Method for preparing low-viscosity alkali-free liquid accelerator from magnetized water
By using magnetized water to prepare low-viscosity alkali-free liquid accelerator, the problem of high viscosity of suspended alkali-free liquid accelerator is solved, the construction stability of shotcrete is improved, and the simplicity and compatibility of the process are achieved, with potential for industrial production.
Patent Information
- Application Number
- CN202410921094.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
The existing suspended alkali-free liquid accelerator has a high viscosity, which makes it difficult to extract and pump at the construction site, affecting the construction stability of shotcrete.
Magnetized water is used as the raw material for accelerating setting agent synthesis. By optimizing the preparation process and formula of magnetized water, a low-viscosity alkali-free liquid accelerating setting agent is prepared, including adding magnetized water, fumed silica, fluorosilicic acid, and aluminum sulfate to the reaction kettle. and sodium hydroxide, and after stirring, heating and cooling, a low-viscosity alkali-free liquid accelerator is obtained.
It significantly reduces the viscosity of the alkali-free liquid accelerator, improves the construction stability of shotcrete, has a simple process, good compatibility, and has the promotion value of industrial-scale production.
Smart Images

Figure CN118754487A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete admixtures, in particular to a method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water. Background Art
[0002] Wet spraying of shotcrete refers to a process in which a certain amount of compressed air is used at the nozzle of the spray gun to mix concrete with an accelerator and spray it onto the sprayed surface to rapidly solidify. Compared with powdered alkali-accelerators, which are harmful to the human body and have a greater impact on the later strength of concrete, liquid alkali-free accelerators have the characteristics of fast hardening speed, high uniformity of the sprayed coating, and little impact on the later strength of concrete, and have gradually replaced traditional powdered alkali-accelerators.
[0003] At present, the most common alkali-free accelerators in the southwest region are suspended alkali accelerators of the fluosilicic acid system, and the main raw materials for production are aluminum sulfate, fluosilicic acid, etc. In the synthesis of accelerators, insoluble substances such as silica sol and aluminum fluoride are often generated and dispersed in the system, which greatly increases the viscosity of the alkali-free accelerator system.
[0004] During the on-site construction process, due to the different power and models of the pumps used to pump the accelerators at the construction site, coupled with the frequent aging and power reduction of on-site pumps, accelerators with too high a viscosity are often difficult to extract and pump during most on-site construction processes. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the existing defects. Aiming at the problem of high viscosity of suspended alkali-free liquid accelerator, the present invention provides a method for preparing low-viscosity alkali-free liquid accelerator by using magnetized water. By using magnetized water as the raw material for accelerator synthesis in the accelerator synthesis process, the preparation process of magnetized water and the formula of accelerator are optimized, and finally a low-viscosity alkali-free liquid accelerator with excellent comprehensive performance is obtained; the accelerator prepared by the method can significantly reduce the viscosity of the alkali-free liquid accelerator and improve the construction stability of shotcrete.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0008] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0009] Step 1: Add 32.5-35 parts of magnetized water to the bottom of the reaction kettle, start stirring, then add 1-2 parts of fumed silica, and continue stirring at room temperature for 1 hour;
[0010] Step 2: Continue to add 0.5-1 parts of triethanolamine and 20-24 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50-55°C;
[0011] Step 3: After the temperature is raised, keep the temperature at 50-55°C constant, add 37-45.3 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0012] Step 4: Turn off the heating, continue stirring and cooling, cool to below 35°C at room temperature, add 0.7-1 parts of sodium hydroxide and continue stirring for 0.5h to obtain a low-viscosity alkali-free liquid accelerator.
[0013] Furthermore, the magnetic field strength of the magnetized water treatment used in step 1 is 180-240 mT, and the flow rate is 0.6-1.2 m / s.
[0014] Furthermore, in step 1, step 3 and step 4, the stirring speed is 60-80 rpm.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The alkali-free liquid quick-setting agent prepared by magnetized water has lower viscosity than commercially available quick-setting agents and is more conducive to on-site construction.
[0017] (2) When magnetized water is used to prepare alkali-free liquid accelerator, there is no need to change the original accelerator production process during the accelerator reaction process, and the compatibility is good.
[0018] (3) The accelerator prepared by this method can significantly reduce the viscosity of the alkali-free liquid accelerator and improve the construction stability of the shotcrete.
