Method for preparing high-molecular-weight copolyester by using waste PET (polyethylene terephthalate)
By using the transesterification reaction catalyzed by MXene materials in waste PET recycling, the problems of high energy consumption and poor environmental protection when preparing high molecular weight copolyesters from waste PET are solved, and efficient and environmentally friendly PET recycling is achieved, which is suitable for industrial production and The environmental protection and biodegradability of the product are improved.
Patent Information
- Application Number
- CN202411111612.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-11
AI Technical Summary
When using waste PET to prepare high-molecular-weight copolyester, the existing technology has problems such as reduced environmental energy consumption, high energy consumption, low efficiency, and difficulty in 100% recycling of the terephthalic acid structural units in PET.
A mixed reaction system containing glycol, recycled PET and MXene materials is used to carry out transesterification or esterification reaction to prepare the prepolymer of copolyester, and obtain high molecular weight copolyester through pre-polycondensation and final polycondensation reaction. Active and environmentally friendly Ti-based MXene catalyst.
It achieves a short reaction process, high efficiency, high utilization rate of waste PET, excellent product color, suitable for large-scale industrial production, high economic and environmental benefits, and can obtain 100% terephthalic acid structural units, which improves the copolymerization efficiency. Environmentally friendly and biodegradable esters.
Smart Images

Figure CN118755072A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling and reusing waste PET, and specifically relates to a method for preparing high molecular weight copolyester by utilizing waste PET. Background Art
[0002] Polyethylene terephthalate (PET) is a widely used type of plastic. Due to its good ductility and high transparency, it is often used to make beverage bottles or other food packaging materials. In 2019, the weight of PET beverage bottles consumed in my country reached 4.42 million tons. However, PET is difficult to degrade under natural conditions, and it takes at least hundreds of years to completely decompose, which brings a heavy burden to the environment and the economy. From an economic point of view, discarding plastic packaging after a single use will lose 95% of its use value; from an environmental point of view, it will also lead to many problems such as reduced crop yields and marine pollution. If used PET plastic bottles, especially beverage bottles, are recycled and recycled, it will be of great significance to environmental protection, economy, society and other aspects.
[0003] The prior art realizes the recycling, high-value recovery and biodegradation of waste PET by alcoholyzing PET into monomers, such as dimethyl terephthalate (DMT), terephthalic acid (TPA) and bis(hydroxyethyl) terephthalate (BHET), and then polymerizing to form materials such as PET, PETG, PCTG and PBAT. However, the separation cost of the monomers is very high, which is one of the main reasons limiting its industrialization. How to simply and efficiently convert PET into high-value products is still a huge challenge. In patent CN116675839A, 1,4-cyclohexanedimethanol (CHDM) and ethylene glycol (EG) are used as alcoholysis liquids to alcoholyze waste PET, and then separated by filtration, a catalyst and a repolymerization step are introduced to successfully prepare high molecular weight PETG / PCTG. Although this process greatly reduces the cost, the steps are complicated and the utilization rate of the terephthalic acid structural unit of waste PET is less than 100%. In addition, a large number of literatures have reported that high molecular weight products can be obtained by using a one-step polycondensation method by introducing high-content (>300 ppm) catalysts such as antimony trioxide, zinc acetate, etc. However, the catalysts used are highly toxic and are used in high amounts, which significantly limits the wide application of the products.
[0004] The melting point of PET material is as high as 240℃, and the activation energy of alcoholysis without catalyst is greater than 180kJ mol -1. Therefore, under normal circumstances, if no catalyst is introduced, the modification of PET using waste PET as raw material requires higher temperature and longer time. The introduction of a catalyst can significantly reduce energy consumption. However, the PET material itself contains a certain amount of antimony trioxide catalyst with a certain toxicity. If a high content (>100ppm) of toxic catalyst is introduced, it will be detrimental to the upgrading and recycling of PET. Therefore, the development of highly active and environmentally friendly catalysts is an effective way to solve the problem. In summary, using PET waste plastic as raw material to simply and efficiently prepare high molecular weight copolyesters containing terephthalic acid structural units is conducive to creating high economic and environmental benefits. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for preparing high molecular weight copolyester using waste PET, so as to solve the problems in the existing chemical recycling and upgrading technology for preparing polyester using waste PET, such as low environmental performance of the product, high energy consumption, low efficiency, and difficulty in 100% recycling of terephthalic acid structural units in PET.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0007] The embodiment of the present invention provides a method for preparing high molecular weight copolyester using waste PET, which comprises:
[0008] A mixed reaction system comprising at least a diol, recycled PET, and a catalyst is subjected to an ester exchange or esterification reaction to obtain a copolyester prepolymer; wherein the catalyst comprises a MXene material;
[0009] And, the prepolymer of the copolyester is subjected to a preliminary polycondensation reaction and a final polycondensation reaction to obtain a high molecular weight copolyester.
