Near-zero-ablation high-entropy carbide single-phase solid solution coating resistant to high temperature of 3000 DEG C as well as preparation method and application of near-zero-ablation high-entropy carbide single-phase solid solution coating
By combining discharge plasma sintering and vacuum plasma spraying, a multi-element high-entropy carbide coating is prepared to form a glass phase surface layer and a ceramic mixed-phase intermediate layer, which solves the problem of insufficient high-temperature ablation performance and achieves high-temperature near-zero ablation and High service temperature reduces preparation cost and complexity.
Patent Information
- Application Number
- CN202410937442.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing high-temperature transition metal carbide coatings have insufficient ablation performance in environments above 3000°C, and it is difficult to prepare dense and uniform high-entropy carbide single-phase solid solution coatings, which limits their application in hypersonic aircraft.
A method combining spark plasma sintering and vacuum plasma spraying is used to prepare a multi-element high-entropy carbide coating to form a dense glass phase surface layer and an ultra-high temperature ceramic mixed-phase intermediate layer to achieve near-zero ablation performance, and by optimizing the ratio and process Parameters ensure complete solid solution between carbides.
It achieves near-zero ablation performance in a high-temperature environment of 3000°C, improves the service temperature and oxidation ablation resistance of the coating, reduces process complexity and economic costs, and obtains an ideal single-phase high-entropy carbide solid solution coating.
Smart Images

Figure CN118754668A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material surface coatings, and further relates to high entropy carbide single-phase solid solution coating technology, specifically a 3000°C high-temperature resistant, near-zero ablation high entropy carbide single-phase solid solution coating and a preparation method thereof, which can be used to protect carbon-based composite materials in a high-temperature oxygen environment. Background Art
[0002] The extreme high temperature, high dynamic pressure and oxygen-rich environment of near-space hypersonic vehicles place extremely high demands on thermal protection materials. C / C composites are lightweight and have excellent mechanical properties, especially at high temperatures. Therefore, they are widely used in parts such as aircraft engines and spacecraft. However, carbon / carbon composites are easily oxidized at oxygen-rich temperatures. Under the scouring of high-temperature gases, the matrix material is rapidly consumed. The current working temperature is generally lower than 1650°C, which greatly restricts the application of C / C composites in hypersonic vehicles. Transition metal carbide ultra-high temperature ceramics have the advantages of high melting point, high thermal conductivity, high strength, high hardness, and high modulus. They are expected to be used as hot end structural components such as nose cones and wing leading edges of reusable aircraft. However, there are currently two major technical difficulties that restrict the application of transition metal carbides: First, the high temperature of 3000°C and the aerobic service environment in near-space place extremely stringent requirements on the ablation resistance of transition metal carbide coating materials, and single-component transition metal carbide materials are not sufficient to meet their requirements. The second is the preparation technology of transition metal carbide ceramic coatings with high density and ideal single-phase solid solution structure characteristics. The strong covalent bonds and low self-diffusion coefficients of ultra-high temperature transition metal carbides make it difficult to achieve full and uniform solid solution of multi-component carbides in the actual preparation process. Therefore, the preparation of multi-component transition metal carbide single-phase solid solution coatings with high temperature resistance of 3000℃ and near-zero ablation has become one of the most critical factors for its application.
[0003] The academic and industrial circles mainly use chemical vapor deposition CVD, magnetron sputtering, supersonic plasma spraying and vacuum plasma spraying to prepare transition metal carbide thermal protection coatings. The transition metal carbide coatings currently studied mainly include four types: single component, double component, three component and high entropy carbide. Among them, single component transition metal carbides mainly include HfC, TaC, ZrC, etc. Double component transition metal carbides mainly include Hf-Ta-C, Hf-Zr-C, Ta-Zr-C, etc. Multi-component transition metal carbide materials mainly include (Hf-Ta-W)C, (Hf-Ta-Zr)C, (Hf-Zr-Ti)C and high entropy carbides (Hf-Ta-Zr-Nb)C, (Hf-Ti-Zr-Ta-Nb)C, etc.
