Phosphate starting glass for high-level nuclear waste phosphate glass solidified body and preparation method of phosphate starting glass
By designing phosphate start-up glass that does not contain transition metal oxides, the problem of crystallization during the start-up of the phosphate glass solidification furnace for high-level radioactive nuclear waste has been solved, achieving the effects of easy start-up, resistance to crystallization and low erosion, ensuring high actinide series Safe solidification of high zirconium and high molybdenum waste phosphate glasses.
Patent Information
- Application Number
- CN202410778239.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
AI Technical Summary
During the start-up process of the phosphate glass solidification furnace for high-level radioactive nuclear waste, the existing phosphate glass formula is prone to crystallization, resulting in large-area crystallization of the melt, endangering the solidification process and facilities, and it is difficult to meet the requirements of easy start-up, anti-crystallization and low erosion requirements.
A phosphate starting glass that does not contain transition metal oxides is designed. The mass percentage of P2O5, SiO2, B2O3 and alkali metal oxides in the composition is not less than 10 but not higher than 14, and the mass percentage of rare earth oxides is not less than 10 but not more than 14. Less than 2, through specific raw material conversion and mixing processes, a phosphate starting glass can be prepared that is easy to start, resists crystallization, and integrates well with high actinide series, high zirconium, and high molybdenum waste phosphate glass.
It achieves easy start-up, no reduction reaction, high crystallization resistance and good fusion properties of the glass, reduces furnace corrosion, avoids transition metal ion reduction reactions, and improves the glass-forming performance and safety of the glass.
Smart Images

Figure CN118754428A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of glass solidification treatment of radioactive nuclear waste, and relates to a phosphate starting glass for high-level nuclear waste phosphate glass solidification body and a preparation method thereof, and is particularly suitable for starting a phosphate glass solidification body furnace with a phosphorus content of less than 50 mass percent in the nuclear industry. Background Art
[0002] The development of nuclear technology and the peaceful use of nuclear energy are one of the greatest achievements of mankind in the 20th century. However, if the nuclear waste generated after the use of nuclear energy cannot be safely handled, it will bring serious harm to humans and the environment. Among them, high-level nuclear waste containing highly radioactive and long-half-life nuclides must be solidified and then disposed of in deep geological conditions to solve its proliferation hazards. At present, the only feasible and engineering-applied treatment technology for high-level nuclear waste is to solidify it with glass. The method is to mix high-level nuclear waste with basic glass materials and put them into a glass melting furnace to melt them into a glass state. After homogenization, they are leaked into steel cylinders to form, thereby obtaining a glass solidified body containing high-level nuclear waste. After the steel cylinders are safely buried in geological conditions, the purpose of preventing high-risk nuclides from migrating to the ecosystem is achieved.
[0003] The unique structure of phosphate glass makes it have the advantages of high solubility for actinide nuclides, transition metal ions and heavy metal ions, and thus high inclusion rate for high-level nuclear waste. European and American countries have conducted a lot of research and accumulation on phosphate glass solidification systems, and since 1987, phosphate glass solidification systems based on aluminum phosphate and iron phosphate have been applied in Russia. In order to accelerate the safe solidification of high-level nuclear waste and realize its engineering as soon as possible, my country has conducted phosphate glass solidification research on high-level nuclear waste with high actinide, high zirconium and high molybdenum characteristics in recent years. The specific content includes the research on the formula of phosphate solidification glass and the necessary and matching furnace startup glass research.