[0010] The embodiment of the present invention also provides a high molecular weight copolyester prepared by the aforementioned method.
[0011] An embodiment of the present invention also provides the use of MXene materials in catalyzing the recycling of PET to prepare copolyesters, wherein the copolyesters are formed by catalyzing the MXene material as a catalyst to react diols, used or unused dibasic acids or dibasic esters with recycled PET.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] (1) The method for preparing copolyester using recycled PET provided by the present invention has the advantages of short reaction process, high efficiency, high utilization rate of waste PET, and can obtain products with excellent color, which is suitable for large-scale industrial production and has high economic and environmental benefits;
[0014] (2) The copolyester prepared by the one-pot melt polycondensation method of the present invention contains 100% of the terephthalic acid structural units in the recycled PET, and the diol unit components contained in the molecular chain of the resultant product are greater than 80% of the feed composition. The yellow index of the copolyester obtained by this method is less than 5 and no external heat stabilizer is added, which improves the environmental protection of the copolyester, can prepare biodegradable copolyester and high Tg copolyester, and broadens the application range of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1a-1d is Ti3C2T prepared in a typical embodiment of the present invention x Structural characterization diagram of MXene;
[0017] Figure 2 The structural formula and NMR spectrum of the copolyester prepared in Example 1 of the present invention;
[0018] Figure 3 The structural formula and NMR spectrum of the copolyester prepared in Example 2 of the present invention;
[0019] Figure 4 The structural formula and NMR spectrum of the copolyester prepared in Example 3 of the present invention;
[0020] Figure 5 is the DSC curve diagram of Examples 1-3 of the present invention;
[0021] Figure 6 is a stress-strain curve diagram of samples of Examples 1-3 of the present invention;
[0022] Figure 7a-Figure 7b These are actual pictures of samples of Examples 1-3 of the present invention. DETAILED DESCRIPTION
[0023] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. Due to the high melting point of PET material (>240°C) and high activation energy of alcoholysis without catalyst (>180kJ mol -1), resulting in the use of waste PET as raw material to modify PET, which requires high temperature and long time, high energy consumption and large carbon emissions. However, due to the toxic antimony trioxide catalyst contained in the PET material itself, if a high content of toxic catalyst is introduced, it is not conducive to the upgrading and recycling of PET. The present invention creatively introduces a highly active and environmentally friendly Ti-based MXene catalyst into the PET modification system, and achieves the goal of preparing copolyesters by chemically recycling and upgrading waste PET with low energy consumption, high efficiency and low catalyst introduction by optimizing the reaction route.
[0024] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Specifically, as one aspect of the technical solution of the present invention, a method for preparing high molecular weight copolyester using waste PET includes:
[0026] A mixed reaction system comprising at least a diol, recycled PET, and a catalyst is subjected to an ester exchange or esterification reaction to obtain a copolyester prepolymer; wherein the catalyst comprises a MXene material;
[0027] And, the prepolymer of the copolyester is subjected to a preliminary polycondensation reaction and a final polycondensation reaction to obtain a high molecular weight copolyester.
[0028] In some preferred embodiments, the method specifically includes: mixing diol, used or unused dibasic acid or dibasic ester, recycled PET and a catalyst to form the mixed reaction system, and then reacting at 180-260° C. for 0.5-1.0 h in a protective atmosphere to obtain a copolyester prepolymer.