[0004] In Tan ZY, Luo C, Zhu W, Yang L, Zhou YC, Wu Q. Reactive plasma spray of supersaturated tungsten super-hard Ta-Hf-WC solid solution coating [J]. Journal of the European Ceramic Society, 2021, 41: 6772-6777., a method combining plasma spheroidization and vacuum plasma spraying was proposed to prepare Ta-Hf-WC solid solution coating. Although this method achieved partial solid solution of the mixed powder and improved the fluidity of the powder to a certain extent; however, since the plasma spheroidization process involves the interaction between powder particles and plasma jet, a complex and high-speed dynamic process, the solid solution between carbides is not sufficient during the formation of the solid solution powder, and the microstructures such as particle phase, density and particle size are extremely uneven, making it difficult to obtain an ideal single-phase Ta-Hf-WC solid solution coating; and the plasma spheroidization equipment is expensive and the economic cost is high. BCSchulz, B.Wang, R.A.Morris, D.Butts, G.B.Thompson.Influence of hafnium carbide on vacuum plasma spray processed tantalum carbide microstructures[J].Journal of the European Ceramic Society, 2013, 33:1219-1224. A method for preparing Hf-Ta-C ternary solid solution coating by vacuum plasma spraying process is proposed; this method effectively avoids oxidation of spraying materials by reducing the O2 content in the spraying environment, and achieves solid solution of TaC and HfC to a certain extent. Moreover, this method has high temperature and fast deposition rate, and is suitable for industrial mass production of ultra-high temperature thermal protective coatings. However, due to the short reaction time and fast speed of vacuum plasma spraying process, coupled with the strong covalent bond and low diffusion coefficient of TaC and HfC, the solid solution between TaC and HfC is not sufficient, and a certain amount of Ta2C and Ta4C3 second phases actually exist in the coating.Y.Wang, B.Zhang, C.Zhang, J.Yin, MJReece.Ablation behavior of(Hf-Ta-Zr-Nb)C high entropy carbide ceramic at temperatures above 2100℃[J].Journal of Materials Science&Technology,2022,113:40-47. (Hf-Ta-Zr-Nb)C high entropy alloy ceramics prepared by spark plasma sintering or hot pressing sintering can obtain single-phase solid solution ceramics, but the research object is mainly high entropy carbide bulk ceramics. Because the fracture toughness of bulk ceramic materials is relatively low, the impact resistance is poor, and it is difficult to withstand complex thermal gradients and thermal stresses, it is difficult to use them as thermal protection materials. In addition, the ablation performance of (Hf-Ta-Zr-Nb)C high entropy ceramics is poor. When the surface temperature reaches 2100℃ and the ablation is 60s, its linear ablation rate is as high as 8.5μm / s.
[0005] The maximum service temperature of the currently reported ultra-high temperature transition metal carbide thermal protection materials is about 2600℃, which cannot meet the higher service temperature requirements above 3000℃. The existing ultra-high temperature carbide coatings are mainly single-component carbides such as HfC, TaC, and ZrC, two-component carbides such as Hf-Ta-C, Hf-Zr-C, and Ta-Zr-C, and three-component carbide coatings such as Hf-Ta-WC and Hf-Ta-Zr-C. During the high-temperature ablation process, when TaC and WC are ablated at high temperature, due to their low melting points, they are prone to melting and instability during ablation, and cannot protect the substrate. When HfC and ZrC are ablated at high temperature, due to their oxide phase change, powder oxidation occurs, and a dense oxide layer cannot be generated, nor can the internal materials be protected. Summary of the invention
[0006] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and propose a high-entropy carbide single-phase solid solution coating resistant to 3000°C and near-zero ablation and a preparation method thereof, so as to solve the problem that the solid solution between transition metal carbides is insufficient in the preparation process of the existing high-entropy transition metal carbide coating, and the ideal single-phase carbide solid solution coating cannot be obtained. The present invention adopts a high-entropy transition metal carbide coating with more than four components, and forms a double-layer structure of a dense glass phase surface layer and an ultra-high temperature ceramic mixed phase intermediate layer during the high-temperature ablation process, effectively inhibiting the diffusion of oxygen, thereby achieving near-zero ablation of the coating; the high-entropy carbide coating is prepared by combining discharge plasma sintering with vacuum plasma spraying, which not only has low preparation cost and high efficiency, but also under the dual sintering of discharge plasma sintering and vacuum plasma spraying, the transition metal carbides are completely solid-dissolved, realizing the preparation of a single-phase high-entropy transition metal carbide solid solution coating.
