Diesel engine cylinder cover aluminum alloy and preparation method thereof

By adjusting the chemical composition and process flow of aluminum alloy materials, the thermal stability and mechanical properties of the diesel engine cylinder head are improved, which solves the problem of insufficient material performance in the existing technology and significantly reduces the failure rate and maintenance costs.

CN118755976APending Publication Date: 2024-10-11KUNMING YUNNEI POWER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410746358.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The thermal stability, strength and cost of diesel engine aluminum alloy cylinder head materials are insufficient, resulting in high failure rates and high maintenance costs.

Method used

Aluminum alloy materials with specific chemical compositions are used, including aluminum ingots, recycled materials, modifiers, AlCu50 master alloys and AlNi20 master alloys. The Si and Mg of the materials are adjusted through centralized melting, refining, chemical composition adjustment, pouring, cooling and heat treatment processes. , Ti, Be, Ni, Cu, Fe, Mn, Zn content to improve the mechanical properties of the material.

Benefits of technology

The normal and high temperature tensile strength, yield strength, hardness and post-break elongation of the aluminum alloy cylinder head are improved, the failure rate and maintenance costs are reduced, and the stability and consistency of the material are significantly improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a diesel engine cylinder cover aluminum alloy and a preparation method thereof, and relates to the technical field of diesel engine casting aluminum alloys. The method comprises seven steps of burdening, melting, refining, adjustment of chemical components of molten aluminum, pouring, box opening and heat treatment. The aluminum alloy cylinder cover material for the diesel engine, which is produced by adopting the process disclosed by the invention, is a high-strength, high-thermal-stability, high-percentage elongation after fracture, low-cost and low-stress aluminum alloy cylinder cover material which is obtained by taking ZL114A as a base material and carrying out modification, microalloying and heat treatment, the silicon content is controlled to be 6.5-7.5%, the casting manufacturability is ensured, the contents of alloy elements are low, namely, 0.1-0.2% of Ni and 0.3-0.6% of Cu, and the aluminum alloy cylinder cover material has the advantages of high strength, high thermal stability, high percentage elongation after fracture, low cost and low stress. According to the prepared aluminum alloy cylinder cover material for the diesel engine, the normal-temperature body tensile strength is larger than or equal to 320 MPa, the yield strength is larger than or equal to 280 MPa, the hardness is larger than or equal to HB105, the percentage elongation after fracture is larger than or equal to 3%, the high-temperature (250 DEG C) body tensile strength reaches 217 MPa, light weight and low oil consumption of the diesel engine are assisted, and the dual-carbon target of energy conservation and consumption reduction is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diesel engine casting aluminum alloy, in particular to a diesel engine cylinder head aluminum alloy and a preparation method thereof. Background Art

[0002] The rapid development of the automobile industry has promoted the renewal of engine design concepts and the advancement of manufacturing technology. In order to achieve the "dual carbon" goal of energy saving and consumption reduction, diesel engines are developing towards high power density and lightweight. The use of aluminum alloy materials for diesel engine cylinder heads is an important way to achieve lightweight. Currently, mainstream diesel engine manufacturers have launched their own aluminum alloy cylinder head products, but there are not many manufacturers that have truly put them on the market in large quantities and have been recognized by the market. One of the reasons is that the comprehensive performance issues of diesel engine aluminum alloy cylinder head materials such as thermal stability, high temperature strength, residual stress, and cost have not been completely resolved.

[0003] At present, the material of aluminum alloy cylinder head of diesel engine is mainly AlSi7Mg0.6 in aluminum silicon alloy, and the chemical composition content is as follows: Si: (6.5-7.5)%; Mg: (0.6-0.8)%; Cu: ≤0.2%; Fe: ≤0.2%; the rest of Al, the tensile strength of the body at room temperature is ≥220MPa; the yield strength of the body at room temperature is ≥180MPa, the hardness is ≥95HBW, the elongation after fracture is ≥1.5%, there is no requirement for high temperature mechanical properties, and the standard material of gasoline engine cylinder head is mainly used.

[0004] The prior art has the following defects: 1. The material of diesel engine aluminum alloy cylinder head is basically the same as that of gasoline engine cylinder head. The tensile strength, hardness and elongation after fracture of the body are low, which cannot fully meet the increasingly high explosion pressure and high temperature working conditions of diesel engine.

[0005] 2. The casting process control of the aluminum alloy cylinder head of the diesel engine is unstable and the consistency is poor. Local positions are prone to non-density and microscopic defects. The engine is prone to cracking when running under harsh working conditions, resulting in high maintenance costs for the engine in the later stage.

[0006] 3. Standard aluminum alloy materials are used without micro-alloying treatment, and the mechanical properties of the materials are not fully utilized.