[0029] Further, the diol includes any one or more combinations of bisphenol A polyoxyethylene ether, bisphenol S polyoxyethylene ether, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, and spiroethylene glycol, and is not limited thereto.
[0030] Further, the dibasic acid includes any one or more combinations of terephthalic acid, furandicarboxylic acid, isophthalic acid, phthalic acid, succinic acid, adipic acid, sebacic acid, and dodecanedioic acid, but is not limited thereto.
[0031] Further, the dibasic ester includes any one or more combinations of terephthalate, furandicarboxylate, isophthalate, phthalate, succinate, adipate, sebacate, and dodecanedioate, but is not limited thereto.
[0032] Furthermore, the catalyst includes any one or more combinations of Ti3C2Tx, Ti4C3Tx, and Ti2CTx, but is not limited thereto.
[0033] Furthermore, the high molecular weight copolyester has a structure as shown in formula (I):
[0034]
[0035] Wherein, x, y, z are integers greater than 0, and z: (x+y) = 0 to 1, x: y = 0.1 to 4; R1 is derived from any one of an aromatic dibasic acid, an aromatic dibasic acid ester, a saturated aliphatic dibasic acid, and a saturated aliphatic dibasic acid ester; R2 is derived from an aromatic diol or a saturated aliphatic diol.
[0036] Further, the protective atmosphere includes a nitrogen atmosphere, but is not limited thereto.
[0037] Furthermore, the molar ratio of the diol to the dibasic acid or dibasic ester is greater than 2.
[0038] Furthermore, the molar ratio of the terephthalic acid structural unit to the dibasic acid or dibasic ester in the recycled PET is 1 to 4:1.
[0039] Furthermore, the molar ratio of the diol to the dibasic acid unit in the mixed reaction system is less than or equal to 2.2.
[0040] Furthermore, when the mixed reaction system does not use dibasic acid or dibasic ester, the molar ratio of terephthalic acid structural units to diols in the recycled PET is 1 to 5:1.
[0041] In some preferred embodiments, the method specifically comprises:
[0042] The temperature of the copolyester prepolymer is raised to 200-260° C., and the pressure of the system is reduced to 5-10 KPa to perform a pre-polycondensation reaction;
[0043] And, after the preliminary polycondensation reaction is completed, the temperature is raised to 220-295° C., and the pressure of the system is reduced to 10-60 Pa to carry out a final polycondensation reaction to obtain a high molecular weight copolyester.
[0044] Furthermore, the pre-polycondensation reaction time is 0.5 to 1.0 h.
[0045] Furthermore, the temperature of the pre-polycondensation reaction is 220-240°C.
[0046] Furthermore, the final polycondensation reaction time is 0.5 to 2.0 hours.
[0047] Furthermore, the temperature of the final polycondensation reaction is 240-275°C.
[0048] In some preferred embodiments, the method for preparing high molecular weight copolyester using waste PET comprises the following steps:
[0049] (1) placing a certain molar ratio of diol, dibasic acid (ester), recovered PET and a catalyst in a reactor, and performing an ester exchange (esterification) reaction for a period of time at a set temperature and in a nitrogen atmosphere at normal pressure to obtain a copolyester prepolymer;
[0050] (2) After the ester exchange (esterification) reaction is completed, the temperature is raised to the desired pre-polycondensation reaction temperature, and the pressure is gradually reduced to the desired pre-polycondensation reaction pressure, and the reaction is carried out for a certain period of time to carry out the pre-polycondensation reaction;
[0051] (3) After the pre-polycondensation reaction is completed, the temperature is gradually raised to the desired final polycondensation temperature, and the pressure is gradually reduced to the desired final polycondensation pressure to carry out the final polycondensation. The reaction is continued for a certain period of time to reach the desired viscosity, and the reaction is terminated and the material is discharged under inert gas protection to obtain a high molecular weight copolyester.