[0007] To achieve the above-mentioned purpose, the present invention proposes a high-entropy carbide single-phase solid solution coating that is resistant to high temperatures of 3000°C and has near-zero ablation. The coating is a high-entropy carbide single-phase solid solution coating obtained by a spark plasma sintering process assisted by a vacuum plasma spraying process. The coating is a single-phase solid solution carbide structure and has high entropy characteristics.
[0008] The coating adopts high entropy carbide TMC mixed powder, deionized water, alcohol and 2wt.% PVA solution as raw materials; the TMC mixed powder includes TaC, HfC, ZrC, WC, TiC and NbC; and the proportion of TaC in the powder is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%.
[0009] Furthermore, the coating thickness is 300-400 μm; the particle size of the TMC mixed powder in the raw material is ≤5 μm, and the purity is ≥99.9%;
[0010] At the same time, a preparation method of a high-entropy carbide single-phase solid solution coating with a high temperature resistance of 3000°C and near-zero ablation is proposed, which includes the following steps:
[0011] (1) Preparation of TMC agglomerated powder by spray granulation:
[0012] (1.1) Using HfC, TaC, WC, TiC, ZrC and NbC as raw materials, and setting their proportions such that TaC is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%, and ball milling and drying is performed by a ball mill to obtain a multi-element high entropy carbide TMC mixed powder;
[0013] (1.2) ball milling the TMC mixed powder with deionized water, alcohol, and 2 wt.% PVA solution in a ratio of 4:4:1:1 to fully mix them to obtain a slurry for spray granulation;
[0014] (1.3) injecting the slurry into the spray tower of the spray granulation equipment, setting the parameters for spray granulation, and obtaining TMC agglomerated powder;
[0015] (2) Preparation of TMC solid solution powder by spark plasma sintering:
[0016] The obtained TMC agglomerated powder is placed in a graphite mold of a spark plasma sintering furnace for sintering and solid solution treatment to obtain TMC solid solution powder;
[0017] (3) Preparation of TMC single-phase solid solution coating by vacuum plasma spraying:
[0018] (3.1) selecting a substrate material, and performing sandblasting treatment on the surface of the substrate material by using a sandblasting machine to obtain a treated substrate sample;
[0019] (3.2) The substrate sample is heated using a spray gun, and then the TMC solid solution powder is sprayed and deposited on the surface of the substrate sample using a vacuum plasma spraying process. During the spraying process, Ar is used as the main gas and carrier gas, H2 is used as the auxiliary gas, and the spraying parameters are set according to actual needs to obtain a TMC single-phase solid solution coating coated on the surface of the substrate sample.
[0020] In addition, a high-entropy carbide single-phase solid solution coating with a high temperature resistance of 3000°C and near-zero ablation is proposed: 2 and 8MW / m 2 The coating is ablated by oxyacetylene under the heat flux density, and the coating generates low melting point oxide after oxyacetylene ablation, and forms a glass phase dense ablation layer on the surface thereof, thereby achieving near-zero ablation characteristics of the coating.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] First, the present invention utilizes a single-phase solid solution of multinary high-entropy carbides as an ultra-high temperature anti-ablation coating. The coating is prepared from a variety of carbides and has an ultra-high melting point. During the ablation process, a transition metal oxide glass phase surface layer is generated, which works together with an ultra-high temperature ceramic mixed phase intermediate layer to effectively reduce surface holes and channels and inhibit oxygen diffusion. Compared with currently used carbon-based thermal protection coatings such as C / C and C / SiC, the multinary high-entropy carbide single-phase solid solution coating has a higher service temperature, and compared with single-component, two-component, three-component and other ultra-high temperature coatings, it has excellent anti-oxidation and ablation performance, and can achieve near-zero ablation of the coating.
