Tin-phosphor bronze strip and preparation method thereof

By adjusting the composition and process of the tin-phosphorus bronze strip, reducing the tin content and optimizing the grain size and grain boundary length fraction, the problem of tin resource consumption is solved, and the high-temperature stability and performance maintenance of the tin-phosphorus bronze strip are achieved.

CN118755992APending Publication Date: 2024-10-11JIANGXI YUNTAI COPPER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410800782.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The high tin content in existing tin-phosphorus bronze materials has led to an increase in the consumption of tin resources, and the gradual reduction of tin resources. It is necessary to develop materials with low tin content to protect scarce resources.

Method used

By adjusting the mass percentage composition of the tin-phosphor bronze strip and optimizing the process, the tin content is reduced to 0.8-2.5%, and by adjusting the grain size and grain boundary length fraction, the high-temperature softening temperature is increased and the material properties are maintained. Specific steps include weighing, melting, homogenization annealing, rough rolling, intermediate rolling, finishing rolling, cold rolling and stretch bending and straightening.

Benefits of technology

It effectively reduces the tin content and protects scarce resources, while maintaining the high strength, hardness and elongation of the tin-phosphorus bronze alloy, ensuring the performance of the material and achieving the high-temperature stability of the tin-phosphorus bronze strip.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of copper alloys, and provides a tin-phosphor bronze strip which comprises the following components in percentage by mass: 0.8-2.5 wt% of tin, 0-0.6 wt% of nickel, 0-0.9 wt% of zinc, 0.05-0.5 wt% of iron, 0.05-0.5 wt% of phosphor, 95-99 wt% of copper and 0-0.1 wt% of impurities, and the grain size of the tin-phosphor bronze strip is controlled to be 1-3.5 microns. The length fraction of a large-angle grain boundary in the tin-phosphor bronze alloy strip is 30-85%, the length fraction of a small-angle grain boundary in the tin-phosphor bronze alloy strip is 15-70%, and the high-temperature softening resistance temperature of the tin-phosphor bronze alloy strip is larger than or equal to 370 DEG C. According to the tin-phosphor bronze strip provided by the invention, the tin-phosphor bronze alloy is subjected to component proportioning again, on the basis of keeping the performance of the tin-phosphor bronze alloy, the tin content is reduced to 0.5-2.5%, so that scarce resources are effectively protected, and on the basis of keeping the performance of the tin-phosphor bronze alloy, the tin content is reduced to 0.5-2.5%, so that the scarce resources are effectively protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloys, in particular to a tin-phosphor bronze strip and a preparation method thereof. Background Art

[0002] After solid solution treatment, combined deformation treatment and low-temperature heat treatment, tin-phosphorus bronze has higher hardness and strength. It is a widely used elastic copper alloy material.

[0003] Tin is the most scarce variety among the ten major non-ferrous metals and one of the few non-ferrous metal resources with pricing power. With the continuous improvement of tin resource exploitation, the tin reserves have been significantly reduced, the shortage of tin ore resources has also become prominent, and the market price is high. At present, the tin content of existing tin bronze generally does not exceed 8% at most, and is not less than 4% at least, which greatly increases the resource consumption of tin. Therefore, it is necessary to develop a tin-phosphor bronze strip with low tin content. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a tin-phosphor bronze strip and a preparation method thereof, which solves the problem of the amount of tin metal used and improves the process by adjusting the trace element composition of the material and optimizing.

[0005] To achieve the above object, the present invention is implemented by the following technical scheme: a tin-phosphor bronze strip, the mass percentage of which is: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is controlled at 1-3.5μm;

[0006] The length fraction of the high-angle grain boundaries in the tin-phosphor bronze alloy strip is 30-85%, the length fraction of the low-angle grain boundaries is 15-70%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

[0007] Preferably, the weight percentage of the tin-phosphor bronze strip is: 1.9wt% tin, 0.4wt% nickel, 0.6wt% zinc, 0.35wt% iron, 0.3wt% phosphorus, 97wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is 2.4μm.