[0052] Furthermore, in step (1), R1 in the prepolymer structure is derived from an aromatic dibasic acid (ester) or a saturated aliphatic dibasic acid (ester). Such aromatic dibasic acid (ester) may be terephthalic acid (ester), furandicarboxylic acid (ester), isophthalic acid (ester), phthalic acid (ester), etc.; saturated aliphatic dibasic acid may be succinic acid (ester), adipic acid (ester), sebacic acid ester, dodecanedioic acid (ester), etc., but the R1 does not include oxalic acid (ester) and malonic acid (ester).
[0053] Furthermore, in step (1), R2 in the prepolymer structure is derived from an aromatic diol or a saturated aliphatic diol, but the saturated aliphatic diol has a boiling point higher than 220°C. Such a diol may be bisphenol A polyoxyethylene ether, bisphenol S polyoxyethylene ether, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, spiroethylene glycol, etc.
[0054] Furthermore, in step (1), the catalyst is a mixture of one or more of Ti3C2Tx, Ti4C3Tx, and Ti2CTx, the reaction temperature is 180 to 260° C., and the reaction time is 0.5 to 1.0 h.
[0055] Furthermore, in step (1), in order to ensure efficient polymerization of diols, the molar ratio of the diols introduced in the feed composition to the dibasic acid (ester) introduced is greater than 2, the molar ratio of the terephthalic acid structural unit from the recycled PET to the dibasic acid (ester) is 1 to 4, and the molar ratio of the diols introduced to the total dibasic acid units is not greater than 2.2. It should be noted that if no dibasic acid (ester) is introduced, the molar ratio of the terephthalic acid structural unit to the diols introduced is 1 to 5.
[0056] Furthermore, in step (2), the pre-polycondensation reaction temperature ranges from 200 to 260° C., the pre-polycondensation reaction pressure ranges from 5 KPa to 10 KPa, and the pre-polycondensation reaction time is 0.5 h; preferably, the pre-polycondensation reaction temperature is 220 to 240° C., and the polycondensation reaction pressure is 10 kPa.
[0057] Furthermore, in step (3), the reaction temperature is 220-295°C, the reaction pressure is 10-60 Pa, and the reaction time is 0.5-2.0 h; the preferred reaction temperature is 240-275°C, and more preferably 260°C.
[0058] Another aspect of the embodiments of the present invention further provides a high molecular weight copolyester prepared by the aforementioned method.
[0059] Furthermore, the high molecular weight copolyester has a structure as shown in formula (I):
[0060]
[0061]
[0062] Wherein, x, y, z are integers greater than 0, and z: (x+y) = 0 to 1, x: y = 0.1 to 4; R1 is derived from any one of an aromatic dibasic acid, an aromatic dibasic acid ester, a saturated aliphatic dibasic acid, and a saturated aliphatic dibasic acid ester; R2 is derived from an aromatic diol or a saturated aliphatic diol.
[0063] Furthermore, the intrinsic viscosity of the high molecular weight copolyester is 0.66 to 0.88 dL / g.
[0064] Another aspect of an embodiment of the present invention further provides the use of MXene materials in catalyzing the recycling of PET to prepare copolyesters, wherein the copolyesters are formed by catalyzing the MXene material as a catalyst to react diols, used or unused dibasic acids or dibasic esters with recycled PET.
[0065] Furthermore, the MXene material includes any one or more combinations of Ti3C2Tx, Ti4C3Tx, and Ti2CTx.
[0066] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0067] Unless otherwise specified, the raw materials or reagents used in the examples are all commercially available and can be purchased through commercial channels. The purity of the raw materials used in the following examples is not less than 97%, and all diols and dibasic acids are purchased from MacLean Company; PET waste materials come from washed and crushed Nongfu Spring brand mineral water bottles.
[0068] Preparation of catalyst MXene:
[0069] The preparation method of MXene is already very mature, so the MXene catalyst product described in this patent can be prepared by yourself or obtained through commercial channels. This patent uses a self-prepared sample, and its preparation method is as follows:
[0070] 1 g LiF was dissolved in 20 ml 6-9 M HCl and completely dissolved in a 100 ml polypropylene plastic bottle, then 1 g Ti3AlC2 was gradually added and reacted at 35 °C for 24 h. The acidic product was thoroughly washed with deionized water and centrifuged at 3500 rpm for several times, with each cycle lasting 5 min, until a stable dark green Ti3C2Tx flake supernatant with a pH ≥ 6 was obtained. At this stage, if the dark supernatant was poured off, a swollen clay-like sediment was observed. Deionized water was added to the precipitate and manually shaken for <5 minutes to promote the stratification of the flakes. After centrifugation at 3500 rpm for 1 h, a MXene concentration of 1.5-2.0 mg ml -1 The supernatant was vacuum dried for 72 hours. The structural characterization of the prepared Ti3C2Tx MXene is shown in the figure Figure 1a-1d shown.