[0004] There are many requirements for the start-up glass of the phosphate glass solidification furnace. First, the glass must be easy to start, that is, the glass resistivity is low; second, the start-up glass must not undergo a reduction reaction with the furnace electrode, or the start-up graphite ring, or the start-up metal ring during the furnace startup process; third, it must have good anti-crystallization ability; fourth, it must have excellent ability to fuse with the solidified glass to ensure that the solidified glass will not cause large-scale crystallization after being added to the furnace. As mentioned above, phosphate solidified glass with a P2O5 content of less than 50% by mass contains a large amount of rare earth, zirconium, molybdenum, transition metals and other components, so the glass forming range is narrow, and it has the characteristics of easily forming crystal phases such as monazite and zirconium pyrophosphate. After fusion with the start-up glass with a large difference in composition, it is very easy to turn to the non-vitrified direction, resulting in large-scale crystallization of the melt, which has great harm to the furnace solidification process, and even causes the furnace to stop production, endangering the normal operation of the entire solidification facility. In this case, the start-up glass formula that meets the above four requirements has always been a difficult problem in the solidification of high-level waste phosphate glass in my country. Therefore, in order to address this research problem, it is necessary to develop a widely adaptable matching phosphate starting glass that can be used with high-actinide, high-zirconium, and high-molybdenum waste phosphate solidification glass to meet a series of requirements for the start-up of the phosphate glass solidification furnace, thereby smoothly advancing the solidification process. Summary of the invention
[0005] In response to the research difficulties in starting glass in the research on phosphate glass solidification of high-level radioactive waste in my country, a phosphate starting glass is proposed, which does not contain transition metal oxides, is easy to start, does not undergo reduction reaction with furnace electrodes or starting graphite rings or starting metal rings, has good anti-crystallization performance, and integrates well with high-actinide, high-zirconium, and high-molybdenum waste phosphate glass solidification glass, so as to meet the startup needs of the above-mentioned high-actinide, high-zirconium, and high-molybdenum waste phosphate glass solidification furnace.
[0006] The specific technical solutions of the present invention are as follows:
[0007] A phosphate starter glass for high-level nuclear waste phosphate glass solidification body, which has the characteristics of easy start-up, no reduction reaction, high anti-crystallization performance, good fusion with solidified glass, low corrosion to the furnace, etc., and its components are as follows by mass percentage:
[0008]
[0009] The sum of the mass percentages of network formers P2O5, SiO2 and B2O3 in this series of glasses is not less than 45, the sum of the mass percentages of alkali metal oxides MgO, CaO, SrO and BaO is not less than 10 but not more than 14, and the sum of the mass percentages of rare earths Ce2O3, La2O3 and Nd2O3 is not less than 2.
[0010] The present invention also provides a method for preparing the above-mentioned phosphate starting glass, comprising the following steps:
[0011] 1) Alkaline earth metals are converted into molar mass and introduced by carbonate or nitrate, Al2O3 is converted into molar mass and introduced by Al(OH)3, B2O3 is converted into molar mass and introduced by boric acid, P2O5 is converted into molar mass and introduced by NaPO3, Na2O is converted into molar mass, and the remaining Na2O is introduced by carbonate after removing the part introduced by NaPO3, and the remaining components are directly introduced by the respective oxides according to the mass percentage;
[0012] 2) According to the glass formula, the glass batch is calculated based on the selected raw materials, and then the raw materials are weighed and mixed evenly to obtain the glass batch;
[0013] 3) Pour the batch materials into a corundum or quartz crucible, melt them in a furnace at 1200°C, clarify them for 1 hour, stir them for 2 hours, and obtain a uniform, bubble-free glass liquid;
[0014] 4) Pour the clarified and homogenized glass liquid into a stainless steel mold and then transfer it to an annealing furnace at 425°C for annealing;
[0015] 5) Each glass block is kept in an annealing furnace for 3 hours, then cooled to 100°C at a rate of 1°C / min, and the annealing furnace is closed to cool naturally to room temperature to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace.