[0008] Preferably, the length fraction of the high-angle grain boundaries in the tin-phosphorus bronze alloy strip is 32%, the length fraction of the low-angle grain boundaries is 68%, and the high-temperature softening temperature of the tin-phosphorus bronze strip is ≥370°C.

[0009] Preferably, the tensile strength of the tin-phosphorus bronze alloy strip is 600-1000 MPa, preferably the yield strength of the tin-phosphorus bronze alloy strip is 550-950 MPa, preferably the elongation of the tin-phosphorus bronze alloy strip is 15-38%, and preferably the hardness of the tin-phosphorus bronze alloy strip is 207-279 HV.

[0010] A method for preparing a tin-phosphor bronze strip comprises the following steps:

[0011] Step 1, weighing materials according to the following composition ratio: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities;

[0012] Step 2: Add electrolytic copper, nickel plate and iron-copper alloy into a cored induction power frequency melting furnace for primary melting, then add zinc ingot, tin block and phosphor copper alloy for secondary melting and mixing, and gradually perform homogenization annealing;

[0013] Step 3: After homogenization annealing, the raw material is milled and rough rolled. After rough rolling, intermediate annealing is performed again. After intermediate annealing, degreasing and pickling are performed. After drying, intermediate rolling is performed.

[0014] Step 4: After the intermediate rolling is completed, the raw material is subjected to the first air cushion furnace annealing, followed by the finishing rolling, and then the second air cushion furnace annealing after the finishing rolling is completed. After the annealing is completed, the finished product is cold rolled, and after the cold rolling is completed, the product is annealed at a low temperature, and then degreased, pickled, and dried;

[0015] Step 5: After rolling, the finished product is straightened and cut into strips.

[0016] Preferably, in step 2, the primary melting temperature and the secondary melting temperature of the metal are both 1250-1300°C.

[0017] Preferably, the temperature of the homogenization annealing in step 2 is 700-760° C., and the holding time is 4-6 hours.

[0018] Preferably, in step three, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower surfaces.

[0019] Preferably, the finishing rate of the finishing rolling in the step 4 is controlled at 60-70%, the annealing temperature of the first air cushion furnace annealing and the second air cushion furnace annealing is 700-800° C., and the heating time in the air cushion furnace is 5-15 seconds.

[0020] Preferably, the processing rate of the finished product in step 4 is controlled at 20-35%.

[0021] The present invention provides a tin-phosphor bronze strip and a preparation method thereof, which has the following beneficial effects:

[0022] The invention provides a tin-phosphor bronze strip, which re-proportions the components of the tin-phosphor bronze alloy, reduces the tin content to 0.5-2.5% while maintaining the performance of the tin-phosphor bronze alloy, and effectively protects scarce resources. The invention also re-proportions the tin content to 0.5-2.5% while maintaining the performance of the tin-phosphor bronze alloy, and effectively protects scarce resources. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The embodiment of the present invention provides a tin-phosphor bronze strip and a preparation method thereof.

[0025] As one aspect of the present invention, the present invention provides a tin-phosphor bronze strip, wherein the weight percentage of the tin-phosphor bronze strip is as follows: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is controlled at 1-3.5μm;

[0026] The length fraction of the high-angle grain boundary in the tin-phosphor bronze alloy strip is 30-85%, the length fraction of the low-angle grain boundary is 15-70%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

[0027] The tensile strength of the tin-phosphor bronze alloy strip is 600-1000 MPa, the yield strength of the tin-phosphor bronze alloy strip is preferably 550-950 MPa, the elongation of the tin-phosphor bronze alloy strip is preferably 15-38%, and the hardness of the tin-phosphor bronze alloy strip is preferably 207-279 HV.