[0071] Example 1
[0072] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), spiroethylene glycol (36.4g, 0.120mol) and 0.3mg MXene (dispersed in ethylene glycol, concentration of 1mg / mL, the same below) were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 200-260°C, and the reaction lasted for 1h, and the normal pressure ester exchange reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 260-280°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. From the beginning of heating of the material to the end of the reaction (the same below), the total time was <4h, and the structural formula and nuclear magnetic resonance spectrum of the prepared copolyester were as shown Figure 2 As shown, the DSC curve is as follows Figure 5 The stress-strain curve is shown in Figure 6 As shown in the figure, the actual sample is as follows Figure 7a-Figure 7b shown.
[0073] Example 2
[0074] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,10-decanediol (27.2g, 0.156mol) and 0.5mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 200-240°C, and the reaction lasted for 1h, and the normal pressure ester exchange reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-polycondensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was less than 4h, and the structural formula and nuclear magnetic spectrum of the prepared copolyester were as shown Figure 3 As shown, the DSC curve is as follows Figure 5 The stress-strain curve is shown in Figure 6 As shown in the figure, the actual sample is as follows Figure 7a-Figure 7b shown.
[0075] Example 3
[0076] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,6-hexanodioic acid (31.0g, 0.21mol), 1,4-butanediol (46.9g, 0.521mol) and 0.3mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 2.0h, and the normal pressure ester exchange reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.5h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <5h. After being buried in the soil for 3 months, the weight of the copolyester decreased by 30%, showing a certain biodegradability. The structural formula and nuclear magnetic resonance spectrum of the prepared copolyester are shown in Figure 4 As shown, the DSC curve is as follows Figure 5 The stress-strain curve is shown in Figure 6 As shown in the figure, the actual sample is as follows Figure 7a-Figure 7b shown.
[0077] Example 4
[0078] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,6-hexanediol (18.4g, 0.156mol) and 0.3mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 1.0h, and the normal pressure transesterification reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction lasted for 0.5h, and the pre-polycondensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction lasted for 0.8h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <4h.
[0079] Example 5
[0080] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,8-octanediol (22.8g, 0.156mol) and 0.5mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 1.0h, and the normal pressure transesterification reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction lasted for 0.5h, and the pre-polycondensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction lasted for 0.8h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <4h.
[0081] Example 6
[0082] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,12-octanediol (31.6g, 0.156mol) and 0.5mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 1.0h, and the normal pressure transesterification reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction lasted for 0.5h, and the pre-polycondensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction lasted for 0.8h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <4h.
[0083] Example 7
[0084] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,6-hexanodioic acid (31.0g, 0.21mol), 1,4-butanediol (46.9g, 0.521mol) and 0.3mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 2.0h, and the normal pressure transesterification reaction ended. Subsequently, the vacuum system was maintained at 10kPa, the reaction lasted for 0.5h, and the pre-polycondensation reaction ended. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction lasted for 1.5h, the reaction ended, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <5h. The weight of the copolyester decreased by 43% after being buried in the soil for 3 months, showing a certain biodegradability.
[0085] Example 8
[0086] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,6-hexanodioic acid (70.1g, 0.480mol), 1,4-butanediol (86.8g, 0.964mol) and 0.3mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 2.0h, and the normal pressure transesterification reaction was completed. Subsequently, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-polycondensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.5h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <5h. The weight of the copolyester was reduced by 88% after being buried in the soil for 3 months, showing a certain biodegradability.