[0019] (4) The process method involved in this technology is simple, the investment cost of magnetized water equipment is low, and it is easy to achieve industrial-scale production, which has great promotion advantages and value. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the viscosity test of alkali-free accelerating setting agent;
[0021] Figure 2 It is the setting time test of alkali-free accelerating setting agent;
[0022] Figure 3 It is the strength test of alkali-free accelerating setting agent; DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Embodiment 1:
[0025] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0026] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0027] Step 1: Using magnetized water obtained by treatment at a flow rate of 1 m / s and a magnetic field strength of 200 mT, 32.5 parts of magnetized water were added to the bottom of the reaction kettle, stirring was started at a stirring speed of 60 rpm, 1.5 parts of fumed silica were added, and stirring was continued at room temperature for 1 hour;
[0028] Step 2: Continue to add 1 part of triethanolamine and 23 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50°C;
[0029] Step 3: After the temperature is raised, keep the temperature at 50°C constant, add 41 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0030] Step 4: Turn off the heating, continue stirring and cooling, cool the system to below 35°C at room temperature, add 1 part of sodium hydroxide and continue stirring for 0.5h.
[0031] Embodiment 2:
[0032] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0033] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0034] Step 1: Using magnetized water obtained by treatment at a flow rate of 0.8 m / s and a magnetic field strength of 180 mT, 32.5 parts of magnetized water were added to the bottom of the reaction kettle, stirring was started at a stirring speed of 60 rpm, 1.5 parts of fumed silica were added, and stirring was continued at room temperature for 1 hour;
[0035] Step 2: Continue to add 1 part of triethanolamine and 23 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50°C;
[0036] Step 3: After the temperature is raised, keep the temperature at 50°C constant, add 41 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0037] Step 4: Turn off the heating, continue stirring and cooling, cool the system to below 35°C at room temperature, add 1 part of sodium hydroxide and continue stirring for 0.5h.
[0038] Embodiment 3:
[0039] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0040] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0041] Step 1: Using magnetized water obtained by treatment at a flow rate of 0.6 m / s and a magnetic field strength of 220 mT, 32.5 parts of magnetized water were added to the bottom of the reaction kettle, stirring was started at a stirring speed of 60 rpm, 1.5 parts of fumed silica were added, and stirring was continued at room temperature for 1 hour;
[0042] Step 2: Continue to add 1 part of triethanolamine and 23 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50°C;
[0043] Step 3: After the temperature is raised, keep the temperature at 50°C constant, add 41 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0044] Step 4: Turn off the heating, continue stirring and cooling, cool the system to below 35°C at room temperature, add 1 part of sodium hydroxide and continue stirring for 0.5h.
[0045] Embodiment 4:
[0046] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0047] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0048] Step 1: Using magnetized water obtained by treatment at a flow rate of 1 m / s and a magnetic field strength of 200 mT, 32.5 parts of magnetized water were added to the bottom of the reaction kettle, stirring was started at a stirring speed of 60 rpm, 1.5 parts of fumed silica were added, and stirring was continued at room temperature for 1 hour;
[0049] Step 2: Continue to add 1 part of triethanolamine and 20 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50°C;
[0050] Step 3: After the temperature is raised, keep the temperature at 50°C constant, add 44 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0051] Step 4: Turn off the heating, continue stirring and cooling, cool the system to below 35°C at room temperature, add 1 part of sodium hydroxide and continue stirring for 0.5h.
[0052] Embodiment 5:
[0053] A method for preparing a low-viscosity alkali-free liquid quick-setting agent by using magnetized water comprises the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silica, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate, and 0.7-1 part of sodium hydroxide.
[0054] A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water comprises the following steps:
[0055] Step 1: Using magnetized water obtained by treatment at a flow rate of 1 m / s and a magnetic field strength of 200 mT, 32.5 parts of magnetized water were added to the bottom of the reaction kettle, stirring was started at a stirring speed of 60 rpm, 1.5 parts of fumed silica were added, and stirring was continued at room temperature for 1 hour;
[0056] Step 2: Continue to add 1 part of triethanolamine and 23 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 55°C;
[0057] Step 3: After the temperature is raised, keep the temperature at 55°C constant, add 41 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour;
[0058] Step 4: Turn off the heating, continue stirring and cooling, cool the system to below 35°C at room temperature, add 1 part of sodium hydroxide and continue stirring for 0.5h.
[0059] Experimental example:
[0060] Referring to Example 1, the water used to synthesize the quick-setting agent was replaced from magnetized water to ordinary water that had not been treated with a magnetic field, and the other process parameters were kept unchanged to synthesize the alkali-free quick-setting agent.