[0023] Second, the method for preparing a multi-component high-entropy carbide single-phase solid solution by combining spark plasma sintering with vacuum plasma spraying proposed in the present invention is more complete in solid solution between carbides, more uniform in element distribution, and has a simple and easy-to-operate preparation process compared to a single vacuum plasma spraying method. It can obtain an ideal single-phase solid solution coating while effectively reducing process complexity and economic costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a process flow chart of preparing the high entropy carbide TMC single-phase solid solution coating in the present invention;
[0025] Figure 2 is an X-ray diffraction diagram of the TMC solid solution powder after spark plasma sintering in the present invention;
[0026] Figure 3This is a scanning electron microscope image of the TMC solid solution powder after spark plasma sintering in the present invention;
[0027] Figure 4 This is a scanning electron microscope image of the cross section of the vacuum plasma sprayed TMC single-phase solid solution coating of the present invention;
[0028] Figure 5 It is a transmission electron microscope image of the vacuum plasma sprayed TMC single-phase solid solution coating in the present invention;
[0029] Figure 6 It is a scanning electron microscope image of the cross section of the TMC single-phase solid solution coating after ablation in the present invention and an ablation mechanism diagram. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the accompanying drawings.
[0031] Embodiment 1: Refer to the attached Figure 1 and 6 The present invention proposes a 3000°C high temperature resistant, near-zero ablation high entropy carbide single-phase solid solution coating, which is obtained by a spark plasma sintering process assisted by a vacuum plasma spraying process; the coating is a single-phase solid solution carbide structure and has high entropy characteristics; high entropy carbide TMC mixed powder, deionized water, alcohol and 2wt.% PVA solution are used as raw materials; wherein the TMC mixed powder includes TaC, HfC, ZrC, WC, TiC and NbC; and the proportion of TaC in the powder is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%. In this embodiment, the preferred coating thickness is 300-400μm, and the particle size of the TMC mixed powder in the preferred raw material is ≤5μm and the purity is ≥99.9%.
[0032] Embodiment 2: Refer to the attached Figure 1 The method for preparing the high entropy carbide single-phase solid solution coating in Example 1 proposed by the present invention specifically comprises the following steps:
[0033] Step 1. Preparation of TMC agglomerated powder by spray granulation:
[0034] (1.1) Using HfC, TaC, WC, TiC, ZrC and NbC as raw materials, and setting their proportions such that TaC is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%, and ball milling and drying is performed by a ball mill to obtain a multi-element high entropy carbide TMC mixed powder;
[0035] (1.2) ball milling the TMC mixed powder with deionized water, alcohol, and 2 wt.% PVA solution in a ratio of 4:4:1:1 to fully mix them to obtain a slurry for spray granulation;
[0036] (1.3) Inject the slurry into the spray tower of the spray granulation equipment, set the parameters for spray granulation, and obtain TMC agglomerated powder. In this embodiment, the granulation process is completed according to the following steps:
[0037] (1.3.1) Preheat the spray granulation equipment;
[0038] (1.3.2) Inject the slurry into the spray tower of the spray granulation equipment, set the parameters for spray granulation, and obtain granulated powder in the collection tank of the equipment;
[0039] (1.3.3) placing the granulated powder into an oven for drying to obtain TMC agglomerated powder;
[0040] Step 2. Preparation of TMC solid solution powder by spark plasma sintering:
[0041] The obtained TMC agglomerated powder is placed in a graphite mold of a spark plasma sintering furnace for sintering and solid solution treatment to obtain TMC solid solution powder;
[0042] Step 3. Preparation of TMC single-phase solid solution coating by vacuum plasma spraying:
[0043] (3.1) Select a base material, and perform sandblasting on the surface of the base material using a sandblasting machine to obtain a treated base sample; specifically, firstly, pre-treat the surface of the selected base material to obtain a base with a smooth surface, and then perform sandblasting on the pre-treated base surface using a sandblasting machine.
[0044] (3.2) The substrate sample is heated using a spray gun, and then the TMC solid solution powder is sprayed and deposited on the surface of the substrate sample using a vacuum plasma spraying process. During the spraying process, Ar is used as the main gas and carrier gas, H2 is used as the auxiliary gas, and the spraying parameters are set according to actual needs to obtain a TMC single-phase solid solution coating coated on the surface of the substrate sample.