[0087] Example 9
[0088] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,6-hexanodioic acid (76.0g, 0.521mol), 1,4-butanediol (103.2g, 1.146mol) and 0.3mg MXene were added to the reactor. In a nitrogen atmosphere, the temperature of the material gradually rose to 180-240°C, and the reaction lasted for 2.0h, and the normal pressure transesterification reaction ended. Subsequently, the vacuum system was maintained at 10kPa, the reaction lasted for 0.5h, and the pre-polycondensation reaction ended. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction lasted for 1.5h, the reaction ended, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <5h. The weight of the copolyester decreased by >90% after being buried in the soil for 3 months, showing full biodegradability.
[0089] Example 10
[0090] The reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,4-cyclohexanedimethanol (15.0g, 0.104mol) and 0.3mg Mexen were added to the reactor. Under nitrogen protection, the temperature of the material gradually rose to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, and the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time was <4h.
[0091] Embodiment 11
[0092] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,4-cyclohexanedimethanol (45.7g, 0.313mol) and 0.3mg Mexen were added to the reactor. Under nitrogen protection, the temperature of the material gradually increased to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, and the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time was <4h.
[0093] Example 12
[0094] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,4-cyclohexanedimethanol (60.0g, 0.417mol) and 0.3mg Mexen were added to the reactor. Under nitrogen protection, the temperature of the material gradually increased to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-polycondensation reaction was completed. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time was <4h.
[0095] Embodiment 13
[0096] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), 1,4-cyclohexanedimethanol (75.0g, 0.521mol) and 0.3mg Mexen were added to the reactor. Under nitrogen protection, the temperature of the material gradually rose to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, and the reaction was carried out for 0.5h, and the pre-polycondensation reaction was completed. At 260-295°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time was <4h.
[0097] Embodiment 14
[0098] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit), bisphenol A polyoxyethylene ether (40.4g, 0.128mol) and 0.3mg Mexen were added to the reactor. Under nitrogen protection, the temperature of the material gradually rose to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, and the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 240-260°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 1.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time was <4h.
[0099] Comparative Example 1
[0100] Add the reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit) and spiroethylene glycol (36.4g, 0.120mol) into the reactor. In a nitrogen atmosphere, the temperature of the material gradually rises to 200-260°C, and reacts for 1h, and the normal pressure ester exchange reaction ends. Subsequently, the vacuum system is maintained at 10kPa, the reaction is carried out for 0.5h, and the pre-polycondensation reaction ends. At 260-280°C, the vacuum system is maintained below 50Pa, the reaction is carried out for 8.0h, the reaction ends, the material is discharged under nitrogen protection, and cooled to room temperature. The total reaction time is >10h.
[0101] Comparative Example 2
[0102] Add the reaction raw materials waste PET (100.0g, containing about 0.521mol of PTA structural unit) and 1,10-decanediol (27.2g, 0.156mol) into the reactor. In a nitrogen atmosphere, the temperature of the material gradually rises to 200-240°C, and reacts for 1h, and the normal pressure ester exchange reaction ends. Subsequently, the vacuum system is maintained at 10kPa, and the reaction is carried out for 0.5h, and the pre-polycondensation reaction ends. At 240-260°C, the vacuum system is maintained below 50Pa, and the reaction is carried out for 6h, and the material is discharged under nitrogen protection and cooled to room temperature. The total time is >8h.
[0103] Comparative Example 3
[0104] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit) and 1,4-cyclohexanedimethanol (45.7g, 0.313mol) were added to the reactor. Under nitrogen protection, the temperature of the material gradually rose to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure transesterification reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, and the reaction was carried out for 0.5h, and the pre-polycondensation reaction was completed. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 5.0h, the reaction was completed, the material was discharged under nitrogen protection, and cooled to room temperature. The total time is >6h.
[0105] Comparative Example 4
[0106] The reaction raw materials of waste PET (100.0g, containing about 0.521mol of PTA structural unit) and 1,4-cyclohexanedimethanol (45.7g, 0.313mol) and 30mg of tetrabutyl titanate were added to the reactor. Under nitrogen protection, the temperature of the material gradually rose to 200-240°C, and the reaction was carried out for 0.5h, and the normal pressure ester exchange reaction was completed. Subsequently, the material was maintained at 240-260°C, the vacuum system was maintained at 10kPa, the reaction was carried out for 0.5h, and the pre-condensation reaction was completed. At 240-275°C, the vacuum system was maintained below 50Pa, the reaction was carried out for 2.0h, the reaction was completed, the material was discharged under nitrogen protection, and it was cooled to room temperature. The total time was <4h.
