according to any one of claims 1 to 6.
8. The nickel sulfide / cobalt sulfide composite material according to claim 7, characterized in that: The nickel sulfide / cobalt sulfide composite material is in a skeleton-like shape, and the particle diameter is 50-200 nm.
9. Use of the nickel sulfide / cobalt sulfide composite material according to claim 8 in a supercapacitor.
10. A supercapacitor, characterized in that: It comprises a counter electrode, a diaphragm, an electrolyte and a Ni3S4 / Co3S4 electrode, wherein the Ni3S4 / Co3S4 electrode comprises a conductive agent, a binder and the nickel sulfide / cobalt sulfide composite material according to claim 7.