[0045] Embodiment 3: Refer to the attached Figure 1-4 The overall implementation steps of this embodiment are the same as those of the second embodiment. Now, given parameter settings, the implementation process of the preparation method of the present invention is further described in detail:
[0046] In the first step, the mixed powder of multi-element high entropy carbide (TMC=HfC, TaC, WC, TiC, ZrC, NbC) after ball milling and drying is further ball milled with deionized water, alcohol and 2wt.% PVA solution in a ratio of 4:4:1:1 to mix evenly; during the ball milling and drying and continued ball milling and mixing, a planetary ball mill is used in this embodiment, and the ball mill speed is set to 200-300rpm and the ball milling time is 4-6h to obtain a fully mixed slurry for spray granulation.
[0047] The second step is to spray granulate within 10 minutes after the slurry is fully mixed to prevent the mixed slurry from secondary sedimentation and stratification. At the same time, the slurry needs to be continuously stirred during the granulation process, and preheating is started in advance according to the heating time of the spray granulation equipment. The parameter settings of the spray granulation equipment involved in the whole process include: injecting the slurry into the spray tower of the spray granulation equipment, setting the spray tower inlet temperature to 330℃~350℃, the spray tower outlet temperature to 100℃~150℃, the slurry pump rate to 14~25rpm, and the spray head speed to 30-40Hz, and spray granulation; finally, the collected granulation powder is placed in an oven, and the drying temperature in the drying process is set to 80-120℃ and the time is set to 10-15h according to the amount of granulation powder; this embodiment is preferably set to dry at 100℃ for 12h to obtain TMC agglomerated powder.
[0048] In the third step, the obtained TMC agglomerated powder was placed in a spark plasma sintering (SPS) sintering mold, and the sintering conditions were set as follows: sintering temperature 1900-2100 °C, heating rate 50-100 °C / min, holding time 5-20 min, chamber vacuum (5.4±0.4)×10 -1 Pa. Sintering and solid solution treatment is carried out. Since spark plasma sintering is a method of heating and sintering by directly passing pulse current between powder particles, it has the characteristics of short sintering time, fast heating speed and controllable organizational structure. Figure 2 and 3 It can be seen that the mixed powder is pretreated by spark plasma sintering. This process can not only achieve complete solid solution of multi-carbide powder, but also provide powder with good density, spherical particles and uniform composition, which provides the prerequisite for ensuring the acquisition of single-phase solid solution coating with uniform microstructure.
[0049] The fourth step is to select metal tungsten, C / SiC composite material or ultra-high temperature alloy as the substrate material, and perform pretreatment operations including grinding, chamfering, polishing and ultrasonic cleaning on its surface to obtain a substrate material with a smooth surface; then the surface of the pretreated substrate material is sandblasted by a sandblasting machine, and the sandblasting machine parameters are set during the treatment process as follows: sandblasting pressure 4-6MPa, sand particle size less than 100μm, sandblasting interval time 4-8s; and obtain the treated substrate sample;
[0050] In this step, the present embodiment preferably uses metal tungsten as the base material and pre-treats its surface to obtain a tungsten base material (W substrate) with a mirror-like and smooth surface. The material is then sandblasted by a sandblasting machine to increase the roughness of the base surface and remove the surface residual stress layer introduced by polishing, thereby enhancing the bonding force with the coating.
[0051] The fifth step is to spray and deposit the TMC single-phase solid solution coating on the W substrate by vacuum plasma spraying. To prevent thermal stress mismatch, the substrate is heated by a spray gun before spraying. In the vacuum plasma spraying process of this step in this embodiment, the spraying parameters are set as follows: equipment current 700A, equipment voltage 72V, gun travel speed 500m / s, powder feeding rate 15-25g / min, main gas Ar flow rate 30-40L / min, auxiliary gas H2 flow rate 10-20L / min, carrier gas Ar flow rate 2-5L / min, spraying distance 150-250mm, chamber pressure 800MPa. In this embodiment, a TMC single-phase solid solution coating with a spray thickness of about 300μm is preferably sprayed, and the obtained coating presents a flaky structure and contains pores and cracks.