[0107] Examples 1-3 compare the processes and product properties of preparing copolyesters using rigid diols, flexible diols, and by introducing other dibasic acids. Examples 4-6 are about regulating the number of carbon atoms (C6-C12) of the flexible diols to thereby regulate the properties of the copolyesters. Examples 7-9 are about regulating the amount of adipic acid and butanediol introduced to thereby regulate the flexibility and biodegradability of the copolyesters. The diol component of Examples 10-13 is cyclohexanedimethanol (CHDM), and the product properties are regulated by regulating the amount of CHDM introduced. The diol component of Example 14 is an aromatic diol. Comparative Examples 1-4 are cases of not introducing a catalyst and introducing a tetrabutyl titanate catalyst.
[0108] Compared with the experimental results given in Comparative Examples 1-4, the utilization rate of the diol component in Examples 1, 2 and 11 is higher, the transparency of the product is better, the yellow index is lower, and the polycondensation time is shorter. Therefore, the method provided by the present invention not only improves the utilization rate of the diol component and the recycled PET, but also can prepare a high molecular weight, light color PET modified copolyester at a low catalyst content and in a short time. By regulating the flexibility and biodegradability of the copolymer units, the structure of the product can be further regulated and different functionalities can be given to the copolyester. For example, high Tg Copolyester (Example 1, Figure 6 ), human body temperature sensitive copolyester (Example 2, Figure 6 ) and degradable copolyesters (Examples 3 and 8-10). In addition, even though MXene is a black filler, the resulting copolyester still exhibits excellent transparency and a low yellow index when in an amorphous state, which is beneficial for expanding the application range of the material.
[0109] Structural characterization: AvIII type nuclear magnetic resonance spectrometer (400MHz) was used with deuterated chloroform (CDCl3) as solvent and TMS as internal standard to measure the nuclear magnetic proton spectra of the samples prepared in the examples and comparative examples. 1 1H NMR).
[0110] Melting behavior characterization: The melting behavior of the prepared copolyester was characterized by using a differential scanning calorimetry (DSC) instrument (Perkine-Elmer). The weight of the sample was about 5 mg. The copolyester was first heated from room temperature to 260°C at a heating rate of 80°C / min, then cooled to -50°C at a cooling rate of 80°C / min to eliminate the thermal history, and then heated to 260°C at a heating rate of 10°C / min to obtain the heating curve of the sample.
[0111] Determination of intrinsic viscosity: The intrinsic viscosity of the prepared copolyester was measured using an Ubbelohde viscometer (ZVISCO), the polyester concentration was 0.5 g / dL, the solvent was a mixed solution of phenol and tetrachloroethane (mass ratio of 1:1), and the test temperature was (25±0.1)°C.
[0112] Color difference measurement: The samples were pressed into 1.5 mm thick films, and then the hues of the examples and comparative examples were tested using a WSC-S colorimeter.
[0113] Transmittance characterization: UV-visible near-infrared spectrophotometer (LAMBDA 950) was used to measure the light transmittance of the obtained sample film. The sample was a 40 mm square film formed by hot pressing of plastic particles, with a thickness of 0.1 to 1.0 mm and a scanning wavelength range of 200-900 nm.
[0114] The above test results are shown in Table 1.
[0115] Table 1. Structure, molecular weight and properties of samples in Examples 1-14 and Comparative Examples 1-4
[0116]
[0117]
[0118] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0119] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing high molecular weight copolyester using waste PET, characterized in that: include: A mixed reaction system comprising at least a diol, recycled PET, and a catalyst is subjected to an ester exchange or esterification reaction to obtain a copolyester prepolymer; wherein the catalyst comprises a MXene material; And, the prepolymer of the copolyester is subjected to a preliminary polycondensation reaction and a final polycondensation reaction to obtain a high molecular weight copolyester.