[0007] Therefore, how to overcome the shortcomings of the existing technology is an urgent problem to be solved in the field of diesel engine casting aluminum alloy technology. Summary of the invention

[0008] The purpose of the present invention is to provide an aluminum alloy for a diesel engine cylinder head and a preparation method thereof, so as to solve the problems in the prior art of uneven material, low strength, poor thermal stability and high failure rate of the aluminum alloy cylinder head for diesel engines.

[0009] In order to solve the above problems, the present invention adopts the following technical means: A diesel engine cylinder head aluminum alloy comprises, by weight, 50-60 parts of aluminum ingots, 38.2-48.2 parts of recycled materials, 0.3-0.65 parts of modifiers, 0.4-0.8 parts of AlCu50 master alloys, and 0.3-0.7 parts of AlNi20 master alloys.

[0010] Preferably, the aluminum ingot is a ZL114A aluminum ingot, and the modifier is an ALSr10 modifier.

[0011] Furthermore, the chemical composition of the aluminum alloy is: Si: 6.8~7.2%, Mg: 0.5~0.7%, Ti: 0.1~0.15%, Be: 0~0.07%, Ni: 0.1~0.2%, Cu: 0.3~0.6%, Fe: 0~0.2%, Mn: 0~0.1%, Zn: 0~0.1%, and the rest is aluminum.

[0012] In addition, a method for preparing the aforementioned diesel engine cylinder head aluminum alloy comprises the following steps: S1. Ingredients; S2. Melting: adding the aluminum ingots and the recycled materials into a centralized melting furnace for melting to obtain aluminum liquid; S3. Refining: The aluminum liquid is transferred to a refining furnace and a modifier is added; S4. Chemical composition adjustment: adding AlCu50 master alloy and AlNi20 master alloy to the refined aluminum liquid, adjusting the chemical composition of the aluminum liquid to: Si: 6.8-7.2%, Mg: 0.5-0.7%, Ti: 0.1-0.15%, Be: 0-0.07%, Ni: 0.1-0.2%, Cu: 0.3-0.6%, Fe: 0-0.2%, Mn: 0-0.1%, Zn: 0-0.1%, and the rest is aluminum; S5. Pouring; S6. Cooling; S7. Heat treatment: Solution treatment, quenching and aging treatment are carried out in sequence.

[0013] Preferably, in step S2, the temperature of the filtrate is maintained at 775°C to 790°C before entering refining.

[0014] Furthermore, in step S3, the refining temperature is 740° C. to 770° C., and after adding the modifier, the refining time is not less than 45 minutes.

[0015] Furthermore, in step S4, when adjusting the chemical composition by using the AlCu50 master alloy and the AlNi20 master alloy, the temperature of the molten aluminum is controlled at 735°C to 755°C.

[0016] Furthermore, in step S5, during the pouring process, the bottom mold temperature is 220°C~250°C before pouring, the temperature of the molten aluminum is 735°C~755°C during the pouring process, the pouring time is 8~14 seconds, and the mold holding time is 6 minutes.

[0017] Furthermore, in step S6, cooling is performed at normal temperature after unpacking, and is cooled to less than 100°C.

[0018] Furthermore, in step S7, the solution temperature is 530°C~540°C, the solution holding time is 340~370 minutes, the quenching temperature is 60°C~80°C, the quenching transfer time does not exceed 15 seconds, the quenching time is 180 seconds, the aging treatment temperature is 160°C~170°C, and the aging holding time is 280 minutes.

[0019] During use, the present invention has the following beneficial effects: The diesel engine aluminum alloy cylinder head material of the present invention has a room temperature bulk tensile strength of >320 MPa, a yield strength of ≥280 MPa, a hardness of >HB105, and an elongation after fracture of >3%. The high temperature (250°C) bulk tensile strength reaches 217 MPa, thereby improving the thermal stability of the engine aluminum alloy cylinder head. Through years of application, the failure rate and subsequent maintenance cost of the aluminum alloy cylinder head are effectively reduced.

[0020] At the same time, the tensile strength, yield strength, hardness and elongation of the aluminum alloy cylinder head material are improved, among which the tensile strength of the material is increased by 45%, the yield strength is increased by 27% and the hardness is increased by 10%.

[0021] The high temperature (250°C) tensile strength reaches 217MPa.