[0052] Reference Figure 4 The cross-sectional SEM image of the vacuum plasma sprayed TMC single-phase solid solution coating of the present invention shows that the coating sprayed by the present invention has good interface bonding with the substrate, and the coating presents a typical plasma spray coating structure with flaky, pores and microcracks. Figure 5 The TEM image of the vacuum plasma sprayed TMC single-phase solid solution coating in the present invention shows that only one set of diffraction spots is found in the coating, corresponding to the face-centered cubic FCC structure, indicating that the carbides have achieved complete solid solution, thereby obtaining a single-phase high-entropy carbide solid solution coating.
[0053] Embodiment 4: The overall implementation steps of this embodiment are the same as those of Embodiments 2 and 3. Now, specific parameters are set to further describe the implementation process of the present invention in the form of examples:
[0054] Step A. Preparation of slurry for spray granulation:
[0055] (a1) using HfC, TaC, WC, TiC, ZrC and NbC in a ratio of 8:4:4:2:2:1 at% as raw materials, using a planetary ball mill, setting the ball mill speed to 280 rpm and the ball milling time to 6 h to obtain a multi-element high entropy carbide TMC mixed powder;
[0056] (a2) The TMC mixed powder was further ball-milled with deionized water, alcohol and 2 wt.% PVA solution in a ratio of 4:4:1:1 to mix them uniformly. The ball mill speed was set to 280 rpm and the ball milling time was set to 5 h to obtain a fully mixed slurry for spray granulation.
[0057] Step B. Preparation of TMC agglomerated powder:
[0058] (b1) preheating the spray granulation equipment;
[0059] (b2) within 10 minutes after the slurry is fully mixed, the slurry is injected into the spray tower of the spray granulation equipment, and the spray tower inlet temperature is set to 340° C., the spray tower outlet temperature is set to 120° C., the slurry pump rate is set to 17 rpm, and the spray head speed is set to 37 Hz, and spray granulation is performed. During the granulation process, the slurry is continuously stirred to obtain granulated powder in the collection tank of the equipment;
[0060] (b3) The collected granulated powder is placed in an oven and the drying temperature is set to 100° C. and the drying time is set to 12 h to obtain TMC agglomerated powder.
[0061] Step C: Place the obtained TMC agglomerated powder into a spark plasma sintering graphite mold, set the sintering temperature to 2000°C, the heating rate to 100°C / min, the holding time to 20min, and the chamber vacuum to (5.4±0.4)×10 -1 The sintering solid solution treatment is carried out to obtain TMC solid solution powder.
[0062] Step D. Select metal tungsten W as the substrate material and pre-treat its surface, then set the sandblasting pressure to MPa, the sand particle size to 10-100 μm, and the sandblasting interval to 6 s, and perform sandblasting on its surface by a sandblasting machine to obtain a treated W substrate sample;
[0063] Step E. Use a spray gun to heat the W substrate sample, and then use a vacuum plasma spraying method to spray and deposit a TMC single-phase solid solution coating on its upper surface. Set the spraying equipment current to 700A, voltage to 72V, gun travel speed to 500m / s, powder feeding rate to 20g / min, main gas Ar flow rate to 38L / min, auxiliary gas H2 flow rate to 12L / min, carrier gas Ar flow rate to 3L / min, spray distance to 200mm, chamber pressure to 800MPa, and spray to obtain a TMC single-phase solid solution coating with a thickness of 350μm coated on the surface of the substrate sample.