[0016] The beneficial effects of the present invention are:
[0017] 1) The low-phosphorus and high-aluminum design can reduce the corrosion of phosphates on the furnace body during high-temperature startup, and ensure excellent glass-forming properties through a high content of aluminum;
[0018] 2) The network generators that are lacking due to low phosphorus are supplemented by boron and silicon, which can ensure that the content of network generators does not decrease significantly due to the decrease in phosphorus;
[0019] 3) Controlling the alkali metal content in the range of 10 to 14 mass percent can ensure that the glass has good anti-crystallization performance, and utilize the alkali metal-alkaline earth metal mixed alkali effect to inhibit the damage of glass chemical stability reduction caused by high content of Na2O;
[0020] 4) The transition metal-free design can prevent the serious harm of transition metal ions being reduced to alloys during the furnace startup process due to the reaction between transition metal ions in the startup glass and the furnace electrodes, or the startup graphite rings, or the startup metal rings;
[0021] 5) The glass formula provided by the present invention has the advantages of easy startup, no risk of transition metal ion reduction, good anti-crystallization performance, and good integration with high-actinide, high-zirconium, and high-molybdenum waste phosphate solidified glass. Compared with traditional phosphate glass, the glass formula of the present invention greatly reduces the corrosion of the furnace body. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the resistivity diagram of the first embodiment of the present invention. DETAILED DESCRIPTION
[0023] The phosphate starting glass for high-level nuclear waste phosphate glass solidification provided in the embodiment has the following components and oxide mass percentages:
[0024]
[0025]
[0026] The total mass percentage of network formers P2O5, SiO2 and B2O3 in this series of glasses is not less than 45, the total mass percentage of alkali metal oxides MgO, CaO, SrO and BaO is not less than 10 but not more than 14, and the total mass percentage of rare earths Ce2O3, La2O3 and Nd2O3 is not less than 2.
[0027] The preparation method of the glass in the embodiment comprises the following steps:
[0028] 1) Alkaline earth metals are converted into molar mass and introduced by carbonate or nitrate, Al2O3 is converted into molar mass and introduced by Al(OH)3, B2O3 is converted into molar mass and introduced by boric acid, P2O5 is converted into molar mass and introduced by NaPO3, Na2O is converted into molar mass, and the remaining Na2O is introduced by carbonate after removing the part introduced by NaPO3, and the remaining components are directly introduced by the respective oxides according to the mass percentage;
[0029] 2) According to the glass formula, the glass batch is calculated based on the selected raw materials, and then the raw materials are weighed and mixed evenly to obtain the glass batch;
[0030] 3) Pour the batch materials into a corundum or quartz crucible, melt them in a furnace at 1200°C, clarify them for 1 hour, stir them for 2 hours, and obtain a uniform, bubble-free glass liquid;
[0031] 4) Pour the clarified and homogenized glass liquid into a stainless steel mold and then transfer it to an annealing furnace at 425°C for annealing;
[0032] 5) Each glass block is kept in an annealing furnace for 3 hours, then cooled to 100°C at a rate of 1°C / min, and the annealing furnace is closed to cool naturally to room temperature to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace.
[0033] The present invention is further described below in conjunction with specific embodiments.
[0034] Table 1 shows the oxide composition of the glass formulations of 6 specific embodiments of the present invention. The batch material of each embodiment is 800g:
[0035] Table 1
[0036] Components (wt%) Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 <![CDATA[P2O5]]> 36 39 41 43 45 46 <![CDATA[Al2O3]]> 19 19 16 13 13 16 <![CDATA[Na2O]]> 19 18 18 22 21 23 <![CDATA[SiO2]]> 5 3 3 3 3 0 <![CDATA[B2O3]]> 5 4 2 4 2 0 CaO 1 0 0 4 0 1 MgO 1 0 4 0 3 2 SrO 3 4 2 0 3 2 BaO 7 9 8 6 5 6 <![CDATA[Ce2O3]]> 0 0 1 1 0 1 <![CDATA[La2O3]]> 1 1 0 1 2 0 <![CDATA[Nd2O3]]> 2 1 2 1 0 1 <![CDATA[ZrO2]]> 1 2 1 2 2 1 <![CDATA[Nb2O5]]> 0 0 2 0 1 1 <![CDATA[P2O5+SiO2+B2O3]]> 46 46 45 50 50 46 MgO+CaO+SrO+BaO 12 13 14 10 11 11 <![CDATA[Ce2O3+La2O3+Nd2O3]]> 3 2 3 3 2 2 1100℃ resistivity / Ω.cm 2.07 1.7 1.99 1.8 1.74 1.64 900℃ resistivity / Ω.cm 3.9 2.24 2.65 2.39 2.3 2.18