[0022] The stability and consistency of the aluminum alloy cylinder head material have been improved, effectively reducing the engine failure rate and subsequent maintenance costs. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0024] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0026] Example 1 S1, ingredients: by weight, ZL114A aluminum ingot: 50 parts, recycled material: 38.2 parts, ALSr10 modifier: 0.3 parts, AlCu50 master alloy: 0.4 parts, AlNi20 master alloy: 0.3 parts; S1, melting: add ZL114A aluminum ingot and recycled materials into the centralized melting furnace according to the proportion of ingredients for melting. After melting, the temperature of the aluminum liquid is controlled between 775℃ and 790℃; S3, refining: the molten aluminum liquid is transferred to the refining furnace, the aluminum liquid temperature is controlled between 740℃-770℃, slag is discharged, 0.3 parts of ALSr10 modifier is added, and slag and gas discharge treatment is carried out for no less than 45 minutes; S4, chemical composition adjustment: use 0.4 parts of AlCu50 master alloy and 0.3 parts of AlNi20 master alloy to adjust the chemical composition. The chemical composition requirements of aluminum liquid are: Si (6.8-7.2)%, Mg (0.5-0.7)%, Ti (0.1-0.15)%, Be (0-0.07)%, Ni: (0.1-0.2)%, Cu (0.3-0.6)%, Fe≤0.2%, Mn≤0.1%, Zn≤0.1%, and the rest is Al. After the treatment is completed, the aluminum liquid is allowed to stand for no less than 12 minutes, and the aluminum liquid temperature is controlled between 735℃-755℃ for pouring.

[0027] S5, pouring: pouring is carried out by robot, bottom mold temperature requirement before pouring: 220℃-250℃, molten aluminum pouring temperature control: 735℃-755℃, pouring time: 8-14 seconds, unpacking time: 6 minutes later (start timing after pouring is completed).

[0028] S6, Cooling: After unpacking and cooling to the casting temperature <100℃, start sand removal, cutting pouring and rising head and cleaning to prepare for heat treatment.

[0029] S7, heat treatment: solution treatment, quenching and aging treatment are carried out in sequence; solution temperature: 530℃-540℃, solution holding time 340-370 minutes, quenching temperature: 60℃-80℃, quenching transfer time: ≤15 seconds, quenching time: 180 seconds, aging temperature: 160℃-170℃, aging holding time: 280 minutes.

[0030] Example 2 S1, ingredients: by weight, ZL114A aluminum ingot: 60 parts, recycled material: 48.2 parts, ALSr10 modifier: 0.65 parts, AlCu50 master alloy: 0.8 parts, AlNi20 master alloy: 0.7 parts; S1, melting: add ZL114A aluminum ingot and recycled materials into the centralized melting furnace according to the proportion of ingredients for melting. After melting, the temperature of the aluminum liquid is controlled between 775℃ and 790℃; S3, refining: the molten aluminum liquid is transferred to the refining furnace, the aluminum liquid temperature is controlled between 740℃-770℃, slag is discharged, 0.65 parts of ALSr10 modifier is added, and slag and gas discharge treatment is carried out for no less than 45 minutes; S4, chemical composition adjustment: use 0.8 parts of AlCu50 master alloy and 0.7 parts of AlNi20 master alloy to adjust the chemical composition. The chemical composition requirements of aluminum liquid are: Si (6.8-7.2)%, Mg (0.5-0.7)%, Ti (0.1-0.15)%, Be (0-0.07)%, Ni: (0.1-0.2)%, Cu (0.3-0.6)%, Fe≤0.2%, Mn≤0.1%, Zn≤0.1%, and the rest is Al. After the treatment is completed, the aluminum liquid is allowed to stand for no less than 12 minutes, and the aluminum liquid temperature is controlled between 735℃-755℃ for pouring.

[0031] S5, pouring: pouring is carried out by robot, bottom mold temperature requirement before pouring: 220℃-250℃, molten aluminum pouring temperature control: 735℃-755℃, pouring time: 8-14 seconds, unpacking time: 6 minutes later (start timing after pouring is completed).

[0032] S6, Cooling: After unpacking and cooling to the casting temperature <100℃, start sand removal, cutting pouring and riser and cleaning to prepare for heat treatment.

[0033] S7, heat treatment: solution treatment, quenching and aging treatment are carried out in sequence; solution temperature: 530℃-540℃, solution holding time 340-370 minutes, quenching temperature: 60℃-80℃, quenching transfer time: ≤15 seconds, quenching time: 180 seconds, aging temperature: 160℃-170℃, aging holding time: 280 minutes.