[0064] Embodiment 5: Refer to the attached Figure 5 and 6This embodiment provides an application of a high-entropy carbide single-phase solid solution coating that is resistant to high temperatures of 3000°C and has near-zero ablation. The high-temperature resistance and near-zero ablation performance of the TMC single-phase solid solution coating are reflected in its specific application. This embodiment further describes the characteristics of the high-entropy carbide single-phase solid solution coating of the present invention that is resistant to high temperatures of 3000°C and has near-zero ablation by applying the TMC single-phase solid solution coating material prepared by the present invention to a high-temperature ablation environment, as follows:
[0065] A high-temperature flame is generated by the combustion of a mixture of oxygen and acetylene gas, and then the flame is directed toward the high-entropy carbide single-phase solid solution coating material prepared by the present invention, at 6MW / m 2 and 8MW / m 2 The coating is ablated by oxyacetylene under the heat flux density. After the oxyacetylene ablation, the coating generates a low melting point oxide, and a glass phase dense ablation layer is formed on its surface, so as to achieve the near-zero ablation characteristic of the coating. The equipment for simulating the high temperature ablation environment in this embodiment is simple, low cost and easy to operate, and can quickly obtain the ablation condition of the coating in the present invention under the high temperature environment. In the specific application of this embodiment, the ablation parameters are set as follows: the nozzle diameter of the oxyacetylene flame is 5mm, the pressure of oxygen is 0.45MPa, the flow rate is 12L / min, the pressure of acetylene is 0.095MPa, the flow rate is 6-8L / min, the distance between the oxyacetylene nozzle and the coating sample is 10mm, and the ablation time is 120s.
[0066] Refer to the attached Figure 6 From the cross-sectional SEM image and ablation mechanism diagram of the TMC single-phase solid solution coating after ablation in the present invention, it can be seen that after the coating is ablated by oxyacetylene, a low-melting-point oxide is generated, and then a dense ablation layer of glass phase is formed on the surface of the coating, which effectively prevents oxygen diffusion, thereby achieving near-zero ablation characteristics of the coating, and its linear ablation rate is less than 0.2μm / s, which provides a favorable guarantee for the application of the coating in hypersonic aircraft.
[0067] The technical problem to be solved by the present invention is the difficulty in preparing a high-entropy carbide single-phase solid solution coating that is expected to meet the major demand for 3000°C thermal protection in aerospace. A high-entropy carbide solid solution coating that is resistant to 3000°C high temperature, has near-zero ablation and has ideal single-phase solid solution characteristics is prepared by mainly using a method combining discharge plasma sintering and vacuum plasma spraying. In view of the problems of strong covalent bonds and low self-diffusion coefficients of ultra-high temperature carbide ceramics, the present invention adopts a method combining discharge plasma sintering and vacuum plasma spraying to prepare a high-entropy carbide coating, wherein the mixed powder is pretreated by discharge plasma sintering. This process can not only achieve complete solid solution of multi-component carbide powders, but also provide good density, spherical particles and powders with uniform composition, providing the prerequisite for ensuring the acquisition of a single-phase solid solution coating with uniform microstructure. In view of the poor high-temperature ablation behavior of single-component carbide ceramics, which is difficult to meet the application requirements of ultra-high temperature extreme environments, the present invention innovatively prepares a single-phase solid solution high-entropy carbide coating from a variety of carbides such as HfC, TaC, ZrC, NbC and WC. This coating not only has a high melting point of over 3000°C, but also effectively inhibits the diffusion of oxygen during the ablation process through the combined effect of generating a transition metal oxide glass phase surface layer and an ultra-high temperature ceramic mixed phase intermediate layer, thereby achieving near-zero ablation of the coating.
[0068] Parts of the present invention that are not described in detail belong to common knowledge among those skilled in the art.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, for professionals in this field, after understanding the content and principles of the present invention, they may make various modifications and changes in form and details without departing from the principles and structures of the present invention. However, these modifications and changes based on the ideas of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A 3000°C high temperature resistant, near zero ablation high entropy carbide single-phase solid solution coating, characterized by: The coating is a high entropy carbide single-phase solid solution coating obtained by a spark plasma sintering process assisted by a vacuum plasma spraying process. The coating is a single-phase solid solution carbide structure and has high entropy characteristics. The coating uses high entropy carbide TMC mixed powder, deionized water, alcohol and 2wt.% PVA solution as raw materials; The TMC mixed powder includes TaC, HfC, ZrC, WC, TiC and NbC; and the proportion of TaC in the powder is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%.
2. The coating according to claim 1, characterized in that: The coating thickness is 300-400 μm; The particle size of the TMC mixed powder in the raw material is ≤5μm and the purity is ≥99.9%.