2. The method according to claim 1, characterized in that Specifically include: The diol, used or unused dibasic acid or dibasic ester, recycled PET and a catalyst are mixed to form the mixed reaction system, and then reacted at 180-260° C. for 0.5-1.0 h in a protective atmosphere to obtain a copolyester prepolymer.
3. The method according to claim 2, characterized in that: The diol includes any one or more combinations of bisphenol A polyoxyethylene ether, bisphenol S polyoxyethylene ether, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, and spiroethylene glycol; And / or, the dibasic acid includes any one or more combinations of terephthalic acid, furandicarboxylic acid, isophthalic acid, phthalic acid, succinic acid, adipic acid, sebacic acid, and dodecanedioic acid; And / or, the dibasic ester includes any one or more combinations of terephthalate, furandicarboxylate, isophthalate, phthalate, succinate, adipate, sebacate, and dodecanedioate; And / or, the catalyst includes any one or more combinations of Ti3C2Tx, Ti4C3Tx, and Ti2CTx; And / or, the high molecular weight copolyester has a structure as shown in formula (I): wherein x, y, z are integers greater than 0, and z:(x+y)=0-1, x:y=0.1-4; R1 is derived from any one of an aromatic dibasic acid, an aromatic dibasic acid ester, a saturated aliphatic dibasic acid, and a saturated aliphatic dibasic acid ester; R2 is derived from an aromatic diol or a saturated aliphatic diol; And / or, the protective atmosphere comprises a nitrogen atmosphere.
4. The method according to claim 2, characterized in that: The molar ratio of the diol to the dibasic acid or dibasic ester is greater than 2; and / or, the molar ratio of terephthalic acid structural units to dibasic acid or dibasic ester in the recycled PET is 1 to 4:1; and / or, the molar ratio of the diol to the dibasic acid unit in the mixed reaction system is less than or equal to 2.2; And / or, when the mixed reaction system does not use dibasic acid or dibasic ester, the molar ratio of terephthalic acid structural units to diols in the recycled PET is 1 to 5:
1.
5. The method according to claim 1, characterized in that Specifically include: The temperature of the copolyester prepolymer is raised to 200-260° C., and the pressure of the system is reduced to 5-10 KPa to perform a pre-polycondensation reaction; And, after the preliminary polycondensation reaction is completed, the temperature is raised to 220-295° C., and the pressure of the system is reduced to 10-60 Pa to carry out a final polycondensation reaction to obtain a high molecular weight copolyester.
6. The method according to claim 5, characterized in that: The pre-polycondensation reaction time is 0.5 to 1.0 h; And / or, the temperature of the pre-polycondensation reaction is 220-240°C; And / or, the final polycondensation reaction time is 0.5 to 2.0 hours; And / or, the temperature of the final polycondensation reaction is 240-275°C.
7. A high molecular weight copolyester prepared by the method of any one of claims 1 to 6.
8. The high molecular weight copolyester according to claim 7, characterized in that: The intrinsic viscosity of the high molecular weight copolyester is 0.66-0.88 dL / g.
9. Use of MXene materials in catalyzing the recovery of PET to prepare copolyesters, wherein the copolyesters are formed by catalyzing the recovery of PET with diols, used or unused dibasic acids or dibasic esters using MXene materials as catalysts.
10. The use according to claim 9, characterized in that: The MXene material includes any one or more combinations of Ti3C2Tx, Ti4C3Tx, and Ti2CTx.
Citation Information
Patent Citations
Bio-based polyester, bio-based polyester film as well as preparation method and application of bio-based polyester film
CN114539512A
Application of waste PET in preparation of poly (ester-carbonate) copolymer and preparation method of poly (ester-carbonate) copolymer
CN118027375A
Process for preparation of polyester
KR1019920018104A
Recycling method for waste pet and biodegradable copolyester prepared by using same
WO2024077921A1
Cited By
Method for recycling waste PET and corresponding polymer
CN119350601A
Method for synthesizing regenerated polymer from waste polyester, polycarbonate and / or polyether and regenerated polymer
CN119751889A