[0061] The viscosity test results of the low-viscosity alkali-free liquid setting accelerator prepared according to the above examples and compared with the traditional alkali-free setting accelerators sold by our company and imported ones are as follows: Figure 1 As shown, the viscosity test equipment is NDJ-8S digital viscometer. Figure 1 It can be seen that the viscosity of the alkali-free liquid quick-setting agent prepared in Examples 1-5 is lower than that of the blank sample, the commercially available DS-6, and the imported Siguni L-54AF alkali-free liquid quick-setting agent, which illustrates the effectiveness of the technology of the present invention in reducing the viscosity of the liquid alkali-free quick-setting agent. In principle, in ordinary water, due to the asymmetry of the water molecule structure, there are a large number of hydrogen bonds between water molecules, which increases the interaction force between water molecules and restrains the flow of water molecules. When liquid water flows vertically through the magnetic field, the water molecules are polarized, and mutual repulsion is generated between the molecules, which will cause the hydrogen bonds between the water molecules to twist and stretch, and eventually break. The breaking of hydrogen bonds reduces the constraints between water molecules, which is manifested as a reduction in the viscosity of the quick-setting agent.
[0062] Figure 2 This is the test result of the setting time of the alkali-free liquid accelerating setting agent. The dosage of the accelerating setting agent in the test is 6%. The test method refers to GB / T 35159-2017 Accelerating Setting Agent for Shotcrete. As can be seen from the figure, after the alkali-free liquid accelerating setting agent synthesized using magnetized water is magnetized, the setting time prepared in most embodiments does not change much, among which the setting time of embodiment 4 is slow. Generally speaking, the promoting effect of fluorosilicic acid on the setting time in the accelerating setting agent is stronger than that of aluminum sulfate. The amount of fluorosilicic acid used in embodiment 4 is small, which ultimately makes the setting time slow.
[0063] Figure 3 This is the strength test result of alkali-free liquid accelerator. The accelerator dosage in the test is 6%. The test method refers to GB / T 35159-2017 Accelerator for Shotcrete. From the test results, compared with the blank sample and Example 1, Example 2, and Example 3, the strength of the alkali-free liquid accelerator synthesized with magnetized water has been slightly improved. This may be the result of increased activity of water after magnetization, which promotes the hydration of new cement. The strength of Example 4 is higher because there is more aluminum sulfate in Example 4. A large amount of aluminum sulfate will promote the formation of calcium sulfonate in the accelerator and increase the early strength of the system.
[0064] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water, characterized in that The invention is composed of the following raw materials in parts by weight: 32.5-35 parts of magnetized water, 1-2 parts of fumed silicon dioxide, 0.5-1 part of triethanolamine, 20-24 parts of fluorosilicic acid, 37-45.3 parts of aluminum sulfate and 0.7-1 part of sodium hydroxide.
2. The method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water according to claim 1, characterized in that: The steps include: Step 1: Add 32.5-35 parts of magnetized water to the bottom of the reaction kettle, start stirring, then add 1-2 parts of fumed silica, and continue stirring at room temperature for 1 hour; Step 2: Continue to add 0.5-1 parts of triethanolamine and 20-24 parts of fluorosilicic acid into the reaction kettle, and then turn on the heating to raise the temperature to 50-55°C; Step 3: After the temperature is raised, keep the temperature at 50-55°C constant, add 37-45.3 parts of aluminum sulfate into the reactor, and continue stirring for 1 hour; Step 4: Turn off the heating, continue stirring and cooling, cool to below 35°C at room temperature, add 0.7-1 parts of sodium hydroxide and continue stirring for 0.5h to obtain a low-viscosity alkali-free liquid accelerator.
3. The method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water according to claim 2, characterized in that: The magnetic field intensity of the magnetized water treatment used in step 1 is 180-240 mT, and the flow rate is 0.6-1.2 m / s.
4. The method for preparing a low-viscosity alkali-free liquid quick-setting agent using magnetized water according to claim 2, characterized in that: The stirring speed in step 1, step 3 and step 4 is 60-80 rpm.
Citation Information
Patent Citations
Magnetized-water-based waterproof grouting material for floor and preparation method of grouting material
CN105753414A
Double-component setting accelerator and preparation method thereof
CN109761527A
Alkali-free liquid accelerator containing fluosilicate as well as preparation method and application of alkali-free liquid accelerator
CN113003976A
Fluorine-free liquid alkali-free accelerator as well as preparation method and application thereof
CN113087441A
Alkali-free liquid accelerator and preparation method thereof
CN113698124A