[0028] As another aspect of the present invention, the method for preparing the tin-phosphor bronze strip is as follows, comprising the following steps:

[0029] Step 1, weighing materials according to the following composition ratio: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities;

[0030] Step 2: Add electrolytic copper, nickel plate and iron-copper alloy to a core induction power frequency melting furnace for primary melting, then add zinc ingot, tin block and phosphor copper alloy for secondary melting and mixing, and gradually perform homogenization annealing. The primary melting temperature and the secondary melting temperature of the metal are both 1250-1300°C, the homogenization annealing temperature is 700-760°C, and the holding time is 4-6h;

[0031] Step 3: After homogenization annealing, the raw material is milled and rough rolled. The milling surface of the raw material is 0.35-0.6 mm on the upper and lower milling surfaces. After the rough rolling, intermediate annealing is performed again. After the intermediate annealing is completed, degreasing and pickling are performed, and intermediate rolling is performed after drying.

[0032] Step 4: After the intermediate rolling is completed, the raw material is subjected to the first air cushion furnace annealing, followed by finish rolling. After the finish rolling is completed, the second air cushion furnace annealing is performed, and the processing rate of the finish rolling is controlled at 60-70%. The annealing temperature of the first air cushion furnace annealing and the second air cushion furnace annealing is 700-800°C, and the time in the heating zone of the air cushion furnace is 5-15s. After the annealing is completed, the finished product is cold rolled, and the processing rate of the finished product is controlled at 20-35%. After the cold rolling is completed, low-temperature annealing is performed, and degreasing, pickling and drying are performed;

[0033] Step 5: After rolling, the finished product is straightened and cut into strips.

[0034] Embodiment 1:

[0035] A tin-phosphor bronze strip, wherein the weight percentage of the tin-phosphor bronze strip is as follows: 1.75wt% tin, 0.36wt% nickel, 0.7wt% zinc, 0.15wt% iron, 0.26wt% phosphorus, 96wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is controlled at 2.8μm;

[0036] The length fraction of the high-angle grain boundary in the tin-phosphor bronze alloy strip is 38%, the length fraction of the low-angle grain boundary is 62%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

[0037] Embodiment 2:

[0038] A tin-phosphor bronze strip comprises the following weight percentages: 1.9wt% tin, 0.4wt% nickel, 0.6wt% zinc, 0.35wt% iron, 0.3wt% phosphor, 97wt% copper and 0-0.1wt% impurities; the grain size of the tin-phosphor bronze strip is 2.4μm.

[0039] The length fraction of the high-angle grain boundary in the tin-phosphor bronze alloy strip is 32%, the length fraction of the low-angle grain boundary is 68%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

[0040] Embodiment 3:

[0041] A tin-phosphor bronze strip, wherein the weight percentage of the tin-phosphor bronze strip is as follows: 1.6wt% tin, 0.15wt% nickel, 0.28wt% zinc, 0.33wt% iron, 0.22wt% phosphorus, 98wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is controlled at 2.5μm;

[0042] The length fraction of the high-angle grain boundary in the tin-phosphor bronze alloy strip is 42%, the length fraction of the low-angle grain boundary is 58%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

[0043] Experimental example;

[0044] Four groups of tin-phosphor bronze strips made of the same raw materials were selected, and experiments were conducted with the mass percentage of copper, tin, nickel, zinc, iron and phosphorus in the tin-phosphor bronze strips. One tin-phosphor bronze strip of the above embodiment was used as an experimental example, and compared with the existing tin-phosphor bronze mass percentage group. The results are shown in Table 1 below:

[0045] Material copper tin nickel Zinc iron phosphorus other Example 1 margin 1.75wt% 0.36wt% 0.15wt% 0.15wt% 0.26wt% <0.01 Example 2 margin 1.9wt% 0.4wt% 0.6wt% 0.35wt% 0.3wt% <0.01 Example 3 margin 1.6wt% 0.15wt% 0.28wt% 0.33wt% 0.22wt% <0.01 Comparative Example margin 6.14wt% 0.08wt% 0.15wt% 0.01wt% 0.13wt% <0.01

[0046] The results show that the present invention optimizes the component ratio of the tin-phosphor bronze alloy, reduces the tin content to 0.5-2.5% while maintaining the performance of the tin-phosphor bronze alloy, and effectively protects scarce resources.