[0034] Example 3 S1, ingredients: by weight, ZL114A aluminum ingot: 55 parts, recycled material: 43.2 parts, ALSr10 modifier: 0.45 parts, AlCu50 master alloy: 0.6 parts, AlNi20 master alloy: 0.5 parts; S1, melting: add ZL114A aluminum ingot and recycled materials into the centralized melting furnace according to the proportion of ingredients for melting. After melting, the temperature of the aluminum liquid is controlled between 775℃ and 790℃; S3, refining: the molten aluminum liquid is transferred to the refining furnace, the aluminum liquid temperature is controlled between 740℃-770℃, slag is discharged, 0.45 parts of ALSr10 modifier is added, and slag and gas discharge treatment is carried out for no less than 45 minutes; S4, chemical composition adjustment: use 0.6 parts of AlCu50 master alloy and 0.5 parts of AlNi20 master alloy to adjust the chemical composition. The chemical composition requirements of aluminum liquid are: Si (6.8-7.2)%, Mg (0.5-0.7)%, Ti (0.1-0.15)%, Be (0-0.07)%, Ni: (0.1-0.2)%, Cu (0.3-0.6)%, Fe≤0.2%, Mn≤0.1%, Zn≤0.1%, and the rest is Al. After the treatment is completed, the aluminum liquid is allowed to stand for no less than 12 minutes, and the aluminum liquid temperature is controlled between 735℃-755℃ for pouring.

[0035] S5, pouring: pouring is carried out by robot, bottom mold temperature requirement before pouring: 220℃-250℃, molten aluminum pouring temperature control: 735℃-755℃, pouring time: 8-14 seconds, unpacking time: 6 minutes later (start timing after pouring is completed).

[0036] S6, Cooling: After unpacking and cooling to the casting temperature <100℃, start sand removal, cutting pouring and riser and cleaning to prepare for heat treatment.

[0037] S7, heat treatment: solution treatment, quenching and aging treatment are carried out in sequence; solution temperature: 530℃-540℃, solution holding time 340-370 minutes, quenching temperature: 60℃-80℃, quenching transfer time: ≤15 seconds, quenching time: 180 seconds, aging temperature: 160℃-170℃, aging holding time: 280 minutes.

[0038] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A diesel engine cylinder head aluminum alloy, characterized in that: By weight, including: 50-60 parts of aluminum ingots, 38.2~48.2 parts of recycled materials, 0.3~0.65 parts of modifiers, 0.4~0.8 parts of AlCu50 master alloys, and 0.3~0.7 parts of AlNi20 master alloys.

2. The diesel engine cylinder head aluminum alloy according to claim 1, characterized in that: The aluminum ingot is a ZL114A aluminum ingot, and the modifier is an ALSr10 modifier.

3. A diesel engine cylinder head aluminum alloy according to claim 1 or 3, characterized in that: The chemical composition of the aluminum alloy is: Si: 6.8-7.2%, Mg: 0.5-0.7%, Ti: 0.1-0.15%, Be: 0-0.07%, Ni: 0.1-0.2%, Cu: 0.3-0.6%, Fe: 0-0.2%, Mn: 0-0.1%, Zn: 0-0.1%, and the rest is aluminum.

4. A method for preparing an aluminum alloy for a diesel engine cylinder head according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Ingredients; S2. Melting: adding the aluminum ingots and the recycled materials into a centralized melting furnace for melting to obtain aluminum liquid; S3. Refining: The aluminum liquid is transferred to a refining furnace and a modifier is added; S4. Chemical composition adjustment: adding AlCu50 master alloy and AlNi20 master alloy to the refined aluminum liquid, adjusting the chemical composition of the aluminum liquid to: Si: 6.8-7.2%, Mg: 0.5-0.7%, Ti: 0.1-0.15%, Be: 0-0.07%, Ni: 0.1-0.2%, Cu: 0.3-0.6%, Fe: 0-0.2%, Mn: 0-0.1%, Zn: 0-0.1%, and the rest is aluminum; S5. Pouring; S6. Cooling; S7. Heat treatment: Solution treatment, quenching and aging treatment are carried out in sequence.

5. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In step S2, the temperature of the filtrate is maintained at 775°C to 790°C before entering the refining process.

6. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In step S3, the refining temperature is 740° C. to 770° C., and after the modifier is added, the refining time is not less than 45 minutes.

7. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In the step S4, when the chemical composition is adjusted by using the AlCu50 master alloy and the AlNi20 master alloy, the temperature of the molten aluminum is controlled at 735° C. to 755° C.

8. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In step S5, during the pouring process, the bottom mold temperature is 220°C to 250°C before pouring, the temperature of the molten aluminum is 735°C to 755°C during the pouring process, the pouring time is 8 to 14 seconds, and the mold retention time is 6 minutes.

9. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In the step S6, cooling is performed at room temperature after unpacking, and the temperature is cooled to less than 100°C.

10. The method for preparing aluminum alloy for a diesel engine cylinder head according to claim 4, characterized in that: In step S7, the solution temperature is 530°C to 540°C, the solution holding time is 340 to 370 minutes, the quenching temperature is 60°C to 80°C, the quenching transfer time is no more than 15 seconds, the quenching time is 180 seconds, the aging treatment temperature is 160°C to 170°C, and the aging holding time is 280 minutes.