[0037] Embodiment 1:
[0038] According to the mass percentage of the oxides in formula No. 1 in Table 1, 800g of batch material is calculated: 328g of sodium metaphosphate, 184.2g of aluminum hydroxide, 35.6g of sodium carbonate, 31.7g of silicon dioxide, 56.3g of boric acid, 11.3g of calcium carbonate, 13.3g of magnesium carbonate, 38.8g of strontium nitrate, 75.6g of barium nitrate, 6.3g of lanthanum oxide, 12.7g of neodymium oxide, and 6.3g of zirconium oxide are weighed and mixed well to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold and transferred to a 425°C annealing furnace for 3 hours. Then the temperature is reduced to 100°C at a rate of 1°C / minute. The annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace. About 600g of glass is cut out and broken for resistivity testing. The glass resistivity is tested every 50°C from 850°C to 1200°C to form a glass starter glass. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 1 at 1100°C and 900°C is 2.07Ω.cm and 3.9Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
[0039] Embodiment 2:
[0040] According to the mass percentage of the oxides in formula No. 2 in Table 1, 800g of batch material is calculated: 360.4g of sodium metaphosphate, 187g of aluminum hydroxide, 10.7g of sodium carbonate, 19.3g of silicon dioxide, 45.7g of boric acid, 52.6g of strontium nitrate, 98.7g of barium nitrate, 6.4g of lanthanum oxide, 6.4g of neodymium oxide, and 12.9g of zirconium oxide are weighed and mixed thoroughly to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold for molding, transferred to an annealing furnace at 425°C for insulation for 3 hours, and then reduced to 100°C at a rate of 1°C / minute, and the annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent, phosphate starter glass suitable for the start-up of a high-level nuclear waste phosphate glass solidification furnace. Cut out about 600g of glass, break it and test its resistivity. Test the resistivity of the glass every 50℃ from 850℃ to 1200℃. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 2 at 1100°C and 900°C is 1.7Ω.cm and 2.24Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
[0041] Embodiment 3:
[0042] According to the mass percentage of the oxides in formula No. 3 in Table 1, 800g of batch material is calculated: 380.5g of sodium metaphosphate, 158.1g of aluminum hydroxide, 1.1g of sodium carbonate, 19.4g of silicon dioxide, 22.9g of boric acid, 54.1g of magnesium carbonate, 26.4g of strontium nitrate, 88.1g of barium nitrate, 17.1g of cerium nitrate, 12.9g of neodymium oxide, 6.5g of zirconium oxide, and 12.9g of niobium pentoxide are weighed and mixed well to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold and transferred to a 425°C annealing furnace for 3 hours. Then the temperature is reduced to 100°C at a rate of 1°C / minute. The annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace. About 600g of glass is cut out and broken for resistivity testing. The glass resistivity is tested every 50°C from 850°C to 1200°C to form a glass starter glass. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 3 at 1100°C and 900°C is 1.99Ω.cm and 2.65Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
[0043] Embodiment 4:
[0044] According to the mass percentage of the oxides in formula No. 4 in Table 1, 800g of batch material is calculated: 407.5g of sodium metaphosphate, 131.1g of aluminum hydroxide, 36.4g of sodium carbonate, 19.8g of silicon dioxide, 46.8g of boric acid, 47.1g of calcium carbonate, 67.5g of barium nitrate, 17.5g of cerium nitrate, 6.6g of lanthanum oxide, 6.6g of neodymium oxide, and 13.2g of zirconium oxide are weighed and mixed thoroughly to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold for molding, transferred to an annealing furnace at 425°C for insulation for 3 hours, and then reduced to 100°C at a rate of 1°C / minute, and the annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent, phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace. Cut out about 600g of glass, break it and test its resistivity. Test the resistivity of the glass every 50℃ from 850℃ to 1200℃. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 4 at 1100°C and 900°C is 1.8Ω.cm and 2.39Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
[0045] Embodiment 5:
[0046] According to the mass percentage of the oxides in formula No. 5 in Table 1, 800g of batch material is calculated: 433.5g of sodium metaphosphate, 133.3g of aluminum hydroxide, 15.5g of sodium carbonate, 20.1g of silicon dioxide, 23.8g of boric acid, 42.1g of magnesium carbonate, 41.1g of strontium nitrate, 57.1g of barium nitrate, 13.4g of lanthanum oxide, 13.4g of zirconium oxide, and 6.7g of niobium pentoxide are weighed and mixed to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold for molding, transferred to an annealing furnace at 425°C for insulation for 3 hours, and then reduced to 100°C at a rate of 1°C / minute, and the annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent, phosphate starter glass suitable for the start-up of a high-level nuclear waste phosphate glass solidification furnace. Cut out about 600g of glass, break it and test its resistivity. Test the resistivity of the glass every 50℃ from 850℃ to 1200℃. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 5 at 1100°C and 900°C is 1.74Ω.cm and 2.3Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
[0047] Embodiment 6:
[0048] According to the mass percentage of the oxides in formula No. 6 in Table 1, 800g of batch material is calculated: 435.2g of sodium metaphosphate, 161.2g of aluminum hydroxide, 32.8g of sodium carbonate, 11.8g of calcium carbonate, 27.6g of magnesium carbonate, 26.9g of strontium nitrate, 67.4g of barium nitrate, 17.4g of cerium nitrate, 6.6g of neodymium oxide, 6.6g of zirconium oxide, and 6.6g of niobium pentoxide are weighed and mixed thoroughly to obtain the batch material. The batch material is poured into a quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid. The clarified and homogenized glass liquid is poured into a stainless steel mold for molding, transferred to an annealing furnace at 425°C for insulation for 3 hours, then cooled to 100°C at a rate of 1°C / min, and the annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent, phosphate starter glass suitable for the start-up of a high-level nuclear waste phosphate glass solidification furnace. Cut out about 600g of glass, break it and test its resistivity. Test the resistivity of the glass every 50℃ from 850℃ to 1200℃. Figure 1 The measured temperature-resistivity curve of the glass shown in the figure shows that the resistivity of Example 6 at 1100°C and 900°C is 1.64Ω.cm and 2.18Ω.cm respectively. This resistivity value indicates that the glass will start very easily.
Claims
1. A phosphate starting glass for high-level nuclear waste phosphate glass solidification, characterized in that: The mass percentages of the glass components are: Among them, the total mass percentage of P2O5, SiO2 and B2O3 is not less than 45, the total mass percentage of alkali metal oxides MgO, CaO, SrO and BaO is not less than 10 but not more than 14, and the total mass percentage of rare earths Ce2O3, La2O3 and Nd2O3 is not less than 2.
2. A method for preparing phosphate starting glass for high-level nuclear waste phosphate glass solidification body as claimed in claim 1, characterized in that The following steps are involved: (1) According to the glass formula, the glass batch is calculated based on the selected raw materials, and then the raw materials are weighed and mixed evenly to obtain the glass batch; (2) melting, clarifying and stirring the glass batch material to obtain a uniform, bubble-free glass liquid; (3) pouring the glass liquid into a stainless steel mold to form it, and then transferring it to a preheated annealing furnace; (4) After annealing in the annealing furnace, each glass block is annealed to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace.
3. The method for preparing phosphate starting glass according to claim 2, characterized in that: The preparation process is carried out according to the following steps: (1) Calculating the glass batch material according to the glass formula and the selected raw materials, then weighing the raw materials and mixing them evenly to obtain the glass batch material; (2) The batch material is placed in a corundum or quartz crucible, melted in a furnace at 1200°C, clarified for 1 hour, and stirred for 2 hours to obtain a uniform, bubble-free glass liquid; (3) pouring the clarified and homogenized glass liquid into a stainless steel mold and then transferring it to an annealing furnace at 425° C. for annealing; (4) Each glass block is kept in an annealing furnace for 3 hours, then cooled to 100° C. at a rate of 1° C. / min. The annealing furnace is closed and naturally cooled to room temperature to obtain a uniform, transparent phosphate starter glass suitable for starting a high-level nuclear waste phosphate glass solidification furnace.