[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A tin-phosphor bronze strip, characterized in that: The weight percentage of the tin-phosphor bronze strip is as follows: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities, and the grain size of the tin-phosphor bronze strip is controlled at 1-3.5μm; The length fraction of the high-angle grain boundaries in the tin-phosphor bronze alloy strip is 30-85%, the length fraction of the low-angle grain boundaries is 15-70%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

2. The tin-phosphor bronze strip according to claim 1, characterized in that: The weight percentage of the tin-phosphor bronze strip is as follows: 1.9wt% tin, 0.4wt% nickel, 0.6wt% zinc, 0.35wt% iron, 0.3wt% phosphorus, 97wt% copper and 0-0.1wt% impurities. The grain size of the tin-phosphor bronze strip is 2.4μm.

3. The tin-phosphor bronze strip according to claim 1, characterized in that: The length fraction of the high-angle grain boundaries in the tin-phosphor bronze alloy strip is 32%, the length fraction of the low-angle grain boundaries is 68%, and the high-temperature softening temperature of the tin-phosphor bronze strip is ≥370°C.

4. A tin-phosphor bronze strip according to any one of claims 1 to 3, characterized in that: The tensile strength of the tin-phosphorus bronze alloy strip is 600-1000 MPa, preferably the yield strength of the tin-phosphorus bronze alloy strip is 550-950 MPa, preferably the elongation of the tin-phosphorus bronze alloy strip is 15-38%, and preferably the hardness of the tin-phosphorus bronze alloy strip is 207-279 HV.

5. A method for preparing a tin-phosphor bronze strip, using the tin-phosphor bronze strip as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, weighing materials according to the following composition ratio: 0.8-2.5wt% tin, 0-0.6wt% nickel, 0-0.9wt% zinc, 0.05-0.5wt% iron, 0.05-0.5wt% phosphorus, 95-99wt% copper and 0-0.1wt% impurities; Step 2: Add electrolytic copper, nickel plate and iron-copper alloy into a cored induction power frequency melting furnace for primary melting, then add zinc ingot, tin block and phosphor copper alloy for secondary melting and mixing, and gradually perform homogenization annealing; Step 3: After homogenization annealing, the raw material is milled and rough rolled. After rough rolling, intermediate annealing is performed again. After intermediate annealing, degreasing and pickling are performed. After drying, intermediate rolling is performed. Step 4: After the intermediate rolling is completed, the raw material is subjected to the first air cushion furnace annealing, followed by the finishing rolling, and then the second air cushion furnace annealing after the finishing rolling is completed. After the annealing is completed, the finished product is cold rolled, and after the cold rolling is completed, the product is annealed at a low temperature, and then degreased, pickled, and dried; Step 5: After rolling, the finished product is straightened and cut into strips.

6. The method for preparing a tin-phosphor bronze strip according to claim 5, characterized in that: In the step 2, the primary melting temperature and the secondary melting temperature of the metal are both 1250-1300°C.

7. The method for preparing a tin-phosphor bronze strip according to claim 5, characterized in that: The temperature of the homogenization annealing in the step 2 is 700-760° C., and the holding time is 4-6 hours.

8. The method for preparing a tin-phosphor bronze strip according to claim 5, characterized in that: In the step 3, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower surfaces.

9. The method for preparing a tin-phosphor bronze strip according to claim 5, characterized in that: The processing rate of the finishing rolling in the step 4 is controlled at 60-70%, the annealing temperature of the first air cushion furnace annealing and the second air cushion furnace annealing is 700-800° C., and the heating time in the air cushion furnace is 5-15 seconds.

10. The method for preparing a tin-phosphor bronze strip according to claim 5, characterized in that: The processing rate of the finished product rolling in the step 4 is controlled at 20-35%.