3. A method for preparing a 3000°C high temperature resistant, near zero ablation high entropy carbide single-phase solid solution coating, characterized in that: The steps include: (1) Preparation of TMC agglomerated powder by spray granulation: (1.1) Using HfC, TaC, WC, TiC, ZrC and NbC as raw materials, and setting their proportions such that TaC is not less than 40at%, HfC is not less than 20at%, ZrC is not less than 20at%, and WC+TiC+NbC is not higher than 20at%, and ball milling and drying is performed by a ball mill to obtain a multi-element high entropy carbide TMC mixed powder; (1.2) ball milling the TMC mixed powder with deionized water, alcohol, and 2 wt.% PVA solution in a ratio of 4:4:1:1 to fully mix them to obtain a slurry for spray granulation; (1.3) injecting the slurry into the spray tower of the spray granulation equipment, setting the parameters for spray granulation, and obtaining TMC agglomerated powder; (2) Preparation of TMC solid solution powder by spark plasma sintering: The obtained TMC agglomerated powder is placed in a graphite mold of a spark plasma sintering furnace for sintering and solid solution treatment to obtain TMC solid solution powder; (3) Preparation of TMC single-phase solid solution coating by vacuum plasma spraying: (3.1) selecting a substrate material, and performing sandblasting treatment on the surface of the substrate material by using a sandblasting machine to obtain a treated substrate sample; (3.2) The substrate sample is heated using a spray gun, and then the TMC solid solution powder is sprayed and deposited on the surface of the substrate sample using a vacuum plasma spraying process. During the spraying process, Ar is used as the main gas and carrier gas, H2 is used as the auxiliary gas, and the spraying parameters are set according to actual needs to obtain a TMC single-phase solid solution coating coated on the surface of the substrate sample.
4. The method according to claim 3, characterized in that: The ball mill is a planetary ball mill with a set rotation speed of 200-300 rpm and a ball milling time of 4-6 hours.
5. The method according to claim 3, characterized in that: The setting parameters in step (1.3) include: spray tower inlet temperature 330°C to 350°C, spray tower outlet temperature 100°C to 150°C, slurry pump speed 14 to 25 rpm, and spray head speed 30-40 Hz.
6. The method according to claim 3, characterized in that: The sintering solution treatment in step (2) is performed under the following conditions: sintering temperature 1900-2100°C, heating rate 50-100°C / min, holding time 5-20min, chamber vacuum degree (5.4±0.4)×10 -1 Pa.
7. The method according to claim 3, characterized in that: The substrate material in step (3.1) is tungsten metal, C / SiC composite material or ultra-high temperature alloy; the pretreatment includes grinding, chamfering, polishing and ultrasonic cleaning; the sandblasting treatment is set at a sandblasting pressure of 4-6 MPa, a sand particle size of less than 100 μm, and a sandblasting interval of 4 to 8 s.
8. The method according to claim 3, characterized in that: The spraying parameters set in step (3.2) include: equipment current 700A, equipment voltage 72V, gun travel speed 500m / s, powder delivery rate 15-25g / min, main gas Ar flow rate 30-40L / min, auxiliary gas H2 flow rate 10-20L / min, carrier gas Ar flow rate 2-5L / min, spraying distance 150-250mm, and chamber pressure 800MPa.
9. An application of the coating according to claim 1, characterized in that: 6MW / m 2 and 8MW / m 2 The coating is ablated by oxyacetylene under the heat flux density, and the coating generates low melting point oxide after oxyacetylene ablation, and forms a glass phase dense ablation layer on the surface thereof, thereby achieving near-zero ablation characteristics of the coating.
10. The use according to claim 9, characterized in that: The coating was ablated by oxyacetylene, and the ablation parameters were set as follows: the nozzle diameter of the oxyacetylene flame was 5 mm, the pressure of oxygen was 0.45 MPa, the flow rate was 12 L / min, the pressure of acetylene was 0.095 MPa, the flow rate was 6-8 L / min, the distance between the oxyacetylene nozzle and the coating sample was 10 mm, and the ablation time was 120 s.
Citation Information
Patent Citations
Ultrahigh-temperature high-entropy carbide powder and preparation method thereof
CN110078512A
Carbide high-entropy ceramic precursor, high-entropy ceramic and preparation method
CN111471268A
Low-temperature preparation method of refractory metal carbide solid solution powder
CN112875704A